Method for producing particles and method for producing molded body
By heat treatment and crushing the fluororesin particles within a specific temperature range, the problems of incomplete removal of low boiling point components and fibrillation in the prior art are solved, and the quality and processing convenience of the molded body are improved.
Patent Information
- Application Number
- CN202410989872.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-17
- Filing Date
- 2019-12-25
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is prone to fibrillated crushing when pulverizing and treating fluororesin particles, and cannot effectively remove low boiling point components, resulting in poor quality of white smoke and molded bodies during coating forming.
The fluororesin particles containing melt-formable fluororesin particles are heat treated within a temperature range above the intermediate point glass transition temperature and below the extrapolated melting start temperature, and then pulverized to remove the low boiling point components and inhibit fibrillation.
Excellent removal of low boiling point components is achieved, densification and fibrillation of fluororesin particles are suppressed, and the convenience of pulverization and quality of molded bodies are improved.
Smart Images

Figure BDA0004958561450000181 
Figure BDA0004958561450000191 
Figure BDA0004958561450000201
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing particles containing a fluororesin and a method for producing a molded body. Background Art
[0002] Fluororesins with excellent heat resistance, chemical resistance, and weather resistance are used in various fields such as the semiconductor industry, the automobile industry, and the chemical industry. For example, by applying a powder composed of particles containing fluororesins to the surface of a substrate by electrostatic coating, fluidization dipping, or rotational molding, a coating film with excellent protection of the substrate surface and chemical resistance can be formed.
[0003] In recent years, there is a demand for fluororesins with a low content of low-boiling-point components. If the particles containing fluororesins contain a large amount of low-boiling-point components, when the particles are used to manufacture a formed body such as a coating, white smoke may sometimes be generated due to the evaporation of the low-boiling-point components. Therefore, Patent Document 1 discloses a method for controlling the melt volume flow rate of the fluororesin when melt-kneading a fluororesin such as ETFE by a twin-screw extruder to remove the low-boiling-point components contained in the fluororesin.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2017 / 209133 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] However, when the inventors pulverized the fluororesin particles obtained by the method described in Patent Document 1, fibrillated pulverized products were sometimes produced, and particles that can be used as powders could not be obtained. Therefore, there is a need for a method for producing particles containing fluororesin that is excellent in removing low-boiling point components and can suppress fibrillation even when pulverized.
[0009] The present invention has been made based on the above-mentioned problems, and an object of the present invention is to provide a method for producing particles and a method for producing a molded body which are excellent in the ability to remove low-boiling point components and can suppress fibrillation even when subjected to a pulverization treatment.
[0010] Technical solutions adopted to solve technical problems
[0011] The present inventors have conducted intensive studies on the above-mentioned problems and have found that if particles A containing a fluororesin capable of melt-forming are heat-treated at a temperature above the midpoint glass transition temperature and below the extrapolated melting start temperature, the removal of low-boiling point components is excellent, and fibrillation can be suppressed even when a pulverization treatment is performed, thereby completing the present invention.
[0012] That is, the inventors have found that the above-mentioned problems can be solved by the following configuration.
[0013] [1] A method for producing particles, characterized in that particles A containing a melt-formable fluororesin are heat-treated at a temperature not less than the midpoint glass transition temperature and not more than the extrapolated melting start temperature to obtain particles B containing the fluororesin.
[0014] [2] The method for producing particles according to [1], wherein the temperature of the heat treatment is 10°C or more higher than the midpoint glass transition temperature and 10°C or more lower than the extrapolated melting start temperature.
[0015] [3] The method for producing particles according to [1] or [2], wherein the heat treatment time is 30 minutes to 10 hours.
[0016] [4] The method for producing particles according to any one of [1] to [3], wherein the fluororesin is obtained by polymerizing a fluorine-containing monomer and a non-fluorine-containing monomer in the presence of a hydrofluorocarbon or a hydrofluoroether.
[0017] [5] The method for producing particles according to [4], wherein the fluorine-containing monomer is at least one selected from tetrafluoroethylene, hexafluoropropylene, perfluoro(alkyl vinyl ether), chlorotrifluoroethylene, vinylidene fluoride, and vinyl fluoride,
[0018] The non-fluorine monomer is at least one selected from ethylene, propylene, itaconic anhydride, and vinyl acetate.
[0019] [6] The method for producing particles as described in any one of [1] to [5], wherein the fluororesin is any one of a copolymer containing units based on tetrafluoroethylene and units based on ethylene, a copolymer containing units based on chlorotrifluoroethylene and units based on ethylene, a copolymer containing units based on tetrafluoroethylene and units based on perfluoro(alkyl vinyl ether), and a copolymer containing units based on tetrafluoroethylene and units based on hexafluoropropylene.
[0020] [7] The method for producing particles according to any one of [1] to [6], wherein the fluororesin is a copolymer containing units based on tetrafluoroethylene and units based on ethylene, and the copolymer further contains a monomer F1 represented by the following formula (F1):
[0021] CH2=CX(CF2) n Y(F1)
[0022] (X and Y are each independently a hydrogen atom or a fluorine atom, and n is an integer of 2 to 8).
[0023] [8] The method for producing particles according to any one of [1] to [7], wherein the average particle size of the particles A is 100 μm to 10.0 mm.
[0024] [9] The method for producing particles according to any one of [1] to [8], wherein the particles A contain a low boiling point component, and the content of the low boiling point component is greater than 0 mass % and less than 0.5 mass % relative to the total mass of the particles A.
[0025]
[10] The method for producing particles according to [9], wherein the reduction ratio of the low boiling point components before and after the heat treatment calculated by the following formula using the content of the low boiling point components contained in the particles A and B is 20 to 100%:
[0026] The reduction ratio of low boiling point components before and after heat treatment [%] = 100 × (the content of low boiling point components contained in particle A - the content of low boiling point components contained in particle B) / (the content of low boiling point components contained in particle A).
[0027]
[11] The method for producing particles according to any one of [1] to
[10] , wherein the particles B are pulverized to obtain particles C.
[0028]
[12] The method for producing particles according to
[11] , wherein the average particle size of particles C obtained by pulverizing the particles B is 10 to 1000 μm.
[0029]
[13] The method for producing particles according to
[11] or
[12] , wherein the apparent density of the particles C obtained by pulverizing the particles B is 0.3 to 1.2 g / cm 3 .
[0030]
[14] A method for producing a molded article, characterized in that particles produced by the production method described in any one of [1] to
[13] are melted at a temperature above the melting point of the fluororesin to obtain a molded article containing the fluororesin.
[0031] Effects of the Invention
[0032] According to the present invention, there can be provided a method for producing particles and a method for producing a molded body, which are excellent in the ability to remove low-boiling point components and can suppress fibrillation even when a pulverization treatment is performed.
[0033] The mechanism by which the above-mentioned effects of the present invention are obtained is not clearly understood, but it is considered that one of the causes is that the densification and fibrillation of the fluororesin particles are suppressed by the removal of the low boiling point components. DETAILED DESCRIPTION
[0034] The meanings of the terms in the present invention are as follows.
[0035] The numerical range expressed with “to” means a range including the numerical values described before and after “to” as the lower limit and the upper limit.
[0036] "Capable of melt forming" means exhibiting melt fluidity. "Exhibiting melt fluidity" means that under a load of 49 N, at a temperature 20°C or higher than the melting point of the resin, there is a temperature at which the melt flow rate reaches 0.1 to 1000 g / 10 minutes. In addition, "melt flow rate" refers to the melt flow rate (MFR) specified in JIS K 7210: 1999 (ISO 1133: 1997).
[0037] The midpoint glass transition temperature and the extrapolated melting start temperature are values (°C) calculated according to the method of JIS K7121 (1987) and are obtained based on the DSC curve obtained by the differential scanning calorimetry (DSC) method. In addition, the midpoint glass transition temperature is also recorded as "T mg The extrapolated melting onset temperature is also recorded as “T im ”.
[0038] "Unit" is a general term for an atomic group derived from one molecule of the monomer directly formed by polymerization of the monomer and an atomic group obtained by chemically changing a part of the atomic group. In addition, hereinafter, a unit derived from each monomer may be referred to as the name of the monomer plus "unit".
[0039] The “average particle size of particles” is a volume-based median particle size measured using a laser diffraction scattering particle size distribution analyzer.
[0040] The method for producing the particles of the present invention is to obtain a particle having a glass transition temperature (T mg ) and the extrapolated melting start temperature (T im ) or less by heat-treating particles A containing a melt-molded fluororesin (hereinafter also referred to as "specific heat treatment") to obtain particles B containing the fluororesin.
[0041] The method for producing particles of the present invention has excellent removal of low boiling point components. The detailed reason is not clear, but it is speculated that if T mg When the particle A is heat treated at a temperature above T, the molecular chain movement of the fluororesin becomes easy to occur, so the low-boiling point components can be fully removed from the particle A. im By heat-treating the particles A at a temperature below 100 °C, the fusion between the particles due to the local melting of the fluororesin can be suppressed, and thus the low-boiling point components can be sufficiently removed from the particles.
[0042] In addition, if T imWhen the particles A are heat-treated at a temperature below 0.5°C, the obtained particles B can be pulverized easily and the generation of fibrillated pulverized products can be suppressed.
[0043] [Particle A]
[0044] The particles A contain a melt-moldable fluororesin (hereinafter also referred to as a "specific fluororesin"). The specific fluororesin is preferably solid at room temperature (25°C).
[0045] The specific fluororesin is not particularly limited as long as it can be melt-molded, and a known fluororesin may be used. However, from the viewpoint of excellent moldability, it is preferred that the specific fluororesin has units based on a fluorine-containing monomer and units based on a non-fluorine-containing monomer.
[0046] Specific examples of fluorinated monomers include tetrafluoroethylene (hereinafter also referred to as "TFE"), hexafluoropropylene (hereinafter also referred to as "HFP"), perfluoro(alkyl vinyl ether), chlorotrifluoroethylene (hereinafter also referred to as "CTFE"), vinylidene fluoride (hereinafter also referred to as "VdF"), and vinyl fluoride. The fluorinated monomers may be used alone or in combination of two or more.
[0047] Specific examples of the non-fluorine-containing monomer include ethylene, propylene, itaconic anhydride, and vinyl acetate. The non-fluorine-containing monomer may be used alone or in combination of two or more.
[0048] Specific examples of the specific fluororesin include copolymers (ETFE) containing units based on TFE (hereinafter also referred to as "TFE units") and units based on ethylene (hereinafter also referred to as "E units"), copolymers (ECTFE) containing units based on CTFE and units based on ethylene, copolymers (PFA) containing TFE units and units based on perfluoro(alkyl vinyl ether) (hereinafter also referred to as "perfluoroalkyl vinyl ether units"), and copolymers (FEP) containing TFE units and units based on hexafluoropropylene (hereinafter also referred to as "hexafluoropropylene units"). From the viewpoint of excellent moldability, ETFE and ECTFE are preferred, and ETFE is particularly preferred.
[0049] In ETFE, the content of the E unit is preferably 20 to 70 mol %, more preferably 25 to 60 mol %, particularly preferably 35 to 55 mol % based on the total content of the E unit and the TFE unit.
[0050] When the ratio of the content of the E unit is at least the lower limit of the above range, the mechanical strength is excellent, and when it is at most the upper limit, the chemical resistance is excellent.
[0051] ETFE may be a copolymer consisting of only E units and TFE units, or may contain one or more other monomer units.
[0052] Preferred examples of other monomers include monomer F1 represented by the following formula (F1).
[0053] CH2=CX(CF2) n Y(F1)
[0054] In formula (F1), X and Y are each independently a hydrogen atom or a fluorine atom, and n is an integer of 2 to 8 (preferably 3 to 7, more preferably 4 to 6).
[0055] As a specific example of monomer F1, CH2=CF(CF2) can be mentioned. n F, CH2=CF(CF2) n H, CH2=CH(CF2) n F, CH2=CH(CF2) n H, preferably CH2=CH(CF2) n F, more preferably CH2=CH(CF2)2F, CH2=CH(CF2)4F ((perfluorobutyl)ethylene, hereinafter referred to as PFBE).
[0056] When ETFE contains other monomer units, the total content thereof is preferably 0.1 to 10 moles, more preferably 0.1 to 5 moles, and particularly preferably 0.2 to 4 moles, based on the total of 100 moles of E units and TFE units. If the content of other monomer units is above the lower limit of the above range, crack resistance is good, and if it is below the upper limit, the melting point of the fluororesin decreases and the moldability becomes good.
[0057] In PFA, the content of TFE units is preferably 9 to 99 mol, more preferably 80 to 99 mol, and particularly preferably 90 to 99 mol, relative to the total content of TFE units and perfluoroalkyl vinyl ether units. PFA can be a copolymer consisting only of TFE units and perfluoroalkyl vinyl ether units, or it can contain one or more other monomer units in addition thereto. As a preferred example of other monomers, hexafluoropropylene can be cited. When other monomer units are included, the content is preferably 0.1 to 10 mol, more preferably 0.1 to 6 mol, and particularly preferably 0.2 to 4 mol, expressed as a molar ratio of 100 mol of TFE units and perfluoroalkyl vinyl ether units.
[0058] In FEP, the content of the TFE unit is preferably 70 to 99 mol %, more preferably 80 to 99 mol %, particularly preferably 90 to 99 mol % relative to the total content of the TFE unit and the hexafluoropropylene unit.
[0059] FEP may be a copolymer consisting of only TFE units and hexafluoropropylene units, or may contain one or more other monomer units. Preferred examples of other monomers include perfluoroalkyl vinyl ethers.
[0060] When other monomer units are contained, the total content thereof is preferably 0.1 to 10 mol, more preferably 0.1 to 6 mol, particularly preferably 0.2 to 4 mol, based on 100 mol of the total of the TFE units and the hexafluoropropylene units.
[0061] In ECTFE, the content of the E unit is preferably 2 to 98 mol %, more preferably 10 to 90 mol %, particularly preferably 30 to 70 mol % based on the total content of the E unit and the chlorotrifluoroethylene unit.
[0062] ECTFE may be a copolymer consisting of only E units and chlorotrifluoroethylene units, or may contain other monomer units.
[0063] Preferred examples of other monomers include perfluoroalkyl vinyl ether.
[0064] When other monomer units are contained, the total content thereof is preferably 0.1 to 10 mol, more preferably 0.1 to 5 mol, particularly preferably 0.2 to 4 mol, based on 100 mol of the total of the E units and the chlorotrifluoroethylene units.
[0065] Particle A may contain low boiling point components. Specific examples of low boiling point components include unreacted monomers in the monomers used to polymerize the specific fluororesin, low molecular weight fluorinated polymers (oligomers, etc.) generated when polymerizing the specific fluororesin, and polymerization solvents used to polymerize the specific fluororesin, but are not limited thereto.
[0066] According to the method for producing particles of the present invention, at least a part of low-boiling-point components that may be contained in the particles A can be removed.
[0067] When particle A contains a low-boiling point component, the content of the low-boiling point component is preferably greater than 0 mass % and less than 0.5 mass %, more preferably greater than 0 mass % and less than 0.3 mass %, and particularly preferably greater than 0 mass % and less than 0.2 mass %, relative to the total mass of particle A.
[0068] Using a differential thermal and differential thermogravimetric simultaneous measuring instrument (e.g., an apparatus based on TG / DTA7200 (manufactured by Hitachi High-Tech Co., Ltd.)), 60 mg of particles A are heated from 50°C at a rate of 10°C / min in dry air and maintained at a temperature 30°C lower than the melting point of the specific fluororesin for 30 minutes. Based on the mass of particles A before and after the treatment, the content of the low-boiling point component is calculated by the following formula.
[0069] Content of low boiling point components in particle A [mass %] = 100 × (mass of particle A before treatment - mass of particle A after treatment) / mass of particle A before treatment)
[0070] The shape of the particle A is not particularly limited, and may be any shape such as a spherical shape (including an ellipsoidal shape) or a columnar shape (for example, a cylindrical shape).
[0071] The average particle size of particles A is preferably 100 μm to 10.0 mm, more preferably 0.5 mm to 10.0 mm, and particularly preferably 0.8 mm to 8.0 mm. If the average particle size of particles A is at least the lower limit of the above range, the handling property is excellent, and if it is at most the upper limit, the crushing property is excellent.
[0072] <Method for producing specific fluororesin>
[0073] Examples of the method for producing the specific fluororesin include known methods such as suspension polymerization, solution polymerization, emulsion polymerization, and bulk polymerization. Suspension polymerization and solution polymerization are preferred, and solution polymerization is particularly preferred.
[0074] As a preferred embodiment of the method for producing the specific fluororesin, there can be mentioned a method of polymerizing a unit based on a fluorine-containing monomer and a unit based on a non-fluorine monomer in the presence of a hydrofluorocarbon or a hydrofluoroether. Hereinafter, as a method for producing the specific fluororesin, description will be given based on this preferred embodiment.
[0075] In addition, the fluorine-containing monomer, the fluorine-free monomer and the specific fluorine resin are as described above, and therefore the description thereof is omitted.
[0076] Hydrofluorocarbons and hydrofluoroethers are used as polymerization solvents or chain transfer agents. Compared with fluorinated solvents containing chlorine atoms such as chlorofluorocarbons (CFCs) and hydrochlorofluorocarbons (HCFCs), hydrofluorocarbons and hydrofluoroethers have excellent environmental protection properties.
[0077] Specific examples of hydrofluorocarbons include 1,1,2,2-tetrafluorocyclobutane, CF3CFHCF2CF2CF3, CF3(CF2)4H, CF3CF2CFHCF2CF3, CF3CFHCFHCF2CF3, CF2HCFHCF2CF2CF3, CF3(CF2)5H, CF3CH(CF3)CF2CF2CF3, CF3CF(CF3)CFHCF2CF3, CF3CF(CF3)CFHCF2CF3, CF3CF(CF3)CFHCFHCF3, CF3CH(CF3)CFHCF2CF3, CF3CF2CH2CH3, and CF3(CF2)3CH2CH3.
[0078] Specific examples of hydrofluoroethers include CF3CH2OCF2CF2H,
[0079] (CF3)2CFCF(CF2CF3)OCH3, (CF3)2CFCF2OCH2CH3, (CF3)2CFCF2OCH3, CF3(CF2)3OCH2CH3, CF3(CF2)3OCH3, C3F7OCH3.
[0080] The amount of the hydrofluorocarbon or hydrofluoroether used as the polymerization solvent is preferably 20 to 99.99 parts by mass, particularly preferably 99 to 99.9 parts by mass, based on the total mass (100 parts by mass) of the polymerization solvent and the chain transfer agent.
[0081] The amount of the hydrofluorocarbon or hydrofluoroether used as the chain transfer agent is preferably 0.01 to 80 parts by mass, particularly preferably 0.1 to 1 part by mass, based on the total mass (100 parts by mass) of the polymerization solvent and the chain transfer agent.
[0082] When polymerizing a specific fluororesin, known components other than the above-mentioned monomers, hydrofluorocarbons and hydrofluoroethers can be used, for example, polymerization solvents (e.g., organic solvents other than hydrofluorocarbons and hydrofluoroethers, and water), chain transfer agents (chain transfer agents other than hydrofluorocarbons and hydrofluoroethers, such as alcohols and hydrocarbons), polymerization initiators, and polymerization inhibitors.
[0083] As the polymerization conditions (eg, reaction temperature, reaction time) for the specific fluororesin, known conditions can be adopted.
[0084] <Method for producing particles A>
[0085] The particles A are obtained, for example, by granulating the slurry containing the specific fluororesin obtained as described above. The slurry refers to a solution in a suspended state in which the specific fluororesin is dissolved or swollen in the above-mentioned polymerization solvent.
[0086] The content of the specific fluororesin is preferably 1 to 40% by mass, particularly preferably 3 to 35% by mass, based on the total mass of the slurry, from the viewpoint of excellent granulation properties.
[0087] From the viewpoint of excellent granulation properties, the content of the polymerization solvent is preferably 60 to 99% by mass, particularly preferably 65 to 97% by mass, based on the total mass of the slurry.
[0088] From the viewpoint of excellent granulation properties, the slurry is preferably mixed with water before use.
[0089] When water is mixed with the slurry for use, the water content is preferably 100 to 700 parts by mass, particularly preferably 150 to 550 parts by mass, based on 100 parts by mass of the slurry, from the viewpoint of excellent granulation properties.
[0090] As the granulation treatment, a known granulation treatment can be mentioned. As a specific example of the granulation treatment, a treatment of stirring the slurry in a granulation tank can be mentioned. The granulation treatment can be carried out while heating.
[0091] The temperature during the granulation treatment (hereinafter also referred to as "granulation temperature") may be lower than the melting point of the specific fluororesin, and specifically, it is preferably 10 to 130°C, particularly preferably 20 to 110°C.
[0092] The time of the granulation treatment and the stirring conditions (for example, the rotation speed of the stirring blade) are not particularly limited and can be appropriately set according to known conditions.
[0093] After the particle A is manufactured, it is preferred that the particle A is not heated at a temperature greater than the extrapolated melting start temperature of the specific fluororesin contained in the particle A until the specific heat treatment is performed to obtain the following particle B. Thereby, it is possible to suppress the melting of a part of the particle A, and thus it is possible to suppress the decrease in crushing property that may be caused by the melted part, so that the particle size after crushing tends to become uniform. Specifically, it is more preferred not to perform melt kneading of the particle A. Thereby, when the following particle B is crushed, the generation of fibrillar crushed products can be suppressed.
[0094] [Specific heat treatment]
[0095] The specific heat treatment is performed at the midpoint glass transition temperature (T mg ) and the extrapolated melting start temperature (T im ) or less. Thereby, particle B can be obtained. If heat treatment is carried out within the range of the heating temperature, low boiling point components can be effectively removed from particle A according to the above reasons. In addition, when the obtained particle B is subjected to pulverization treatment, there are advantages such as pulverization treatment becomes easy and generation of fibrillated pulverized products can be suppressed.
[0096] The specific heat treatment is carried out at a temperature above the midpoint glass transition temperature, but from the perspective of more effectively removing low-boiling point components from the particles A, it is preferably carried out at a temperature 10° C. or higher than the midpoint glass transition temperature (i.e., T mg +10≤the heating temperature of the specific heat treatment [°C]), preferably at a temperature 30°C or higher than the midpoint glass transition temperature (i.e., T mg +30≤the heating temperature of the specific heat treatment [°C]), and it is particularly preferred to carry out the treatment at a temperature 50°C or higher than the midpoint glass transition temperature (i.e., T mg +50≤heating temperature of specific heat treatment [℃]).
[0097] The specific heat treatment is carried out below the extrapolated melting start temperature, but from the perspective of being able to more effectively remove low-boiling point components from the particles A, it is preferably carried out at a temperature close to the extrapolated melting start temperature, and is particularly preferably carried out at the extrapolated melting start temperature. Herein, the temperature close to the extrapolated melting start temperature refers to, for example, T im -10<Heating temperature of specific heat treatment [℃]≤T im within the range of temperature.
[0098] In addition, from the perspective of making the mechanical pulverization process easier when the obtained particles B are pulverized, and from the perspective of further suppressing the generation of fibrillated pulverized products when the obtained particles B are pulverized, it is preferred to carry out the specific heat treatment at a temperature 10°C or more lower than the extrapolated melting start temperature (i.e., the heating temperature [°C] ≤ T im -10), and more preferably, the specific heat treatment is carried out at a temperature 20°C or more lower than the extrapolated melting start temperature (i.e., the heating temperature of the specific heat treatment [°C] ≤ T im -20), and it is particularly preferred to carry out the treatment at a temperature 30°C or more lower than the extrapolated melting start temperature (i.e., the heating temperature of the specific heat treatment [°C] ≤ T im -30).
[0099] In addition, other preferred ranges can be listed as specific heat treatments. For example, specific heat treatments are preferably performed at a temperature that is 10°C higher than the midpoint glass transition temperature and 10°C lower than the extrapolated melting start temperature (i.e., T mg +10≤Heating temperature of specific heat treatment[℃]≤T im -10), more preferably at a temperature 30°C higher than the midpoint glass transition temperature and 20°C lower than the extrapolated melting start temperature (ie, T mg +30≤Heating temperature of specific heat treatment[℃]≤T im -20), and it is particularly preferred to be carried out at a temperature 50°C higher than the midpoint glass transition temperature and 30°C lower than the extrapolated melting start temperature (i.e., T mg +50≤Heating temperature of specific heat treatment[℃]≤T im -30).
[0100] The midpoint glass transition temperature and extrapolated melting start temperature of ETFE vary depending on the content of each unit contained in ETFE, but generally, the midpoint glass transition temperature of ETFE is 40 to 100°C, and the extrapolated melting start temperature of ETFE is 160 to 250°C.
[0101] The time of the specific heat treatment (heat treatment time of particle A) can be appropriately set according to the heating temperature during the specific heat treatment, but from the perspective of more effectively removing low-boiling point components from particle A, facilitating the pulverization of the obtained particle B, and suppressing the production of fibrillated pulverized products, it is preferably 30 minutes to 10 hours, more preferably 40 minutes to 6 hours, and particularly preferably 60 minutes to 3 hours.
[0102] When the heating temperature during the specific heat treatment is 40° C. or more lower than the extrapolated melting start temperature, the time of the specific heat treatment is preferably 30 minutes to 10 hours, preferably 60 minutes to 5 hours, and preferably 60 minutes to 3 hours.
[0103] In addition, in the case of a direct heating method such as hot air drying for a specific heat treatment, if the heating temperature is 60°C or more lower than the extrapolated melting start temperature, the specific heat treatment time is preferably 30 minutes to 10 hours, preferably 60 minutes to 8 hours, and preferably 60 minutes to 5 hours. Among them, when a hot air drying method is used in which hot air passes between particles A, even if the heating temperature is low and the heat treatment time is short, low boiling point components can still be efficiently removed.
[0104] In addition, in the case of an indirect heating method such as a conical dryer, if the heating temperature is 60° C. or more lower than the extrapolated melting start temperature, the specific heat treatment time is preferably 1 to 20 hours, preferably 5 to 10 hours. In the case of an indirect heating method, even if a part of the particles A are damaged during the specific heat treatment, since there is no blowing as in the direct heating method, the particles B can still be almost completely recovered.
[0105] From the perspective of further reducing the generation of white smoke caused by the evaporation of low-boiling-point components during molding and obtaining a molded body with fewer foaming marks on the surface, it is preferred to carry out the specific heat treatment in a manner that the reduction ratio of the low-boiling-point components before and after the specific heat treatment represented by the following formula reaches 20 to 100%, more preferably 40 to 100%, and particularly preferably 50 to 100%.
[0106] The reduction ratio of the low boiling point components before and after the specific heat treatment [%] = 100×(the content of the low boiling point components contained in the particle A-the content of the low boiling point components contained in the particle B) / (the content of the low boiling point components contained in the particle A).
[0107] The specific heat treatment can be performed using a known heat treatment apparatus. From the viewpoint of more effectively removing low boiling point components, the specific heat treatment can be performed while the particles A are stirred.
[0108] As a heat treatment device, any one of a direct heating method and an indirect heating method can be used. As a direct heating method, a solid phase polymerization device such as a rack furnace (shed oven) (hot air circulation thermostat) or a heat treatment tank, a fluidized bed dryer can be used. As an indirect heating method, a conical dryer such as a vacuum drum dryer, a paddle dryer, a steam tube dryer, a reverse conical dryer, a Nauta mixer, etc. can be used. In addition, a direct heating method and an indirect heating method can be used in combination. In addition to the above-mentioned heating by hot air or heating jacket, an infrared heater or the like may be used.
[0109] [Particle B]
[0110] Particles B are particles containing a specific fluororesin and are obtained by subjecting particles A to a specific heat treatment.
[0111] Particle B may contain the above-mentioned low boiling point component. However, since at least a part of the low boiling point component is removed from particle A by a specific heat treatment, the content of the low boiling point component is less than that which may be contained in particle A.
[0112] When particle B contains a low boiling point component, the content of the low boiling point component in particle B is preferably 0 to 0.1% by mass, more preferably 0 to 0.05% by mass, and particularly preferably 0 to 0.03% by mass, relative to the total mass of particle B.
[0113] The method for calculating the content of the low-boiling-point component that may be contained in the particle B is the same as the method for calculating the content of the low-boiling-point component that may be contained in the particle A, except that the particle B is used.
[0114] The shape and average particle size of the particles B are not particularly limited and are the same as those of the particles A, so description thereof is omitted.
[0115] [Crushing treatment]
[0116] The method for producing particles of the present invention may include a pulverization treatment of pulverizing particles B. In this way, particles C having a smaller particle size than particles B can be obtained.
[0117] Since the particles B are particles obtained by the above-mentioned specific heat treatment, they can be easily pulverized by a mechanical pulverization treatment, and the generation of fibrillated pulverized materials during pulverization can be suppressed.
[0118] The pulverization is preferably implemented by shearing or cutting. As a specific example of the method of shearing, there is a method of applying pressure to particle B and pulverizing by applying shearing force. As a specific example of the method of cutting, a method of pulverizing by cutting particles B by cutting tools such as knives can be listed.
[0119] The pulverization can be carried out, for example, by mechanical pulverization treatment using a pulverizer, etc. Examples of the pulverizer include a turbo mill, a cross-mill, a rotor mill, and a carding mill.
[0120] The pulverization may be carried out at room temperature or while heating.
[0121] [Particle C]
[0122] Particles C are obtained by pulverizing particles B and are particles containing a specific fluororesin.
[0123] The average particle size of particles C is preferably 10 to 1000 μm, more preferably 20 to 500 μm, and particularly preferably 25 to 400 μm. When the average particle size of particles C is at least the lower limit of the above range, the handling property is excellent, while when it is at most the upper limit, the surface smoothness after melting is excellent.
[0124] The apparent density of particles C is preferably 0.3 to 1.2 g / cm 3 , more preferably 0.4 to 1.1 g / cm 3 , particularly preferably 0.5 to 1.0 g / cm 3 When the apparent density of the particles C is at least the lower limit of the above range, the handling properties are excellent, and when it is at most the upper limit, the surface smoothness is excellent.
[0125] An aggregate composed of a large number of particles C is also called a powder, and is used as a powder coating in the field of coatings, for example.
[0126] The powder may contain components other than the fluororesin contained in the particles C. Specific examples of components other than the fluororesin include additives such as flow improvers (e.g., silica, alumina), reinforcing agents (e.g., inorganic fillers), thermal stabilizers (e.g., cuprous oxide, cupric oxide, cuprous iodide, cupric iodide), ultraviolet absorbers, and acid absorbers (e.g., composite metal oxides, metal compounds). Components other than the fluororesin may be mixed with the particles C for use.
[0127] [Method for producing molded article]
[0128] The method for producing a molded article of the present invention is a method for obtaining a molded article containing the specific fluororesin by melting particles (specifically, particles B or particles C) produced by the above-mentioned method for producing particles at or above the melting point of the specific fluororesin.
[0129] Since the method for producing a molded body of the present invention uses the particles B obtained by the above-mentioned specific heat treatment or the particles C obtained by pulverizing the particles B, the generation of white smoke during the production of the molded body can be suppressed. In addition, a molded body with suppressed foaming marks caused by low boiling point components can be obtained.
[0130] The melting of particles B or particles C can be carried out by using a known device capable of melt-kneading. Examples of such a device include a twin-screw extruder.
[0131] The twin-screw extruder preferably includes two screws, a barrel housing the two screws, a vacuum exhaust pipe provided in the barrel, a raw material supply port provided in the barrel, and a die provided at the downstream end of the barrel.
[0132] The twin-shaft extruder can be a co-rotating twin-shaft extruder that rotates in the same direction 2 screws of the barrel of the screw barrel that penetrates the through hole, or can be a counter-rotating extruder that rotates 2 screws in different directions. As a twin-shaft extruder, from the perspective of excellent carrying capacity, melting and mixing capacity, separation (dehydration) ability and being able to carry out continuous resin treatment, the efficiency of the treatment process is also excellent, preferably a co-rotating twin-shaft extruder.
[0133] The meshing of the two screws may be non-meshing, partially meshing or fully meshing.
[0134] Examples of the screw include a screw in which a plurality of screw elements are mounted on a shaft.
[0135] The screw element preferably has the same cross-sectional shape in the direction perpendicular to the axis. In the screw element, the spiral angle rotating around the axis as the center according to the number of spiral fins and the cross-sectional shape in the direction perpendicular to the axis exerts a unique function. As screw elements, there are rotating elements, kneading elements, and mixing elements according to different functions.
[0136] Examples of the rotating element include a screw element having a helical angle that continuously rotates around an axis and has a conveying capacity.
[0137] Examples of the kneading element include a screw element composed of a plurality of plate-like circular plates having no helical angle.
[0138] Examples of the mixing element include a screw element having notches formed on all flight elements of a normal thread or a screw element having notches formed on all flight elements of a reverse thread. The mixing element may or may not have a self-cleaning property.
[0139] As the screw of the twin-screw extruder, a screw composed of a rotating element, a kneading element, and a mixing element is preferably used.
[0140] The barrel preferably has a structure in which a plurality of barrel sections are connected in series.
[0141] The barrel section is preferably formed with a through hole corresponding to the cross-sectional shape of the screw.
[0142] The vacuum exhaust pipe can further remove low-boiling point components that may be contained in the specific fluororesin when the particles B or particles C are melt-kneaded by the screws of the twin-screw extruder.
[0143] The vacuum exhaust pipe can be provided in the twin-screw extruder by using a barrel segment with a vacuum exhaust pipe, for example. The vacuum exhaust pipe can be provided in a plurality of barrel segments.
[0144] The die preferably has a structure that can extrude the specific fluororesin to form a strand.
[0145] The number of discharge ports in the die may be one or more. The die is preferably one that can form a plurality of strands, and preferably has several to dozens of discharge ports from the viewpoint of good productivity.
[0146] The temperature of melt kneading is preferably 10 to 150°C higher than the melting point of the specific fluororesin, more preferably 20 to 130°C higher, particularly preferably 30 to 100°C higher.
[0147] The melting point of the specific fluororesin of the present invention refers to the temperature (°C) corresponding to the maximum value of the melting peak of the specific fluororesin when the temperature of the specific fluororesin is increased at a rate of 10°C / min, as recorded by a differential scanning calorimeter (e.g., an apparatus based on DSC 7020 (manufactured by Seiko Instruments)).
[0148] The specific fluororesin is extruded from a die of a twin-screw extruder and molded into a desired shape. The shape of the molded body containing the specific fluororesin may be any shape such as a pellet or a film.
[0149] When pellets are produced as a molded body, there can be mentioned a method of obtaining pellets by extruding a molten specific fluororesin from a die attached to a discharge port of a twin-screw extruder to form strands, and then cutting the strands with a pelletizer.
[0150] When a film is produced as a molded body, a method of extruding a molten specific fluororesin from a die attached to a discharge port of a twin-screw extruder to form a film can be cited.
[0151] Although the method of obtaining a molded body by melting the particles B or particles C using a twin-screw extruder is shown, a molded body can also be produced by the following method.
[0152] For example, when a powder composed of a large number of particles C is used as a powder coating, the powder can be coated (for example, electrostatically coated) on a substrate. After the coating layer composed of the powder is formed, the coating layer is melted by heating to form a coating film (an embodiment of a molded body) on the substrate.
[0153] Example
[0154] The present invention is described in detail below by giving examples. However, the present invention is not limited to these examples. In addition, the blending amount of each component in the following table is expressed on a mass basis.
[0155] [Ratio of units]
[0156] The ratio of each unit in the fluororesin is calculated from data measured by melt NMR analysis, fluorine content analysis, and infrared absorption spectrum analysis.
[0157] [Mid-point glass transition temperature and extrapolated melting start temperature]
[0158] The midpoint glass transition temperature and the extrapolated melting start temperature of the fluororesin were determined based on a DSC curve measured with a differential scanning calorimeter (DSC 7020, manufactured by Seiko Instruments) in accordance with JIS K7121 (1987).
[0159] [Melting point]
[0160] The melting peak of the fluororesin when the temperature is increased at a rate of 10°C / min is recorded using a differential scanning calorimeter (DSC 7020, manufactured by Seiko Instruments Co., Ltd.), and the temperature (°C) corresponding to the maximum value of the melting peak of the fluororesin is determined, and this value is taken as the melting point of the fluororesin.
[0161] [Content of low boiling point components]
[0162] Using a differential thermal and differential thermogravimetric analyzer (TG / DTA7200, manufactured by Hitachi High-Tech Corporation), 60 mg of particles (particles containing fluororesin) were heated from 50°C at a rate of 10°C / min in dry air, and the fluororesin was maintained at 230°C for 30 minutes. The mass of the particles before and after the treatment was calculated by the following formula.
[0163] Content of low boiling point components in particles [mass %] = 100 × (mass of particles before treatment - mass of particles after treatment) / mass of particles before treatment)
[0164] [Reduction ratio of low boiling point components before and after heat treatment]
[0165] Reduction ratio of low boiling point components in particles before and after heat treatment [%] = 100 × (content of low boiling point components contained in particles before heat treatment - content of low boiling point components contained in particles after heat treatment) / content of low boiling point components contained in particles before heat treatment)
[0166] [Average particle size]
[0167] The particles were dispersed in a 0.1 mass % surfactant (Nycool 1308FA (90), manufactured by Nippon Emulsifier Co., Ltd.) aqueous solution, and the volume-based median particle size was measured using a laser diffraction scattering particle size distribution analyzer (LA-920, manufactured by Horiba Manufacturing Co., Ltd.).
[0168] [Apparent density]
[0169] The apparent density of the particles was measured in accordance with JIS K6819.
[0170] [Putting test]
[0171] The pulverized particles of the Examples and Comparative Examples were filled in a rectangular mold of 2 cm × 5 cm placed on a glass slide so that the film thickness after sintering was about 200 μm. After gently removing the mold, the film was sintered in an electric furnace at 300°C for 60 minutes. The foaming state of the sintered coating was visually observed and evaluated using the following criteria. The results are shown in Table 1.
[0172] ◎: No foaming marks were observed at all.
[0173] ○: Almost no foaming mark was confirmed.
[0174] ×: Foaming marks were confirmed throughout the entire area.
[0175] [Fibrillation test]
[0176] Each of the pulverized particles was visually observed and evaluated based on the following criteria.
[0177] Yes: fibrillation occurs
[0178] None: No fibrillation occurred
[0179] [Production of Particles A1 Comprising Fluororesin 1]
[0180] The polymerization tank with a stirring machine and a volume of 430 L was degassed. 418.2 kg of CF3(CF2)5H, 2.12 kg of PFBE, and 3.4 kg of methanol were added to the polymerization tank, and the temperature was raised to 66°C while stirring. A mixed gas of TFE / ethylene = 84 / 16 (molar ratio) was introduced into the polymerization tank until the pressure in the polymerization tank reached 1.5 MPa [gage]. A solution obtained by mixing 26 g of a 50 mass % CF3(CF2)5H solution of tert-butyl peroxypivalate and 4974 g of CF3(CF2)5H was injected into the polymerization tank to start polymerization. During the polymerization, a mixed gas of TFE / ethylene = 54 / 46 (molar ratio) and PFBE in an amount corresponding to 1.4 mol % relative to 100 mol % of the mixed gas were continuously introduced under the condition that the pressure in the polymerization tank reached 1.5 MPa [gage]. After 34 kg of TFE / ethylene mixed gas was added, the polymerization tank was cooled and residual gas was purged to terminate the polymerization. In this way, a slurry containing fluororesin 1 was obtained. Fluororesin 1 is a resin that can be melt-formed.
[0181] The slurry in the polymerization tank was transferred to an 850 L granulation tank, 340 L of water was added, and the mixture was heated at 105° C. while stirring to remove the solvent and unreacted monomers to obtain granules. The granules were dried at 150° C. for 5 hours to obtain 34 kg of particles A1 (average particle size 1.6 mm) containing fluororesin 1.
[0182] The molar ratio of the unit based on ethylene to the unit based on TFE (E unit / TFE unit) contained in the fluororesin 1 was 45.0 / 55.0 (molar ratio), and the content of the unit based on PFBE was 1.7 mol% based on the total units constituting the polymer of the fluororesin.
[0183] The midpoint glass transition temperature of fluororesin 1 is 90°C, the extrapolated melting start temperature is 240°C, and the melting point is 260°C.
[0184] [Example 1]
[0185] 25 kg of particles A1 containing fluororesin 1 were stored in a heat treatment tank (hot air method, manufactured by Osaka Reken Co., Ltd.) and heat treated at 150° C. for 1 hour to obtain particles B1 containing fluororesin 1.
[0186] The obtained particles B1 were pulverized with a turbo pulverizer (manufactured by Turbine Industry Co., Ltd.) to obtain particles C1 containing the fluororesin 1.
[0187] [Examples 2 to 6, Comparative Examples 1 to 2]
[0188] Except that the heat treatment conditions (heat treatment temperature, heat treatment time) of particle A1 were changed to those shown in Table 1, heat-treated particles B2 to B8 and pulverized particles C2 to C8 were obtained in the same manner as in Example 1.
[0189] [Table 1]
[0190]
[0191] [Examples 7 to 14]
[0192] 20 kg of particles A1 containing fluororesin 1 were placed in a vacuum drum dryer (50 L) manufactured by Nikko Kogyo Co., Ltd. (Nikko Kogyo) and heat treated at a rotation speed of 10 rpm and a vacuum degree of 5 torr at the temperature and time shown in Table 2. After the heat treatment, the particles were pulverized in the same manner as in Example 1.
[0193] [Table 2]
[0194]
[0195] [Examples 15 to 17]
[0196] 15 kg of particles A1 containing fluororesin 1 were heat treated using a batch fluidized bed dryer (B-FBD) manufactured by Nara Machinery Co., Ltd. at a heat treatment temperature of 200°C and for the time shown in Table 3. After the heat treatment, the particles were pulverized in the same manner as in Example 1.
[0197] [Table 3]
[0198]
[0199] [Examples 18 to 21]
[0200] 15 kg of particles A1 containing fluororesin 1 were heat treated using a small hot air circulation thermostat TRO-52DPA manufactured by Kato Corporation under the hot air temperature and time conditions shown in Table 4. After the heat treatment, the particles were pulverized in the same manner as in Example 1.
[0201] [Table 4]
[0202]
[0203] [Example 22]
[0204] When a lining test was performed on particles C1 to C6 and C9 to C21 under the following conditions, it was confirmed that white smoke from low-boiling point components was significantly reduced compared to particle C8.
[0205] Lining test: It is carried out in a vibration furnace. The particles are put into a steel pipe with an outer diameter of 20 mm and heated by direct flame for lining. After a certain period of time, a part of the flange is opened and the white smoke from the low boiling point component is visually observed.
[0206] As shown in Tables 1 to 4, it was confirmed that when the particles containing the melt-formable fluororesin were heat-treated at a temperature higher than the midpoint glass transition temperature and lower than the extrapolated melting start temperature, the low boiling point components were removable well (Examples 1 to 21).
[0207] On the other hand, when the particles containing the melt-moldable fluororesin were heat-treated at a temperature higher than the extrapolated melting start temperature, the particles were fused to each other and could not be pulverized, and various evaluations could not be performed (Comparative Example 1).
[0208] Furthermore, when the particles containing the melt-moldable fluororesin were heat-treated at a temperature lower than the midpoint glass transition temperature, it was confirmed that the removability of the low-boiling point components was poor (Comparative Example 2).
[0209] In addition, the entire contents of the specifications, claims, and abstracts of Japanese Patent Application No. 2018-245705 filed on December 27, 2018 and Japanese Patent Application No. 2019-168193 filed on September 17, 2019 are cited here as a disclosure of the description of the present invention.
Claims
1. A method for producing particles, It is characterized in that Particles A containing a melt-formable fluororesin are heat-treated at a temperature above the midpoint glass transition temperature and below the extrapolated melting start temperature to obtain particles B containing the fluororesin, wherein: The heat treatment time is 30 minutes to 10 hours. The fluorine resin is obtained by polymerizing a fluorine-containing monomer and a non-fluorine monomer in the presence of a hydrofluorocarbon or a hydrofluoroether, The particles A are particles obtained through a step of drying a slurry containing the fluororesin to obtain granules containing the fluororesin, and then drying the granules.
2. The method for producing particles according to claim 1, It is characterized in that The temperature of the heat treatment is a temperature higher than the midpoint glass transition temperature by 10° C. or more and lower than the extrapolated melting start temperature by 10° C. or more.
3. The method for producing particles according to claim 1, in, The fluorine-containing monomer is at least one selected from tetrafluoroethylene, hexafluoropropylene, perfluoro(alkyl vinyl ether), chlorotrifluoroethylene, vinylidene fluoride, and vinyl fluoride, The non-fluorine monomer is at least one selected from ethylene, propylene, itaconic anhydride, and vinyl acetate.
4. The method for producing particles according to claim 1, in, The fluororesin is any one of a copolymer containing a unit based on tetrafluoroethylene and a unit based on ethylene, a copolymer containing a unit based on chlorotrifluoroethylene and a unit based on ethylene, a copolymer containing a unit based on tetrafluoroethylene and a unit based on perfluoro(alkyl vinyl ether), and a copolymer containing a unit based on tetrafluoroethylene and a unit based on hexafluoropropylene.
5. The method for producing particles according to claim 1, in, The fluororesin is a copolymer containing units based on tetrafluoroethylene and units based on ethylene, and the copolymer further contains a monomer F1 represented by the following formula (F1): CH 2 =CX(CF 2 ) n Y(F1) X and Y are each independently a hydrogen atom or a fluorine atom, and n is an integer of 2-8.
6. The method for producing particles according to claim 1, in, The average particle size of the particles A is 100 μm to 10.0 mm.
7. The method for producing particles according to claim 1, in, The particles A contain a low boiling point component, and the content of the low boiling point component is greater than 0 mass % and 0.5 mass % or less relative to the total mass of the particles A.
8. The method for producing particles according to claim 7, in, The reduction ratio of the low boiling point components before and after the heat treatment calculated by the following formula using the content of the low boiling point components contained in the particles A and B is 20 to 100%: The reduction ratio of low boiling point components before and after heat treatment [%] = 100 × (the content of low boiling point components contained in particle A - the content of low boiling point components contained in particle B) / (the content of low boiling point components contained in particle A).
9. The method for producing particles according to claim 1, in, The particles B are pulverized to obtain particles C.
10. The method for producing particles according to claim 9, in, The average particle size of the particles C obtained by pulverizing the particles B is 10 to 1000 μm.
11. The method for producing particles according to claim 9 or 10, in, The apparent density of the particles C obtained by pulverizing the particles B is 0.3 to 1.2 g / cm 3 .
12. A method for producing a formed body, It is characterized in that The particles produced by the production method according to any one of claims 1 to 11 are melted at a temperature not lower than the melting point of the fluororesin to obtain a molded body containing the fluororesin.