Polyimide film and preparation method thereof

By introducing all-alicyclic diamine and aromatic diamine into the polyimide chain, the charge transfer between the molecular chain is reduced, and a high thermal stability and light-colored transparent polyimide film is prepared, which solves the dark color of the traditional film The problem is applicable to the field of high optical transparency.

CN118930924AActive Publication Date: 2024-11-12ZHUHAI E-SUN MATERIALS TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411232059.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

Traditional aromatic polyimide films have dark colors due to the charge transfer and complexation between molecular chains, which limit their application in the field of high optical transparency, especially in display devices.

Method used

Introducing cheap all-alicyclic diamine into the polyimide chains to reduce the charge transfer and complexation between molecular chains. By combining aromatic diamines, high thermal stability and Light-colored transparent polyimide film.

Benefits of technology

Polyimide films with high thermal stability and good optical transparency are achieved, which simplifies the preparation process and is environmentally friendly. They are suitable for packaging, microelectronics manufacturing and display devices with high optical transparency requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to a polyimide film and a preparation method thereof.The preparation method comprises the steps that NBDA and / or M-Tol are / is dissolved in DMAC, N2 is introduced, stirring is conducted till the NBDA and / or M-Tol are / is completely dissolved, and a mixed solution is obtained; adding BPADA or ODPA into the mixed solution, maintaining the introduction of N2, and reacting for a period of time to obtain a PAA glue solution; the preparation method comprises the following steps: dropping PAA glue liquid on a tool plate, uniformly coating the tool plate according to a required thickness, putting the tool plate into a drying oven, carrying out thermal imidization, taking out the tool plate, naturally cooling the tool plate to room temperature, putting the tool plate into warm water until a film coated on the tool plate falls off from the tool plate, putting the film into the drying oven, and drying to obtain a finished product. And cooling to obtain the polyimide film. The preparation method of the polyimide film is simple and environment-friendly, and the polyimide film has good optical transparency and thermal properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field The present invention relates to polymer materials, in particular to layered products actually composed of synthetic resins, and more particularly to a protective film, such as a polyimide film. The present invention also relates to a method for manufacturing the protective film (i.e., the polyimide film). Background Art Polyimide (PI) is a high-performance polymer containing repeated imide ring units on the main chain. Its special structure gives it excellent chemical resistance, radiation resistance, thermal stability and other properties. It is widely used in aerospace engineering, microelectronics, automotive and other fields. PI has been processed into various types of materials, such as films, coatings, foams, fibers, adhesives, etc. Among various PI products, film is one of the most dominant types. Due to its excellent performance, it is widely used in packaging, microelectronics manufacturing, solar substrates, etc., such as base film for flexible printed circuits (FPC), chip-scale packaging (CSP), etc. However, traditional aromatic PI presents dark brown or dark yellow-brown due to the charge transfer complexation (CTC) generated between molecular chains, which limits its application in fields requiring high optical transparency and display devices. Therefore, the research and development of light-colored transparent PI films with excellent properties has become a hot topic for researchers and a difficulty that needs to be overcome urgently. Summary of the invention The technical problem to be solved by the present invention is to avoid the deficiencies of the above-mentioned prior art and provide a polyimide film and a preparation method thereof. The preparation method of the polyimide film of the present invention introduces a low-cost fully alicyclic diamine into the polyimide (PI) chain. The fully alicyclic diamine is an isomeric monomer with a norbornane skeleton structure, which can effectively reduce the charge transfer complexation generated between molecular chains to prepare a light-colored or even colorless and transparent polyimide (PI) film. On this basis, aromatic diamines are introduced to prepare a light-colored polyimide (PI) film with both high transparency and good thermal properties, so that the polyimide film of the present invention has the characteristics of high thermal stability and light color and transparency.

[0004] The technical solution adopted by the present invention to solve the technical problem is: A method for preparing a polyimide film is provided, comprising the following steps in sequence: Step A: dissolving bicyclo[2.2.1]heptanedimethylamine or 2,2'-dimethyl-4,4'-diaminobiphenyl of a diamine monomer in a solvent N,N-dimethylacetamide, introducing nitrogen, and stirring until completely dissolved to obtain a mixed solution; Step B: adding bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride to the above mixed solution, maintaining the introduction of nitrogen, and reacting for a period of time to obtain a polyamic acid glue solution; Step C: drop the above polyamic acid glue liquid on the tool plate, and evenly coat the tool plate with the required thickness, put it into an oven for thermal imidization, then take out the tool plate, cool it naturally to room temperature, then put the tool plate into warm water until the film coated on the tool plate falls off the tool plate, and then place the film in an oven for drying, and obtain a polyimide film after cooling.

[0005] The molar ratio of the bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride to the bicyclo[2.2.1]heptane dimethylamine or 2,2'-dimethyl-4,4'-diaminobiphenyl is (1-1.02):1.

[0006] Alternatively, another method for preparing a polyimide film is provided, comprising the following steps in sequence: Step A: dissolving bicyclo[2.2.1]heptanedimethylamine and 2,2'-dimethyl-4,4'-diaminobiphenyl of diamine monomers in N,N-dimethylacetamide solvent, introducing nitrogen, and stirring until completely dissolved to obtain a mixed solution; Step B: adding bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride to the above mixed solution, maintaining the introduction of nitrogen, and reacting for a period of time to obtain a polyamic acid glue solution; Step C: drop the above polyamic acid glue liquid on the tool plate, and evenly coat the tool plate with the required thickness, put it into an oven for thermal imidization, then take out the tool plate, cool it naturally to room temperature, then put the tool plate into warm water until the film coated on the tool plate falls off the tool plate, and then place the film in an oven for drying, and obtain a polyimide film after cooling.

[0007] The molar ratio of the bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride to the total amount of the bicyclo[2.2.1]heptane dimethylamine and 2,2'-dimethyl-4,4'-diaminobiphenyl is (1-1.02):1; the molar ratio of the bicyclo[2.2.1]heptane dimethylamine to 2,2'-dimethyl-4,4'-diaminobiphenyl is (10-0):(0-10).

[0008] In step A, the mass percentage of N,N-dimethylacetamide in the mixed solution is 15% to 25%.

[0009] In step C, the oven is operated at 80°C / h (vacuum), 120°C / h (vacuum), 150°C / h (vacuum), 200°C / h, and 250°C / h for thermal imidization.

[0010] The present invention also provides a polyimide film, which is obtained according to the above-mentioned method for preparing the polyimide film. Specifically, the polyimide film comprises N,N-dimethylacetamide, bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride, and diamine monomers such as bicyclo[2.2.1]heptanedimethylamine and / or 2,2'-dimethyl-4,4'-diaminobiphenyl.

[0011] Compared with the prior art, the polyimide film and the preparation method thereof of the present invention have the following beneficial effects: The preparation method of the invention uses N,N-dimethylacetamide (DMAC) as a solvent, bicyclo[2.2.1]heptanedimethylamine (NBDA) and / or 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) of diamine monomers, and bisphenol A diether dianhydride (BPADA) or 4,4'-oxydiphthalic anhydride (ODPA) to synthesize a light-colored or even colorless transparent polyimide film with high thermal stability; the light-colored or even colorless transparent polyimide film with high thermal stability obtained by the invention adopts a binary polymerization and a ternary copolymerization method, and the binary polymerization obtains a nearly colorless and transparent high thermal stability polyimide film; on the basis of the binary polymerization, the aromatic diamine M-Tol is introduced by a ternary copolymerization method to obtain a light-colored or even colorless transparent polyimide film with good optical transparency and thermal properties; the preparation method of the polyimide film of the invention is simple and environmentally friendly; the polyimide film of the invention has good optical transparency and thermal properties. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 is the Fourier transform infrared spectrum of each embodiment of the polyimide film of the present invention; Figure 2 1 is a UV transmittance spectrum of each embodiment of the polyimide film of the present invention; Figure 3 is a table of ultraviolet data of various embodiments of the polyimide film of the present invention; Figure 4 is a differential scanning calorimetry (DSC) graph of various embodiments of the polyimide film of the present invention; Figure 5 is a thermogravimetric analysis (TGA) curve diagram of each embodiment of the polyimide film of the present invention; Figure 6 is a thermogravimetric analysis (DTG) curve of each embodiment of the polyimide film of the present invention; Figure 7 The following is a table of thermal properties of various embodiments of the polyimide film of the present invention. DETAILED DESCRIPTION

[0013] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0014] In the present invention, NBDA is the English abbreviation of bicyclo[2.2.1]heptanedimethylamine of the diamine monomer; DMAC is the English abbreviation of N,N-dimethylacetamide; M-Tol is the English abbreviation of 2,2'-dimethyl-4,4'-diaminobiphenyl; BPADA is the English abbreviation of bisphenol A diether dianhydride; ODPA is the English abbreviation of 4,4'-oxydiphthalic anhydride; and PAA is the English abbreviation of polyamic acid.

[0015] A method for preparing a polyimide film comprises the following steps in sequence: Step A: dissolving bicyclo[2.2.1]heptanedimethylamine (NBDA) and / or 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) of diamine monomers in a non-protonic polar organic solvent N,N-dimethylacetamide (DMAC), introducing nitrogen (N2), stirring until completely dissolved, and obtaining a colorless or light-colored transparent mixed solution; the mass percentage of N,N-dimethylacetamide (DMAC) in the mixed solution is 15% to 25%; Step B: quickly add bisphenol A diether dianhydride (BPADA) or 4,4'-oxydiphthalic anhydride (ODPA) to the above mixed solution, maintain the introduction of nitrogen (N2), and react for a period of time to obtain a colorless or light-colored transparent polyamic acid (PAA) glue solution; the reaction period in this step B is 6 hours to 24 hours, the reaction temperature is 0°C to 50°C, and the total solid content is 15% to 25%; The molar ratio of the bisphenol A diether dianhydride (BPADA) or 4,4'-oxydiphthalic anhydride (ODPA) to the bicyclo[2.2.1]heptanedimethylamine (NBDA) or 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (1-1.02):1; Alternatively, the molar ratio of the total amount of the bisphenol A diether dianhydride (BPADA) or 4,4'-oxydiphthalic anhydride (ODPA) to the bicyclo[2.2.1]heptane dimethylamine (NBDA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (1-1.02):1; the molar ratio of the bicyclo[2.2.1]heptane dimethylamine (NBDA) to 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (10-0):(0-10); Step C: drop the above polyamic acid glue liquid on a clean tool plate, such as a clean glass plate, and use a four-sided preparation device to evenly coat the tool plate, such as a glass plate, with the required thickness, and put it into an oven for thermal imidization. The oven can be thermally imidized at 80°C / h (vacuum), 120°C / h (vacuum), 150°C / h (vacuum), 200°C / h, and 250°C / h. Then take out the tool plate, such as a glass plate, and cool it naturally to room temperature. Then put the tool plate, such as a glass plate, into warm water, which refers to water at 40°C to 60°C, until the film coated on the tool plate, such as the glass plate, falls off the glass plate. Then, place the film in a blast oven for drying. The temperature of the blast oven during drying is 80 to 120°C, and the drying time is 0.5 to 1.5 hours. For example, the temperature of the blast oven during drying is 100°C, and the drying time is 1.0 hour. After cooling, a polyimide film is obtained. 80 ℃ / h (vacuum) and 120 ℃ / h (vacuum) are carried out in an oven in the early stage by using a vacuum pump to evacuate to a vacuum state. 200 ℃ / h and 250 ℃ / h are generally carried out by transferring to another high-temperature oven.

[0016] The present invention also provides a polyimide film obtained by the above-mentioned preparation method of the polyimide film. The polyimide film of the present invention comprises N,N-dimethylacetamide (DMAC), bisphenol A diether dianhydride (BPADA) or 4,4'-oxydiphthalic anhydride (ODPA), and diamine monomers such as bicyclo[2.2.1]heptanedimethylamine (NBDA) and / or 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol).

[0017] That is, the polyimide film of the present invention includes N,N-dimethylacetamide (DMAC), bisphenol A diether dianhydride (BPADA) and bicyclo[2.2.1]heptane dimethylamine (NBDA) of a diamine monomer; wherein the molar ratio of bisphenol A diether dianhydride (BPADA) to bicyclo[2.2.1]heptane dimethylamine (NBDA) is (1-1.02):1, and N,N-dimethylacetamide (DMAC) accounts for 15%-25% of the mixed solution.

[0018] Alternatively, the polyimide film of the present invention comprises N,N-dimethylacetamide (DMAC), bisphenol A diether dianhydride (BPADA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol); wherein the molar ratio of bisphenol A diether dianhydride (BPADA) to 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (1-1.02):1, and N,N-dimethylacetamide (DMAC) accounts for 15%-25% of the mixed solution.

[0019] Alternatively, the polyimide film of the present invention comprises N,N-dimethylacetamide (DMAC), bisphenol A diether dianhydride (BPADA), diamine monomers of bicyclo[2.2.1]heptane dimethylamine (NBDA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol); wherein the molar ratio of bisphenol A diether dianhydride (BPADA) to the total amount of bicyclo[2.2.1]heptane dimethylamine (NBDA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (1-1.02):1; the molar ratio of bicyclo[2.2.1]heptane dimethylamine (NBDA) to 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (10-0):(0-10), and N,N-dimethylacetamide (DMAC) accounts for 15%-25% of the mixed solution.

[0020] Alternatively, the polyimide film of the present invention comprises N,N-dimethylacetamide (DMAC), 4,4´-oxydiphthalic anhydride (ODPA) and diamine monomer bicyclo[2.2.1]heptanedimethylamine (NBDA); wherein the molar ratio of 4,4´-oxydiphthalic anhydride (ODPA) to bicyclo[2.2.1]heptanedimethylamine (NBDA) is (1-1.02):1, and N,N-dimethylacetamide (DMAC) accounts for 15%-25% of the mixed solution.

[0021] Alternatively, the polyimide film of the present invention comprises N,N-dimethylacetamide (DMAC), 4,4´-oxydiphthalic anhydride (ODPA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol); wherein the molar ratio of 4,4´-oxydiphthalic anhydride (ODPA) to 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (1-1.02):1, and N,N-dimethylacetamide (DMAC) accounts for 15%-25% of the mixed solution.

[0022] Alternatively, the polyimide film of the present invention comprises N,N-dimethylacetamide (DMAC), 4,4´-oxydiphthalic anhydride (ODPA), diamine monomers of bicyclo[2.2.1]heptane dimethylamine (NBDA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol); wherein the molar ratio of 4,4´-oxydiphthalic anhydride (ODPA) to the total amount of bicyclo[2.2.1]heptane dimethylamine (NBDA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (1-1.02):1; the molar ratio of bicyclo[2.2.1]heptane dimethylamine (NBDA) to 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is (10-0):(0-10), and N,N-dimethylacetamide (DMAC) accounts for 15%-25% of the mixed solution.

[0023] The polyimide film of the present invention is used in the fields of packaging, microelectronics manufacturing and solar substrates, for example, as a base film of a flexible printed circuit (FPC), a chip-scale package (CSP), etc., and is particularly used in objects of displays requiring high optical transparency. Example

[0024] A method for preparing a polyimide film comprises the following steps in sequence: Step A: At room temperature (25-30°C), add 5.3980 g of DMAC solvent and 0.3085 g of NBDA (2 mmol) into a 250 ml three-necked flask, introduce nitrogen (N2), and start magnetic stirring to obtain a colorless and transparent mixed solution; mmol is millimole; Step B: 1.0410 g of bisphenol A diether dianhydride BPADA (2 mmol) was quickly added to the above mixed solution, with a total solid content of 20%. After the addition of BPADA, a large amount of white flocculent precipitate appeared. After magnetic stirring for about 3 to 5 minutes, the precipitate was completely dissolved. The nitrogen (N2) was kept flowing. After reacting for 24 hours, a colorless and transparent polyamic acid (PAA) glue solution was obtained; Step C: drop the above polyamic acid glue onto a clean glass plate, and evenly coat the glass plate with a four-sided preparation device, put the glass plate into an oven, and heat the oven at 80°C / h (vacuum), 120°C / h (vacuum), 150°C / h (vacuum), 200°C / h, and 250°C / h to remove the solvent (i.e., perform thermal imidization), then take out the glass plate, cool it naturally to room temperature, and then put the glass plate into warm water until the film formed by the polyamic acid glue coated on the glass plate falls off the glass plate, and then place the film in a blast oven for drying at a temperature of 100°C for 1 hour, and after cooling, an almost colorless and transparent polyimide film is obtained, the film thickness of the polyimide film is 40 microns, and it is marked as PI-1. In this embodiment 1, the molar ratio of bisphenol A diether dianhydride (BPADA) and bicyclo[2.2.1]heptane dimethylamine (NBDA) is 1:1, and N,N-dimethylacetamide (DMAC) accounts for 20% of the total mixed solution. Example

[0025] It is basically the same as Example 1, except that the substances and amounts added in step B are different. In step B of this Example 2, ODPA is used instead of BPADA in Example 1. In step B of this Example 2, the amount of ODPA is 0.6204 g, 2 mmol, and the total solid content is also 20%. In step C of this Example 2, an almost colorless and transparent polyimide film is also obtained, and the film thickness of the polyimide film is also 40 microns, marked as PI-2. In this Example 2, the molar ratio of 4,4'-oxydiphthalic anhydride (ODPA) and bicyclo[2.2.1]heptanedimethylamine (NBDA) is 1:1, and N,N-dimethylacetamide (DMAC) accounts for 20% of the total mixed solution. Example

[0026] The method is basically the same as Example 1, except that the substances and amounts added in step A are different, specifically: Step A: At room temperature (25-30°C), add 5.6304 g of DMAC solvent, 0.1543 g of NBDA (1 mmol), and 0.2123 g of M-Tol (1 mmol) into a 250 ml three-necked flask, introduce nitrogen (N2), start magnetic stirring, and stir until completely dissolved to obtain a light-colored transparent mixed solution; The polyamic acid (PAA) glue obtained in step B is light-colored and transparent; The polyimide film obtained in step C is light-colored and transparent, and the film thickness of the polyimide film is also 40 microns, and is marked as PI-3.

[0027] In this embodiment 3, the molar ratio of bisphenol A diether dianhydride (BPADA), bicyclo[2.2.1]heptane dimethylamine (NBDA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is 10:5:5. Example

[0028] The method is basically the same as Example 3, except that the substances and amounts in step B are slightly different, specifically: Step B: 0.6204 g of ODPA (2 mmol) was quickly added to the mixed solution in step A, and the total solid content was 20%. After the addition of ODPA, a large amount of white flocculent precipitate appeared. After about 3 to 5 minutes of magnetic stirring, the precipitate was completely dissolved. The nitrogen (N2) was kept flowing. After reacting for 24 hours, a light-colored transparent polyamic acid (PAA) glue solution was obtained; The polyimide film obtained in step C is also light-colored and transparent, and the film thickness of the polyimide film is also 40 micrometers, and is marked as PI-4.

[0029] In this Example 4, the molar ratio of 4,4'-oxydiphthalic anhydride (ODPA), bicyclo[2.2.1]heptanedimethylamine (NBDA) and 2,2'-dimethyl-4,4'-diaminobiphenyl (M-Tol) is 10:5:5.

[0030] The properties of the polyimide films prepared in the above-mentioned Examples 1 to 4 were measured: 1. Determination of Fourier infrared spectrum The measurement was performed using a TENSOR27 Fourier transform infrared spectrometer from Bruker, Germany, in total reflection (ATR) mode with a test range of 4000–600 cm -1 (centimeter -1 ), the number of scans was 32, and the resolution was 4 cm -1 .

[0031] Figure 1 The infrared spectra of the polyimide films PI-1 to PI-4 obtained in Examples 1 to 4 are shown in FIG. Figure 1 The ones marked in the figure are the characteristic absorption peaks of polyimide film. Among them, 1772 cm -1 、1709 cm -1 、740 cm -1 The absorption peaks at 1361 cm-1 correspond to the asymmetric stretching vibration peak, symmetric stretching vibration peak, and bending vibration peak of C=O on the imide ring of polyimide; -1 The absorption peak at 2871-2949 cm corresponds to the CN stretching vibration peak on the imide ring; -1 The absorption peak at 3400 cm is the characteristic absorption peak of the saturated CH bond on the diamine monomers NBDA and M-Tol; -1 There is no characteristic absorption peak of amino group near the surface, nor is there any absorption peak of polyamic acid (PAA) at 1660 cm -1 and 1550 cm -1 The characteristic absorption peak at indicates that the polyimide has been completely imidized.

[0032] 2. UV optical performance test The ultraviolet optical properties of the polyimide film were measured using a UV-2550 ultraviolet spectrometer from Shimadzu Corporation of Japan, with air as a reference and a wavelength range of 200 to 800 nm.

[0033] Figure 2 The UV-visible spectra of the polyimide films PI-1 to PI-4 obtained in Examples 1 to 4; Figure 3 This is a table showing the UV data of the polyimide films PI-1 to PI-4 obtained in Examples 1 to 4.

[0034] from Figure 3 From the UV data table, we can see that the cutoff wavelength of the polyimide film is in the range of 355-367 nm; the transmittance at 450 nm is between 79.11% and 84.31%, and except for PI-3, all are higher than 81%; the maximum transmittance at 800 nm is between 87.54% and 89.13%, all are higher than 87%; in summary, the four PI films have good UV transmittance, and the PI film still has good UV transmittance after the introduction of aromatic diamine M-Tol. This is because the introduced NBDA is a non-coplanar alicyclic diamine containing a mixture of isomers, and the molecular chain contains methylene and ether bonds, which can effectively reduce the conjugation degree of the PI molecular chain, inhibit the formation of charge transfer complexes (CTC) in the molecular chain, and the disordered arrangement of different isomers can destroy the symmetry and regularity of the PI chain, weaken the intermolecular force, and thus achieve the purpose of improving the color of the film.

[0035] 3. Determination of thermal properties The glass transition temperature (Tg) of the polyimide film was measured using a differential scanning calorimeter model Q20 from TA (Thermal Analysis Instruments, Inc., USA) under nitrogen (N2) conditions with a N2 flow rate of 50 mL•min -1 , the temperature was increased from 40 ℃ to 250 ℃ or 300 ℃ at a heating rate of 20 ℃ / min, and the cycle was repeated twice. The second test result was taken as the glass transition temperature of the PI film.

[0036] The thermal stability of the polyimide film was determined using a thermogravimetric analyzer model 209F3 produced by Netzsch (German Mechanical Manufacturing Group). Under nitrogen (N2) conditions, the N2 flow rate was 20 mL•min-1, the heating rate was 20 ℃•min-1, and the temperature was increased from 40 ℃ to 800 ℃ to obtain the TGA data of the PI film.

[0037] Figure 4 The DSC curves of the polyimide films PI-1 to PI-4 obtained in Examples 1 to 4 are shown in FIG. 1 . The Chinese meaning of DSC is differential scanning calorimetry (full name in English: differential scanning calorimetry, referred to as DSC). Figure 4 The horizontal axis of the DSC curve is temperature, in degrees Celsius; the vertical axis is heat flow rate, which refers to the amount of heat absorbed or released by a unit mass of sample per unit time, in watts per gram (W / g).

[0038] Figure 5The thermogravimetric analysis (TGA) graphs of the polyimide films PI-1 to PI-4 obtained in Examples 1 to 4 are shown in FIG. 1 , wherein the abscissa represents temperature in ° C. and the ordinate represents mass fraction in percentage.

[0039] Figure 6 The following are the differential thermogravimetric analysis (DTG) curves of the polyimide films PI-1 to PI-4 obtained in Examples 1 to 4, where the ordinate is DTG, in % / min, and the abscissa is temperature, in °C.

[0040] Figure 7 The following is a table showing the thermal properties of various embodiments of polyimide films.

[0041] Depend on Figure 4 and Figure 7 As can be seen from the table, the polyimide films PI-1 to PI-4 obtained in the four embodiments 1 to 4 have relatively high glass transition temperatures (T g ), glass transition temperature (T g ) ranged from 152.77 to 205.64℃, all above 152℃. The glass transition temperature (T g ) is lower than the glass transition temperature (T g ) is 30.08℃ higher, and the glass transition temperature (Tg) of PI-4 is 30.08℃ higher than that of PI-2. g ) is 45.82 ℃ higher. This is because M-Tol is a biphenyl structure. Its introduction into the PI chain can enhance the rigidity of the chain, thereby restricting the movement of the chain. Therefore, the glass transition temperature (T g ) is significantly improved; combined with the test data of the ultraviolet optical properties of the PI film, it is shown that the introduced aromatic diamine monomer M-Tol can significantly improve the heat resistance of the PI film without significantly reducing the optical properties of the PI film.

[0042] Depend on Figure 5 , Figure 6 and Figure 7 As can be seen from the table, the polyimide films PI-1 to PI-4 obtained from the four embodiments 1 to 4 have relatively high initial thermal decomposition temperatures (T d ) and the temperature corresponding to the maximum decomposition rate (T dmax ); where the initial thermal decomposition temperature (T d ) is around 480 ℃, the temperature range is 479.0~485.2 ℃; the maximum decomposition rate (T dmax) The corresponding temperature is between 499.2 and 503.8 °C, and the four have little difference. The carbon residue rate (R w800 ) are all above 20%, among which the R w800 R of polyimide film PI-1 w800 The R of polyimide film PI-4 is 24.35% higher. w800 R w800 It is 22.28% higher. This is because the M-Tol introduced in the polyimide film PI-3 and the polyimide film PI-4 is a biphenyl structure, and a large number of benzene ring structures are introduced into the molecular chain, which increases its thermal stability. Combined with the ultraviolet optical performance test data of the PI film, it shows that the introduced aromatic diamine monomer M-Tol can significantly increase the thermal stability of the polyimide film without significantly reducing the optical properties of the polyimide film.

[0043] Compared with the prior art, the light-colored or even colorless and transparent polyimide film with high thermal stability obtained by the present invention adopts the method of binary polymerization and ternary copolymerization. The binary polymerization obtains a nearly colorless and transparent high thermal stability polyimide film; on the basis of binary polymerization, the aromatic diamine M-Tol is introduced by ternary copolymerization to obtain a light-colored or even colorless and transparent polyimide film with good optical transparency and thermal properties. The preparation method of the present invention is simple and environmentally friendly; in summary, through the characterization and analysis of infrared spectroscopy, ultraviolet optics and thermal properties, the present invention determines that a light-colored or even colorless and transparent polyimide film with high thermal stability has been successfully synthesized.

[0044] The above-mentioned embodiments only express the preferred implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the patent scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, all equivalent changes and modifications made to the scope of the claims of the present invention should belong to the scope covered by the claims of the present invention.

Claims

1. A method for preparing a polyimide film, characterized in that: The following steps are included in sequence: Step A: dissolving bicyclo[2.2.1]heptanedimethylamine or 2,2'-dimethyl-4,4'-diaminobiphenyl of a diamine monomer in a solvent N,N-dimethylacetamide, introducing nitrogen, and stirring until completely dissolved to obtain a mixed solution; Step B: adding bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride to the above mixed solution, maintaining the introduction of nitrogen, and reacting for a period of time to obtain a polyamic acid glue solution; Step C: drop the above polyamic acid glue liquid on the tool plate, and evenly coat the tool plate with the required thickness, put it into an oven for thermal imidization, then take out the tool plate, cool it naturally to room temperature, then put the tool plate into warm water until the film coated on the tool plate falls off the tool plate, and then place the film in an oven for drying, and obtain a polyimide film after cooling.

2. The method for preparing a polyimide film according to claim 1, wherein: In step A, the mass percentage of N,N-dimethylacetamide in the mixed solution is 15% to 25%.

3. The method for preparing a polyimide film according to claim 1, wherein: The molar ratio of the bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride to the bicyclo[2.2.1]heptane dimethylamine or 2,2'-dimethyl-4,4'-diaminobiphenyl is (1-1.02):

1.

4. The method for preparing a polyimide film according to claim 1, wherein: In step C, the oven is operated at 80°C / h (vacuum), 120°C / h (vacuum), 150°C / h (vacuum), 200°C / h, and 250°C / h for thermal imidization.

5. A method for preparing a polyimide film, characterized in that: The following steps are included in sequence: Step A: dissolving bicyclo[2.2.1]heptanedimethylamine and 2,2'-dimethyl-4,4'-diaminobiphenyl of diamine monomers in N,N-dimethylacetamide solvent, introducing nitrogen, and stirring until completely dissolved to obtain a mixed solution; Step B: adding bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride to the above mixed solution, maintaining the introduction of nitrogen, and reacting for a period of time to obtain a polyamic acid glue solution; Step C: drop the above polyamic acid glue liquid on the tool plate, and evenly coat the tool plate with the required thickness, put it into an oven for thermal imidization, then take out the tool plate, cool it naturally to room temperature, then put the tool plate into warm water until the film coated on the tool plate falls off the tool plate, and then place the film in an oven for drying, and obtain a polyimide film after cooling.

6. The method for preparing a polyimide film according to claim 5, characterized in that: In step A, the mass percentage of N,N-dimethylacetamide in the mixed solution is 15% to 25%.

7. The method for preparing a polyimide film according to claim 5, characterized in that: The molar ratio of the bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride to the total amount of the bicyclo[2.2.1]heptane dimethylamine and 2,2'-dimethyl-4,4'-diaminobiphenyl is (1-1.02):1; the molar ratio of the bicyclo[2.2.1]heptane dimethylamine to 2,2'-dimethyl-4,4'-diaminobiphenyl is (10-0):(0-10).

8. The method for preparing a polyimide film according to claim 5, characterized in that: In step C, the oven is operated at 80°C / h (vacuum), 120°C / h (vacuum), 150°C / h (vacuum), 200°C / h, and 250°C / h for thermal imidization.

9. A polyimide film, characterized in that: The polyimide film obtained by the preparation method of the polyimide film according to any one of claims 1 to 8, specifically, the polyimide film comprises N,N-dimethylacetamide, bisphenol A type diether dianhydride or 4,4'-oxydiphthalic anhydride, and diamine monomers such as bicyclo[2.2.1]heptanedimethylamine and / or 2,2'-dimethyl-4,4'-diaminobiphenyl.

Citation Information

Patent Citations

  • Colorless transparent polyimide thin film and preparation method thereof

    CN108424540A

  • Preparation method for polyimide film

    CN109337101A

  • Colorless and transparent copolyimide film and preparation method thereof

    CN113072702A

  • Polyimide composite flocculus and preparation method thereof

    CN117067732A

  • Polyamic acids resin composition comprising polyfunctional photo-crosslinkable monomer and photosensitive polyimides resin composition manufactured therefrom