Preparation method of waste-paper-based cellulose aerogel and modified asphalt of waste-paper-based cellulose aerogel
By adding waste paper-based cellulose aerogel and polyethylene glycol to the asphalt, the problems of asphalt pavement are prone to deformation and poor crack resistance at high temperatures are solved, the resistance to rut and thermal stability of asphalt is improved, and the road surface is extended The service life and reduce production costs, achieving the development of green and environmentally friendly asphalt pavement materials.
Patent Information
- Application Number
- CN202410909540.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-12
AI Technical Summary
Existing asphalt pavement materials are prone to permanent deformation, poor crack resistance and insufficient thermal stability at high temperatures, resulting in reduced pavement flatness, shortened service life, and large weight, affecting economic benefits.
Use waste paper-based cellulose aerogel and polyethylene glycol as modifiers to prepare waste paper-based cellulose aerogel and mix it with asphalt to form high-performance modified asphalt to enhance the resistance to rut and resistance of asphalt. Cracking and thermal stability.
It significantly improves the rut resistance, thermal performance and water resistance of asphalt, reduces the possibility of permanent deformation and thermal cracking, extends the service life of the road surface, reduces production costs, and meets green and environmental protection requirements.
Smart Images

Figure BDA0004933155300000081 
Figure HDA0004933155310000011 
Figure HDA0004933155310000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road engineering material preparation, and specifically relates to a preparation method of waste paper-based cellulose aerogel and modified asphalt thereof. Background Art
[0002] With the development of my country's economy and transportation industry, the traffic volume is increasing, and the requirements for highway construction are becoming increasingly stringent. Most high-grade highways use asphalt pavement, but as a temperature-sensitive viscoelastic material, asphalt is more viscous at high temperatures and is very likely to undergo permanent deformation when subjected to large loads. The main manifestations are: the rutting phenomenon caused by the lateral displacement of the structural layer material due to the additional compaction of the pavement structure layer and the soil base under the repeated load of driving; the displacement caused by the insufficient shear strength of the asphalt mixture pavement under the horizontal load; the structural damage cracks caused by the action of driving loads and the temperature cracks caused by the temperature change of the asphalt surface layer. Excessive deformation of the road surface not only affects the flatness of the road surface, but also reduces the thickness of the asphalt layer at the wheel track of the road surface, weakening the overall strength of the surface layer and the road surface structure, which is easy to induce other diseases. In addition, the permanent deformation of the road surface seriously affects the service life of the road surface and even aggravates the occurrence of other road diseases, such as looseness, potholes, cracks, etc., thereby reducing the use quality of the asphalt pavement, shortening its service life, and bringing huge economic losses.
[0003] In order to improve the above problems, in the prior art, SBS modifier (styrene-butadiene-styrene block copolymer) is usually added to the asphalt mixture or anti-rutting agent is added for modification. For example, the invention patent CN109180077B discloses an asphalt mixture and its production process, including the following components: 4-12wt% modified asphalt, 72-88wt% aggregate, 5-10wt% filler, 0.5-3wt% fiber stabilizer, 0.5-3wt% anti-rutting agent, and the oil-stone ratio is 5.6-14%; the modified asphalt includes base asphalt and SBS. The invention patent CN103059587B discloses an anti-rutting modifier for asphalt pavement and an asphalt mixture containing the anti-rutting modifier, including: high-density low-pressure polyethylene, rubber powder and rock asphalt. Although the above method improves the rutting resistance and elastic deformation ability of asphalt to a certain extent, it does not significantly improve other properties, such as pavement crack resistance, thermal stability, temperature stability, water damage resistance and weight.
[0004] Aerogel is a solid material with a nanoporous network structure composed of nanoparticles aggregated together. It has excellent properties such as ultra-low density, ultra-high specific surface area, ultra-high porosity, and low thermal conductivity. The porosity of aerogel materials is above 90%, and the mesoporous structure inside the aerogel material can make the aerogel have excellent thermal insulation properties. Therefore, aerogel can be an alternative technology to enhance the performance of asphalt by transferring its thermal properties, and aerogel can make asphalt materials more stable before temperature fluctuations. If cellulose is added in the form of aerogel, it will reduce the sensitivity of asphalt to destructive thermal effects, reduce the possibility of permanent deformation and thermal cracking, and is expected to solve the problem of heavy asphalt weight.
[0005] my country has a huge annual output of waste paper. As one of the sources of cellulose, waste paper has the characteristics of wide sources, cheap and easy to obtain, and about 50% of cellulose is contained in waste paper. The waste paper cellulose extracted after simple pretreatment as the matrix material of composite aerogel not only maintains the original performance but also reduces the cost, which is in line with green environmental protection and is an ideal matrix material for composite aerogel. However, it is generally used as an adsorbent, and there are few reports on its use in modified asphalt. In addition, the single waste paper cellulose aerogel has a simple structure and unstable performance, and needs to be improved to form a composite aerogel to improve the structural characteristics and comprehensive performance. Summary of the invention
[0006] In view of the above problems existing in the prior art, the present invention provides a method for preparing waste paper-based cellulose aerogel and modified asphalt thereof, so as to solve the problems of poor mechanical properties, poor rutting resistance, easy cracking and poor temperature stability existing in the existing modified asphalt.
[0007] To achieve the above object, the present invention adopts the following scheme: a method for preparing waste paper-based cellulose aerogel, comprising the following steps:
[0008] 1) Take waste paper, chop it, and use a high-speed multifunctional pulverizer to obtain flocculent waste paper fibers for later use;
[0009] 2) dissolving urea and sodium hydroxide in water to obtain a solvent, stirring continuously, and simultaneously adding the waste paper fibers obtained in step 1), placing the solvent in a water bath at 60° C. to 80° C. and stirring, and then adding polyacrylic acid to obtain a reaction solution, and standing overnight;
[0010] 3) placing the reaction solution obtained in step 2) in an ice water bath, then subjecting it to ultrasonic treatment at low temperature, and then allowing it to stand at -18°C to 24°C for 12 to 48 hours, and then freeze-drying it to obtain the waste paper-based cellulose aerogel.
[0011] Preferably, the mass ratio of waste paper fiber to polyacrylic acid in the reaction solution is 2:(0.1-6).
[0012] Preferably, the mass fraction of sodium hydroxide in the solvent is 1% to 5%, and the mass fraction of urea is 15% to 19%.
[0013] Another object of the present invention is to provide waste paper-based cellulose aerogel prepared by the above method.
[0014] Another object of the present invention is to provide the use of the above-mentioned waste paper-based cellulose aerogel in the preparation of modified asphalt.
[0015] Another object of the present invention is to provide a high-performance modified asphalt that is resistant to rutting and high temperature, including base asphalt, polyethylene glycol and the above-mentioned waste paper-based cellulose aerogel.
[0016] Preferably, the mass ratio of the matrix asphalt, polyethylene glycol and waste paper-based cellulose aerogel is 100:(1-20):(1-10).
[0017] Preferably, the molecular weight of the polyethylene glycol is 500-3000; and the base asphalt is 70# or 90# base asphalt.
[0018] Another object of the present invention is to provide a method for preparing the above-mentioned high-performance modified asphalt, comprising the following steps:
[0019] 1) Heat and soften the matrix asphalt to a fluid state, and then transfer it to a constant temperature of 70-110°C;
[0020] 2) adding the waste paper-based cellulose aerogel prepared above into the matrix asphalt, and then continuing to shear at a low speed under the original constant temperature conditions to obtain an asphalt / cellulose aerogel system;
[0021] 3) Continue to add polyethylene glycol to the asphalt / cellulose aerogel system in step 2), and then continue to shear at a low speed under the original constant temperature conditions. After the shearing is completed, pour the obtained modified asphalt sample onto a polytetrafluoroethylene release cloth and naturally cool to room temperature to obtain the modified asphalt.
[0022] Preferably, the shearing rotation speed is 1000-1500 rpm, and the shearing time is 20-120 min.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The present invention uses waste paper fiber and polyacrylic acid as raw materials to prepare cellulose aerogel, wherein polyacrylic acid can undergo self-crosslinking in an alkaline environment to form a three-dimensional network structure, which interacts with the network structure of waste paper fiber, and the network structure of the prepared gel is more uniform and has greater strength. The method has the characteristics of green environmental protection, recycling, and low economic benefits, and has a simple preparation process, low production cost, and is suitable for mass production, with good social benefits.
[0025] 2. In the modified asphalt of the present invention, waste paper-based fiber aerogel and polyethylene glycol are used as asphalt modifiers. On the one hand, waste paper-based cellulose aerogel is a spatial network structure with high porosity and high specific surface area. Therefore, it has good toughness and strong adsorption, so that the asphalt is effectively combined in a network structure to inhibit the generation of cracks, thereby improving the low-temperature crack resistance of the asphalt. At the same time, the addition of fibers can disperse and transfer the load on the asphalt material, make the force uniformity of the material better, and make the asphalt mixture have higher resistance to rutting and cracking. Furthermore, the addition of cellulose in the form of aerogel will reduce the sensitivity of asphalt to destructive thermal effects and reduce the possibility of permanent deformation and thermal cracking; on the other hand, further compounded polyethylene glycol can improve the high temperature, temperature sensitivity and anti-aging properties of asphalt. Therefore, the present invention greatly improves the high temperature anti-rutting performance, elasticity and water resistance of the modified asphalt, and improves the thermal properties of the modified asphalt.
[0026] 3. The cellulose aerogel modified asphalt prepared by the present invention has significant advantages over traditional asphalt modification technology in terms of environmental protection, mechanical properties, water resistance, high temperature resistance, durability, construction convenience, economic benefits, etc. At the same time, the present invention can effectively improve the recycling rate of waste paper and the level of high-value utilization, opening up a new way to develop green and low-carbon economic asphalt pavement materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the microstructure of waste paper-based fiber aerogel.
[0028] Figure 2 This is the infrared spectrum analysis diagram of waste paper-based fiber aerogel.
[0029] Figure 3 This is the relationship diagram of the composite modulus G*-frequency of different modified asphalts at 60°C.
[0030] Figure 4 This is the phase angle δ-frequency relationship diagram of different modified asphalts at 60°C.
[0031] Figure 5 Differential scanning diagrams of different modified asphalts; A is the cooling curve and B is the heating curve.
[0032] Figure 6 This is the relationship curve between mass fraction weight (%) and temperature T (℃) of different modified asphalts.
[0033] Figure 7 The microstructure of different modified asphalts under an optical microscope.
[0034] Figure 8 is the water absorption rate of different modified asphalts.
[0035] Fig. 9 Contact angle test of different modified asphalt. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below with reference to specific embodiments.
[0037] 1. A method for preparing high-performance modified asphalt mixed with waste paper-based cellulose aerogel.
[0038] Example 1
[0039] (1) A method for preparing waste paper-based cellulose aerogel, comprising the following steps:
[0040] Take waste paper such as old newspapers, office paper or packaging paper, and grind them into flocculent waste paper fibers with a diameter of 1 to 30 μm by a high-speed multifunctional grinder for later use.
[0041] 13.7 g of urea and 1.9 g of sodium hydroxide were dissolved in 84.4 g of deionized water, and dispersed with magnetic stirring for 30 minutes. Then, 2 g of waste paper fiber was added and magnetically stirred for 20 minutes. Then, it was placed in an 80°C water bath and dispersed with magnetic stirring for 2 hours. Then, 3.231 g of polyacrylic acid (PAA) was added dropwise to obtain a reaction solution, which was sealed and allowed to stand overnight. The reaction solution was taken out and placed in an ice / water bath for pre-cooling for 10 minutes. Then, it was ultrasonicated at low temperature (ice bath) for 10 minutes. After the solution was allowed to stand at -18°C for 48 hours, it was freeze-dried in a freeze dryer for 2 days to obtain the desired waste paper-based cellulose aerogel.
[0042] (2) A modified asphalt mixed with waste paper-based cellulose aerogel, comprising the following raw materials in parts by weight: 100 parts of 70# base asphalt, 20 parts of polyethylene glycol and 2 parts of waste paper-based cellulose aerogel, and prepared by the following method:
[0043] S1: Heat 70# base asphalt in a forced air oven at 140°C to soften it to a fluid state, and then transfer it to a constant temperature oil bath at 110°C.
[0044] S2: Add the prepared waste paper-based cellulose aerogel to the matrix asphalt, and then continue to shear at a low speed at a constant temperature of 110°C, with a shear rate of 1000 rpm and a shear time of 2 h to obtain an asphalt / cellulose aerogel system.
[0045] S3: Continue to add polyethylene glycol to the asphalt / cellulose aerogel system in S2, and then continue to shear at a low speed under a constant temperature of 110°C, with a shear rate of 1500rpm and a shear time of 20min. After the shearing is completed, pour the obtained modified asphalt sample onto a polytetrafluoroethylene release cloth and naturally cool to room temperature to obtain the modified asphalt.
[0046] Comparative Example 1
[0047] A modified asphalt is composed of the following raw materials in parts by weight: 100 parts of 70# base asphalt and 20 parts of polyethylene glycol; and is prepared by the following method:
[0048] S1: Heat 70# base asphalt in a forced air oven at 140°C to soften it to a fluid state, and then transfer it to a constant temperature oil bath at 110°C.
[0049] S2: Add polyethylene glycol to the base asphalt, and then perform low-speed shearing at a constant temperature of 110°C, with a shear rate of 1500rpm and a shear time of 20min. After the shearing is completed, pour the obtained modified asphalt sample onto a polytetrafluoroethylene release cloth and cool it naturally to room temperature to obtain the modified asphalt.
[0050] Comparative Example 2
[0051] A modified asphalt is composed of the following raw materials in parts by weight: 100 parts of 70# base asphalt and 2 parts of waste paper-based cellulose aerogel; and is prepared by the following method:
[0052] S1: Heat 70# base asphalt in a forced air oven at 140°C to soften it to a fluid state, and then transfer it to a constant temperature oil bath at 110°C.
[0053] S2: Add the prepared waste paper-based cellulose aerogel to the matrix asphalt, and then shear at a low speed at a constant temperature of 110°C, with a shear rate of 1000 rpm and a shear time of 2 hours. After the shearing is completed, pour the obtained modified asphalt sample onto a polytetrafluoroethylene release cloth and naturally cool to room temperature to obtain the modified asphalt.
[0054] Comparative Example 3
[0055] A modified asphalt is composed of the following raw materials in parts by weight: 100 parts of 70# base asphalt and 4 parts of SBS; and is prepared by the following method:
[0056] S1: Heat 70# base asphalt to 100°C to soften it.
[0057] S2: Add SBS to the base asphalt, heat it to 180°C, and then shear it at a low speed at a constant temperature of 110°C, with a shear rate of 1000rpm and a shear time of 2h. After the shearing is completed, pour the obtained modified asphalt sample onto a polytetrafluoroethylene release cloth and cool it naturally to room temperature to obtain the modified asphalt.
[0058] 2. Performance Testing
[0059] 1. The morphology of the waste paper-based cellulose aerogel prepared by the present invention was observed under an electron microscope. The results are as follows: Figure 1 shown.
[0060] As can be seen from the figure, the waste paper-based cellulose aerogel has a porous structure, which gives the material good air permeability and adsorption. In addition, the interlacing and entanglement between the fibers in the waste paper-based cellulose aerogel form a certain network structure, which improves the mechanical strength and elasticity of the material. The presence of fine pores greatly increases the specific surface area of the material, which is beneficial to improving its adsorption performance and reaction activity. In addition, the roughness of the fiber surface gradually increases with the increase of magnification. The rough surface can provide more active sites, which has a positive effect on adsorption.
[0061] 2. The waste paper-based cellulose aerogel prepared by the present invention was analyzed by infrared spectroscopy using a Fourier transform infrared spectrometer. The results are as follows: Figure 2 shown.
[0062] It can be seen from the figure that the aerogel has a peak at 3464 cm -1 , 2891cm -1 , 1676cm -1 , 1458cm -1 and 1165cm -1 There are obvious absorption peaks at 3464cm -1 It is the -OH stretching vibration in the cellulose structure, 2891cm -1 It is the -CH stretching vibration in the cellulose ring structure, 1676cm -1 It is -C=O stretching vibration, 1458cm -1 It is the in-plane bending vibration of -CH2 and -OCH in the cellulose structure, 1165cm -1 It is the -C=O stretching vibration in the cellulose structure. This shows that the waste paper-based cellulose aerogel still maintains the cellulose structure from dissolution to aerogel formation.
[0063] 3. The modified asphalt prepared in Example 1 and Comparative Examples 1 to 3 was subjected to rheological property test. The equipment used was a dynamic shear rheometer (DSR). The temperature was maintained at 60°C, which is usually regarded as the highest temperature of asphalt pavement. The strain was fixed at 1%. Dynamic frequency scanning was used. The frequency scanning range was 100 to 0.01 Hz. The high-temperature rheological properties of the modified asphalt were measured by scanning from high frequency to low frequency. Composite modulus G * It can reflect the anti-rutting ability of asphalt materials. * The larger the value, the better the anti-rutting ability. The phase angle δ reflects the viscoelasticity of the material, and its value is between 0 and 90°. When δ = 0°, the material is purely elastic, and when δ = 90°, the material is purely viscous. For asphalt materials under high temperature conditions, a δ value that is too high will cause the road surface to become sticky and the anti-rutting ability will decrease. The lower the δ value, the better the elasticity, that is, the greater the deformation recovery ability, and the improved anti-rutting ability. 45° is the dividing line between the elasticity and viscosity of the material.
[0064] Complex modulus G of different modified asphalt * As the frequency changes Figure 3 As shown, it can be found that in the entire scanning frequency range, when the frequency F>1Hz, the G* curves of Example 1 and Comparative Examples 1 to 3 overlap, indicating that the composite moduli of different modified asphalts in the high-frequency region are not much different; when the frequency F<1Hz, the G* curve of the modified asphalt in Example 1 is significantly higher than that of Comparative Examples 1 to 3; when the frequency F<0.1Hz, the G* curve of the modified asphalt in Example 1 presents a platform, which is due to the presence of a network structure in the system. The results show that the present invention adds polyethylene glycol and waste paper-based fiber aerogel composite modification at the same time, which significantly improves the anti-rutting performance and resistance to external permanent deformation of asphalt, and also makes the asphalt have better viscoelasticity and stiffness, thereby improving its overall mechanical properties.
[0065] The phase angle δ of different modified asphalts varies with frequency as shown in Figure 4 At low frequency, the δ value of the modified asphalt of Example 1 is significantly lower than that of Comparative Examples 1 to 3, indicating that the permanent deformation resistance and elasticity of the composite modified asphalt of the present invention are significantly improved.
[0066] 4. The modified asphalt prepared in Example 1 and Comparative Examples 1-2 was subjected to differential scanning. The results are as follows: Figure 5 shown.
[0067] As can be seen from the figure, the base asphalt and comparative example 2 have no obvious absorption and exothermic peaks, indicating that the modified asphalt obtained by the above formulation system has no crystallization; the modified asphalts of comparative example 1 and example 1 have crystallization peaks near the crystallization temperature of PEG, and also have crystallization peaks below the crystallization temperature, which is due to the occurrence of supercooling. Supercooling is a delay in the crystallization process, which often occurs in phase change materials, and the melting temperature (T m ), crystallization temperature (T c ) is greater than the composite modified asphalt of Example 1. The modified asphalt of Comparative Example 1 is more prone to supercooling during the cooling process due to its higher melting temperature and crystallization temperature. This shows that its crystal structure is tighter and the molecular chain arrangement is more regular. However, the existence of supercooling may increase the brittleness of the material, which is not conducive to its use in practical applications. In contrast, the composite modified asphalt of Example 1 exhibits lower melting temperature and crystallization temperature due to the introduction of waste paper-based cellulose aerogel, which reduces the occurrence of supercooling and improves the comprehensive performance of the material.
[0068] Furthermore, the crystallinity of the modified asphalt prepared in Example 1 and Comparative Examples 1-2 was calculated according to formula (1). The results are shown in Table 1.
[0069]
[0070] Where x (%) is the crystallinity; △Hm is the melting enthalpy; △H 100 is the melting enthalpy of 100% complete crystallization; X m is the quality score.
[0071] Table 1
[0072] sample Crystallinity x(%) Base asphalt / Comparative Example 2 / Comparative Example 1 87.85% / 97.57% Example 1 38.59% / 70.60%
[0073] Note: “ / ” indicates no crystallization.
[0074] It can be seen from Table 1 that the base asphalt and the modified asphalt of comparative example 2 are not crystallized; the modified asphalts of comparative example 1 and example 1 have two crystallinities of 87.85% / 97.57% and 38.59% / 70.60%, respectively, which is consistent with the differential scanning results. And the crystallinity of the modified asphalt of comparative example 1 is significantly greater than that of the modified asphalt of example 1. The modified asphalt of comparative example 1 exhibits excellent mechanical properties and thermal stability due to its high crystallinity. However, although example 1 has a lower crystallinity, it still has a moderate crystalline structure. This feature enables the composite modified asphalt to achieve a better balance in mechanical properties, processing properties and thermal stability, and has a broader application prospect.
[0075] 5. Thermogravimetric analysis (TGA) was performed on the base asphalt, Example 1 and Comparative Examples 1-2. The results are as follows: Figure 6And as shown in Table 2.
[0076] Table 2
[0077] sample <![CDATA[T 5% (℃)]]> <![CDATA[T max (℃)]]> Residual ash content (wt%) Base asphalt 332 531 20.80 Comparative Example 1 348 525 18.43 Comparative Example 2 326 550 20.37 Example 1 340 530 18.52
[0078] from Figure 6 As can be seen from Table 2, compared with the base asphalt, the T 5% 348℃ and 340℃ respectively, both higher than the base asphalt (332℃), indicating that their thermal stability is better than that of the base asphalt. 5% The temperature of Comparative Example 2 is 326℃, which is lower than that of the base asphalt and has poor thermal stability. max The highest (550°C), indicating that it decomposes fastest at high temperatures and may contain high heat-resistant components. max are close to each other, 531°C and 530°C, respectively, indicating that their thermal decomposition behaviors at high temperatures are similar. max The residual ash content of the matrix asphalt is 525°C, which is slightly lower than that of the matrix asphalt. The residual ash content of the matrix asphalt is the highest, which is 20.80%. The residual ash content of Example 1 and Comparative Example 1 are 18.52% and 18.43%, respectively, which are lower than that of the matrix asphalt, indicating that they are more completely decomposed at high temperatures. The residual ash content of Comparative Example 2 is 20.37%, which is close to that of the matrix asphalt. The initial decomposition temperature (T 5% ) and maximum decomposition temperature (T max ) are relatively high, and the residual ash rate is relatively low, indicating that it excels in thermal stability and high-temperature decomposition performance, and is superior to the base asphalt and comparative example 1. This shows that the thermal properties of asphalt can be significantly improved by the modification method of Example 1. Although the maximum decomposition temperature of comparative example 2 is relatively high, the initial decomposition temperature is low and the residual ash rate is relatively high, and the overall thermal stability is not as good as that of example 1. The above results show that the introduction of waste paper-based cellulose aerogel in modified asphalt significantly improves the mechanical properties, processing properties and thermal stability of the modified asphalt through its nanoscale skeleton structure, high specific surface area and good thermal stability.
[0079] 6. The modified asphalt film samples of Example 1 and Comparative Examples 1-2 were observed using an optical microscope. The results are as follows: Figure 7 shown.
[0080] Under microscope observation, the modified asphalt in comparative example 1 showed obvious phase separation structure; in the modified asphalt in comparative example 2, a large number of small particles were distributed in the matrix material, and these small particles were cellulose aerogels. Compared with comparative example 1, the modified asphalt in comparative example 2 had smaller particle size and more uniform distribution; and although the modified asphalt in Example 1 showed obvious phase separation structure and was distributed in an "island" structure, the "islands" and "islands" were mutually aggregated, and the "islands" transitioned from the "island" structure to the "network" structure, and the "network" structure provided a certain elasticity for the modified asphalt material to resist deformation. Among them, the cellulose aerogel was distributed in the asphalt phase in a block shape, and was distributed irregularly in the aerogel in a filament shape. Aerogel is a spatial network structure with the characteristics of low density, low thermal conductivity, high porosity and high specific surface area. It can not only make the modified asphalt have a certain low density, but also the large surface area can effectively disperse and transmit the load on the composite material, so that the material is more evenly stressed and the deformation resistance of the composite material is improved. Furthermore, the random distribution of waste paper fibers will constrain and hinder the material, thereby reducing the relative slip between the materials, similar to the role of reinforcing ribs. More importantly, the addition of cellulose in the form of aerogel will reduce the sensitivity of asphalt to destructive thermal effects and reduce the possibility of permanent deformation and thermal cracking. Aerogel can be an alternative technology to enhance the performance of asphalt by transferring its thermal properties and aerogel can make asphalt materials more stable before temperature fluctuations.
[0081] 7. The modified asphalt prepared in Example 1 and Comparative Examples 1-2 was placed in water for several hours. Every two hours, the surface moisture was wiped off after taking out and the water absorption rate was calculated to test the water absorption performance. The results are as follows: Figure 8 shown.
[0082] As can be seen from the figure, within 2 hours of water absorption, the water absorption rate of the modified asphalt in comparative example 2 increased the most, and the water absorption rate of the modified asphalt in Example 1 was the smallest, which may be because the cellulose aerogel itself has a strong water absorption capacity. However, after 6 hours, the water absorption rate of comparative example 2 and the matrix asphalt reached a stable level, while the water absorption rate of the modified asphalt in comparative example 1 and Example 1 was still slowly increasing, which may be because PEG is hydrophilic. The results show that the water absorption rate of the modified asphalt of the present invention is relatively small overall, which can effectively prevent the impact of floods in the rainy season.
[0083] 8. The modified asphalt prepared in Example 1 and Comparative Examples 1-2 was tested for hydrophobicity. When the contact angle θ<90°, the solid surface was hydrophilic; when the contact angle θ>90°, the solid surface was hydrophobic. Fig. 9 shown.
[0084] As can be seen from the figure, the contact angles of the three modified asphalts are all less than 90°, which shows that all three groups of samples are hydrophilic. Since cellulose aerogel itself is a strong water-absorbing substance, the modified asphalt containing cellulose aerogel (Comparative Example 2) has the greatest hydrophilicity, which is consistent with the water absorption test results. The contact angles of the modified asphalts of Comparative Example 1 and Example 1 are larger, indicating that the hydrophilicity of both is smaller. Compared with Comparative Example 2, the modified asphalt of the present invention improves the strong hydrophilicity brought by the fiber aerogel through the composite modification of waste paper-based fiber aerogel and polyethylene glycol, making its surface relatively more hydrophobic, which can improve the comprehensive performance of the modified asphalt in practical applications, especially in terms of water resistance, aging resistance and construction convenience.
[0085] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the applicant has described the present invention in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that modifications or equivalent substitutions of the technical solution of the present invention without departing from the purpose and scope of the technical solution of the present invention should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing waste paper-based cellulose aerogel, It is characterized in that The following steps are involved: 1) Take waste paper, chop it, and use a high-speed multifunctional pulverizer to obtain flocculent waste paper fibers for later use; 2) dissolving urea and sodium hydroxide in water to obtain a solvent, stirring continuously, and simultaneously adding the waste paper fibers obtained in step 1), placing the solvent in a water bath at 60° C. to 80° C. and stirring, and then adding polyacrylic acid to obtain a reaction solution, and standing overnight; 3) placing the reaction solution obtained in step 2) in an ice water bath, then subjecting it to ultrasonic treatment at low temperature for 10 to 30 minutes, and then allowing it to stand at -18°C to 24°C for 12 to 48 hours, and then freeze-drying it for 12 to 72 hours to obtain the waste paper-based cellulose aerogel.
2. The method for preparing waste paper-based cellulose aerogel according to claim 1, It is characterized in that The mass ratio of waste paper fiber to polyacrylic acid in the reaction solution is 2:(0.1-6).
3. The method for preparing waste paper-based cellulose aerogel according to claim 1, It is characterized in that The mass fraction of sodium hydroxide in the solvent is 1% to 5%, and the mass fraction of urea is 15% to 19%.
4. A waste paper-based cellulose aerogel prepared according to the method according to any one of claims 1 to 3.
5. Use of the waste paper-based cellulose aerogel as claimed in claim 4 in the preparation of modified asphalt.
6. A high performance modified asphalt, It is characterized in that The invention comprises matrix asphalt, polyethylene glycol and the waste paper-based cellulose aerogel as claimed in claim 4.
7. The high performance modified asphalt according to claim 6, It is characterized in that The mass ratio of the matrix asphalt, polyethylene glycol and waste paper-based cellulose aerogel is 100:(1-20):(1-10).
8. The high performance modified asphalt according to claim 6, It is characterized in that The molecular weight of the polyethylene glycol is 500-3000; the base asphalt is 70# or 90# base asphalt.
9. A method for preparing the high performance modified asphalt according to any one of claims 6 to 8, It is characterized in that The following steps are involved: 1) Heat and soften the matrix asphalt to a fluid state, and then transfer it to a constant temperature of 70-110°C; 2) adding the waste paper-based cellulose aerogel described in claim 4 into the matrix asphalt, and then continuing to shear at a low speed under the original constant temperature conditions to obtain an asphalt / cellulose aerogel system; 3) Continue to add polyethylene glycol to the asphalt / cellulose aerogel system in step 2), and then continue to shear at a low speed under the original constant temperature conditions. After the shearing is completed, pour the obtained modified asphalt sample onto a polytetrafluoroethylene release cloth and naturally cool to room temperature to obtain the modified asphalt.
10. The method for preparing the high-performance modified asphalt according to claim 9, It is characterized in that The rotation speed of the low-speed shearing is 1000-1500 rpm, and the time of the low-speed shearing is 20-120 min.
Citation Information
Patent Citations
Anti-rutting modifier for asphalt pavement and asphalt mixture containing anti-rutting modifier
CN103059587B
An asphalt mixture and its production process
CN109180077B
Cited By
Biomass aerogel reinforced asphalt material and preparation method thereof
CN119592089A