Preparation method and application of polysulfonamide silver nanowire aerogel
Through the preparation of polysulfone amide silver nanowire aerogel, the problems of high density and uneven structure of electromagnetic shielding materials are solved, and low-density, uniform and stable electromagnetic shielding performance is achieved, which is suitable for a variety of application fields.
Patent Information
- Application Number
- CN202411159704.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing electromagnetic shielding materials have problems such as high density, uneven structure and low shielding performance. The mechanical properties of the composite materials are reduced after the addition of conductive fillers are added, and the production difficulty and cost increase.
The preparation method of polysulfone amide silver nanowire aerogel is adopted to prepare polysulfone amide fibers and silver nanowires by electrospinning, and combined with in-situ hydrolysis-condensation reaction, an aerogel with a directional pore structure is formed to achieve uniform structure stability. and low density electromagnetic shielding materials.
It realizes the easy preparation of polysulfone amide silver nanowire aerogel and the internal pore structure can be adjusted. It has excellent electromagnetic shielding performance, especially for the total electromagnetic shielding effect of 8.2-12.4GHz band ≥80dB, suitable for electromagnetic shielding and antibacterial inhibition. In the fields of bacteria, intelligent sensing and filtration separation.
Smart Images

Figure CN118930954A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aerogels, and particularly relates to a preparation method and application of polysulfoneamide silver nanowire aerogel. Background Art
[0002] The development of modern communication technology has greatly facilitated people's daily lives, but high-energy electromagnetic waves can also pose a major threat to human health, electronic equipment, and national defense security. A large number of studies have shown that long-term exposure to electromagnetic radiation can cause a decline in human immunity, metabolic disorders, memory loss, and even lead to various diseases; electromagnetic pollution also interferes with the normal operation of precision electronic equipment, seriously affecting the accuracy and stability of data and signals. Electronic information warfare is dominating the development of modern warfare, and detection technologies such as radar and satellite communications have become strategic weapons on the modern battlefield. Therefore, the effective prevention and control of electromagnetic radiation is crucial to people's lives, economic production, and national defense construction.
[0003] Among traditional electromagnetic shielding materials, metal-based electromagnetic shielding materials have the disadvantages of high density, difficult processing, and corrosion resistance. Polymer-based electromagnetic shielding materials require the addition of conductive fillers such as carbon nanotubes, graphene, carbon black, and transition metal carbon / nitride (MXene). Although the preparation method is relatively simple and the shielding performance is related to the loading amount of conductive fillers, the increase in filler loading will cause the mechanical properties of the composite material to decrease, while increasing the difficulty and cost of preparation.
[0004] Different from traditional shielding materials, aerogels can absorb incident electromagnetic waves and convert them into heat energy through internal channels due to their porous structure, ultra-lightness, high elasticity and other characteristics, further improving the performance of shielding materials. Current aerogel materials have the defects of uneven structure, high density and low shielding performance. Therefore, the development of electromagnetic shielding materials that meet high shielding performance, uniform and stable structure and low density is becoming more and more popular. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a preparation method and application of polysulfoneamide silver nanowire aerogel. The preparation process is easy to implement, and the internal pore structure of the prepared aerogel is controllable, the structure is uniform and stable, the density is low, and it has excellent electromagnetic shielding performance.
[0006] To this end, the present invention provides a method for preparing polysulfoneamide silver nanowire aerogel, comprising: (1) Preparation of polysulfoneamide fiber: Using a mixed system of N, N-dimethylacetamide and dichloromethane as a solvent, preparing a polysulfoneamide spinning solution; and electrospinning the polysulfoneamide spinning solution to prepare polysulfoneamide fibers; (2) Preparation of silver nanowires: Dissolving silver nitrate particles in ethylene glycol to prepare a silver nitrate solution; dissolving magnesium chloride in ethylene glycol to prepare a magnesium chloride solution; Dissolve polyvinyl pyrrolidone and polyethylene glycol in ethylene glycol respectively, stir and dissolve to obtain a mixed solution, heat the mixed solution to 130-180° C.; dropwise add magnesium chloride solution and silver nitrate solution into the mixed solution in sequence, and keep the mixture warm for reaction; The reaction system after the reaction is cooled to room temperature, and a precipitate is obtained by filtering; acetone is added to the precipitate to precipitate the silver nanowires, the supernatant is removed by centrifugation, the silver nanowire precipitate is repeatedly washed with ethanol, and the silver nanowire is dried to obtain the silver nanowires; (3) Aerogel preparation: Dispersing polysulfoneamide fibers and silver nanowires in a mixed solution system of tert-butyl alcohol and water in sequence to obtain a homogeneous dispersion; Vinyltrimethoxysilane is dissolved in water and then added dropwise into a homogeneous dispersion to carry out an in-situ hydrolysis-condensation reaction. The product of the in-situ hydrolysis-condensation reaction is subjected to directional / non-directional freeze-molding and freeze-drying to obtain a polysulfoneamide silver nanowire aerogel.
[0007] Preferably, in step (1), the volume ratio of N,N-dimethylacetamide to dichloromethane is (3-4):1; the concentration of polysulfoneamide spinning solution is 20%-30%, and the diameter of polysulfoneamide fiber is 100-400nm.
[0008] Preferably, in step (2), the concentration of the silver nitrate solution is 0.01 mol / L-0.5 mol / L, and the concentration of the magnesium chloride solution is 0.01 mol / L-0.5 mol / L.
[0009] Preferably, in step (2), the molecular weight of polyvinyl pyrrolidone is 10,000-100,000, and the molecular weight of polyethylene glycol is 200-7000; The mass ratio of polyvinyl pyrrolidone to polyethylene glycol in the mixed solution is 9.9:0.1-9:1.
[0010] Preferably, in step (2), the silver nitrate solution and the magnesium chloride solution are added at a rate of 0.5 mL / min-10 mL / min, the magnesium chloride solution is added first, and then the silver nitrate solution is added; and the insulation time is 15 min-60 min.
[0011] Preferably, in step (2), the length of the silver nanowires is 0.1 μm-100 μm.
[0012] Preferably, in step (3), the volume ratio of tert-butyl alcohol and water is 4:1, the mass ratio of polysulfoneamide fiber and silver nanowire in the dispersion is 9.9:0.1-5:5, the concentration of vinyltrimethoxysilane solution is 5-100 mg / mL, and the mixing reaction time is 15 min-6 h.
[0013] Preferably, in step (3), the freeze-molding process parameters are: freezing temperature of -50°C to -5°C, freezing time of 15 min to 120 min; freeze-drying process parameters are: freeze-drying machine temperature of -20°C to -50°C, freeze-drying time of 12 h to 72 h, and vacuum degree of 0.5 Pa to 10 Pa.
[0014] Preferably, in step (3), the density of the polysulfoneamide silver nanowire aerogel is 5-100 mg / cm 3 The pore structure of the polysulfonamide silver nanowire aerogel is directional; the total electromagnetic shielding effectiveness of the polysulfonamide silver nanowire aerogel for the frequency band of 8.2-12.4GHz is ≥80dB.
[0015] The present invention also provides applications of the aerogel prepared by the preparation method of the polysulfoneamide silver nanowire aerogel in the fields of electromagnetic shielding, antibacterial and antimicrobial inhibition, intelligent sensing, filtration and separation.
[0016] Compared with the prior art, the advantages and positive effects of the present invention are: the present invention provides a preparation method and application of polysulfoneamide silver nanowire aerogel, the preparation process of the polysulfoneamide silver nanowire aerogel of the present invention is easy to implement, the internal pore structure of the prepared aerogel is controllable, the structure is uniform and stable, the density is low, and it has excellent electromagnetic shielding performance.
[0017] After reading the specific embodiments of the present invention in conjunction with the accompanying drawings, other features and advantages of the present invention will become more clear. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a morphology image of the silver nanowires prepared in Example 1 of the present invention; Figure 2 This is a morphology picture of the polysulfoneamide silver nanowire aerogel prepared in Example 1 of the present invention; Figure 3 This is the electromagnetic shielding data of the polysulfoneamide silver nanowire aerogel prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0019] The present invention will be further described below in conjunction with specific embodiments. These embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. Meanwhile, after reading the present invention, those skilled in the art may make various modifications or changes to the present invention, and these equivalent forms also fall within the scope limited by the appended claims of the application.
[0020] The preparation method of the polysulfoneamide silver nanowire aerogel of the present invention comprises: (1) Preparation of polysulfoneamide fiber: A mixed system of N, N-dimethylacetamide and dichloromethane is used as a solvent to prepare a polysulfoneamide spinning solution, and the polysulfoneamide spinning solution is subjected to electrostatic spinning to prepare polysulfoneamide fibers; The present invention uses a mixed system of N, N-dimethylacetamide and dichloromethane as an electrospinning solvent. N, N-dimethylacetamide has a high boiling point of 153°C. The volatilization rate of the N, N-dimethylacetamide solvent during the fiber forming process is slow, which is not conducive to the rapid forming of the fiber. However, the boiling point of dichloromethane is 40°C, which has a low boiling point, and the volatilization rate of dichloromethane during the fiber forming process is fast. Through the coordinated use of N, N-dimethylacetamide and dichloromethane, there is a difference in the volatilization rate of different solvents during the spinning process, which satisfies the dual functions of the fiber being stretched and refined under the action of the electrostatic field and the fiber forming being stable.
[0021] The volume ratio of N, N-dimethylacetamide and dichloromethane is (3-4):1, which is conducive to fiber spinning and can make the polysulfoneamide fiber quickly form, meeting the requirements of fiber drawing, refinement and stable forming under the action of electrostatic field.
[0022] The concentration of polysulfoneamide spinning solution is 20%-30%, which is conducive to fiber spinning and can make polysulfoneamide fiber quickly form and meet the requirements of fiber drawing, refinement and stable forming under the action of electrostatic field.
[0023] The diameter of polysulfoneamide fiber is 100-400nm, and the fiber diameter is controlled at the nanometer level, which can provide the prerequisite for the realization of ultra-light, low-density and high-porosity aerogel materials prepared subsequently.
[0024] (2) Preparation of silver nanowires: Dissolve silver nitrate particles in ethylene glycol to prepare a silver nitrate solution, the concentration of the silver nitrate solution is 0.01 mol / L-0.5 mol / L; Dissolve magnesium chloride in ethylene glycol to prepare a magnesium chloride solution, wherein the concentration of the magnesium chloride solution is 0.01 mol / L-0.5 mol / L; Dissolve polyvinyl pyrrolidone and polyethylene glycol in ethylene glycol respectively, stir and dissolve to obtain a mixed solution, heat the mixed solution to 130-180° C.; the molecular weight of polyvinyl pyrrolidone is 10,000-100,000, and the molecular weight of polyethylene glycol is 200-7000; the mass ratio of polyvinyl pyrrolidone to polyethylene glycol in the mixed solution is 9.9:0.1-9:1; During the preparation of silver nanowires, polyvinyl pyrrolidone is used as a protective agent for the silver nanowires. During the growth of the silver nanowires, polyvinyl pyrrolidone can prevent the silver nanowires from being oxidized and maintain the purity of the silver nanowires.
[0025] During the preparation of silver nanowires, the main function of polyethylene glycol is to remove moisture from the reaction system, which is beneficial to accelerate the nucleation and growth rate of silver nanowires, increase the yield, and is beneficial to the synthesis of silver nanowires with a high aspect ratio.
[0026] The mass ratio of polyvinyl pyrrolidone to polyethylene glycol in the mixed solution is 9.9:0.1-9:1. The synergistic cooperation of polyvinyl pyrrolidone and polyethylene glycol can effectively prevent the silver nanowires from being oxidized, so that the silver nanowires maintain a high purity; at the same time, it can also be beneficial to the formation and growth of the silver nanowires.
[0027] The molecular weight of polyvinyl pyrrolidone is 10,000-100,000, and the molecular weight of polyethylene glycol is 200-7000, which can help regulate the length and diameter of the silver nanowires, so that the silver nanowires have good uniformity and high dispersion.
[0028] The magnesium chloride solution and the silver nitrate solution are sequentially added dropwise to the mixed solution, and the mixture is kept warm for reaction, and the reaction time is 15min-60min; the silver nitrate solution and the magnesium chloride solution are added dropwise at a speed of 0.5mL / min-10mL / min, and the order of addition requires that the magnesium chloride solution is added dropwise first, and then the silver nitrate solution is added dropwise, which can slowly generate silver particles, reduce the generation of particulate matter, accelerate the generation and length growth of silver nanowires, and improve the aspect ratio of the silver nanowires. The preparation method of the silver nanowires of the present invention has the advantages of simple process, low cost, and the prepared silver nanowires have the advantages of longer wire length, larger aspect ratio and less particulate matter.
[0029] The reaction system after the reaction is cooled to room temperature and filtered to obtain a precipitate; acetone is added to the precipitate to precipitate the silver nanowires, the supernatant is removed by centrifugation, the silver nanowire precipitate is repeatedly washed with ethanol, and the silver nanowire is dried to obtain the silver nanowire, the length of the silver nanowire is 0.1 μm-100 μm.
[0030] (3) Aerogel preparation: Dispersing polysulfoneamide fibers and silver nanowires in a mixed solution system of tert-butyl alcohol and water in sequence to obtain a homogeneous dispersion; Vinyltrimethoxysilane is dissolved in water, and then added dropwise into a homogeneous dispersion to carry out an in-situ hydrolysis-condensation reaction. The product of the in-situ hydrolysis-condensation reaction is subjected to directional freeze molding and freeze drying to obtain a polysulfoneamide silver nanowire aerogel.
[0031] Vinyltrimethoxysilane is first subjected to a hydrolysis reaction in a homogeneous dispersion to generate silanol, and then subjected to a condensation reaction to generate a Si-O-Si cross-linked network, so that cross-linking occurs between fibers to obtain a polysulfoneamide silver nanowire aerogel.
[0032] The volume ratio of tert-butyl alcohol and water is 4:1, which can make the polysulfoneamide fiber and silver nanowires disperse evenly. Homogeneous dispersion.
[0033] The mass ratio of polysulfoneamide fiber to silver nanowire in the dispersion is 9.9:0.1-5:5, which is conducive to forming a conductive network of silver nanowires inside the aerogel and a large number of pore structures inside the aerogel, and is conducive to obtaining an aerogel with excellent electromagnetic shielding performance.
[0034] The concentration of vinyl trimethoxysilane solution is 5-100 mg / mL, and the mixing reaction time is 15min-6h, which is beneficial to vinyl The uniform and rapid in-situ hydrolysis-condensation reaction of trimethoxysilane is beneficial to the formation of a conductive network of silver nanowires inside the aerogel, as well as the formation of a large number of pore structures inside the aerogel, which is beneficial to obtaining an aerogel with excellent electromagnetic shielding performance.
[0035] The conductive network inside the aerogel can isolate and absorb electromagnetic waves, and the pore structure can cause electromagnetic waves to be reflected / refracted multiple times inside the aerogel, converted into energy and absorbed, thus giving the aerogel excellent electromagnetic shielding properties.
[0036] The freeze-molding process parameters are: freezing temperature -50℃ to -5℃, freezing time 15min-120min; the freeze-drying process parameters are: freeze-drying machine temperature -20℃ to -50℃, freeze-drying time 12h-72h, vacuum degree 0.5Pa-10Pa.
[0037] Directed freezing can make the internal pore structure of the prepared aerogel oriented, making the internal structure of the aerogel controllable, uniform and stable, showing high compressive strength in the direction parallel to the layers, and excellent compressive flexibility in the direction perpendicular to the layers, which can make the aerogel density low and is beneficial to improving the electromagnetic shielding performance of the aerogel.
[0038] The density of polysulfoneamide silver nanowire aerogel is 5-100 mg / cm 3 , preferably 10-50 mg / cm 3 The density of aerogel is small, which is conducive to the practical application of aerogel. The pore structure of polysulfonamide silver nanowire aerogel is directional, and the total electromagnetic shielding effectiveness of polysulfonamide silver nanowire aerogel for the frequency band of 8.2-12.4GHz is ≥80dB.
[0039] The preparation process of the polysulfoneamide silver nanowire aerogel of the invention is easy to implement, the internal pore structure of the prepared aerogel is controllable, the structure is uniform and stable, the density is low, and the aerogel has excellent electromagnetic shielding performance.
[0040] The present invention also provides the application of the aerogel prepared by the preparation method of the polysulfoneamide silver nanowire aerogel in the fields of electromagnetic shielding, antibacterial and bacteriostatic, intelligent sensing, filtration and separation. Silver nanowires are a silver ion antibacterial agent with antibacterial and bactericidal effects and a broad spectrum of antibacterial activity, which can kill bacteria and viruses in water and can be applied to functional antibacterial textiles and filter antibacterial. Due to the formation of a silver nanowire conductive network, a network for electrical signal transmission can be formed inside the aerogel, so it can be used in the field of intelligent sensing. The pore structure of the aerogel itself shows great advantages in the field of filtration and separation. Example 1
[0041] (1) Preparation of polysulfoneamide fiber A mixed system of N, N-dimethylacetamide and dichloromethane was used as a solvent with a volume ratio of N, N-dimethylacetamide to dichloromethane of 3.4:1 to prepare a polysulfoneamide spinning solution with a concentration of 25%. The polysulfoneamide spinning solution was electrospun to prepare polysulfoneamide fibers with a diameter of 350±21 nm.
[0042] (2) Preparation of silver nanowires Silver nitrate particles were dissolved in ethylene glycol to prepare a silver nitrate ethylene glycol solution with a concentration of 0.1 mol / L; magnesium chloride was dissolved in ethylene glycol to prepare a magnesium chloride ethylene glycol solution with a concentration of 0.05 mol / L.
[0043] Dissolve polyvinyl pyrrolidone with a molecular weight of 40,000 in ethylene glycol and stir to dissolve; dissolve polyethylene glycol with a molecular weight of 400 in ethylene glycol and stir to dissolve; then blend the polyvinyl pyrrolidone solution and the polyethylene glycol solution according to the mass ratio of solute polyvinyl pyrrolidone to polyethylene glycol of 9.9:0.1. Put the mixed solution into an oil bath and slowly heat it to 160°C, then add magnesium chloride solution and silver nitrate solution to the mixed solution in turn, with a drop rate of 1.5 mL / min, and keep it at 160°C for 30 minutes.
[0044] The mixed solution after the reaction was cooled to room temperature, acetone was added dropwise to precipitate the silver nanowires, the supernatant was removed by centrifugation, the silver nanowire precipitate was repeatedly washed with ethanol, and dried to obtain high-purity silver nanowires. Figure 1 This is a morphology picture of the silver nanowires prepared in Example 1. The average length of the silver nanowires is 21 μm.
[0045] (3) Aerogel preparation 0.1 g of polysulfoneamide fiber and 0.1 g of silver nanowire were dispersed in a solution system of tert-butanol and water in sequence, with a volume ratio of tert-butanol to water of 4:1, to obtain a homogeneous dispersion.
[0046] Vinyltrimethoxysilane was dissolved in water to prepare a solution with a concentration of 60 mg / mL, and then added dropwise to the homogeneous dispersion and mixed for reaction for 2 h.
[0047] The homogeneous dispersion was slowly frozen at -50°C, the freezing time was controlled at 30 minutes, and then placed in a freeze dryer for freeze drying. The parameters of the freeze dryer were set as follows: freezing temperature -20°C, freeze drying time 24 hours, and vacuum degree 0.5 Pa.
[0048] Figure 2 This is a morphology of the polysulfoneamide silver nanowire aerogel prepared in Example 1. The aerogel has a large number of tiny pore structures composed of nanofibers and silver nanowires. The density of the aerogel is measured to be 16.5 mg / cm 3 , the density of aerogel is small.
[0049] Figure 3 This is the electromagnetic shielding data of the polysulfoneamide silver nanowire aerogel prepared in Example 1. The total electromagnetic shielding effectiveness of the aerogel in the frequency band of 8.2-12.4 GHz is 90 dB. Example 2
[0050] (1) Preparation of polysulfoneamide fiber A mixed system of N, N-dimethylacetamide and dichloromethane was used as a solvent with a volume ratio of N, N-dimethylacetamide to dichloromethane of 3.4:1 to prepare a polysulfoneamide spinning solution with a concentration of 20%. The polysulfoneamide spinning solution was electrospun to prepare polysulfoneamide fibers with a diameter of 170±21 μm.
[0051] (2) Preparation of silver nanowires Silver nitrate particles were dissolved in ethylene glycol to prepare a 0.1 mol / L silver nitrate ethylene glycol solution; magnesium chloride was dissolved in ethylene glycol to prepare a 0.05 mol / L magnesium chloride ethylene glycol solution.
[0052] Dissolve polyvinyl pyrrolidone with a molecular weight of 40,000 in ethylene glycol and stir to dissolve; dissolve polyethylene glycol with a molecular weight of 600 in ethylene glycol and stir to dissolve; then blend the polyvinyl pyrrolidone solution and the polyethylene glycol solution according to the mass ratio of solute polyvinyl pyrrolidone to polyethylene glycol of 9.9:0.1. Put the mixed solution into an oil bath and slowly heat it to 160°C, then add magnesium chloride solution and silver nitrate solution to the mixed solution in turn, with a drop rate of 1.5 mL / min, and keep it at 160°C for 30 minutes.
[0053] The mixed solution after the reaction was cooled to room temperature, acetone was added dropwise to precipitate the silver nanowires, the supernatant was removed by centrifugation, the silver nanowire precipitate was repeatedly washed with ethanol, and dried to obtain high-purity silver nanowires. The average size of the nanowires was 21 μm.
[0054] (3) Aerogel preparation 0.7 g of polysulfoneamide fiber and 0.3 g of silver nanowires were dispersed in a solution system of tert-butanol and water in sequence, with a volume ratio of tert-butanol to water of 4:1, to obtain a homogeneous dispersion.
[0055] Vinyltrimethoxysilane was dissolved in water to prepare a solution with a concentration of 60 mg / mL, and then added dropwise to the homogeneous dispersion and mixed for reaction for 2 h.
[0056] The homogeneous dispersion was slowly frozen at -50°C, the freezing time was controlled at 30 min, and then placed in a freeze dryer for freeze drying. The parameters of the freeze dryer were set as follows: freezing temperature -20°C, freeze drying time 24 h, and vacuum degree 0.5 Pa.
[0057] After freeze drying, the density of the aerogel was measured to be 39.5 mg / cm 3 The total electromagnetic shielding effectiveness in the frequency band of 8.2-12.4GHz is 90 dB. Example 3
[0058] (1) Preparation of polysulfoneamide fiber A mixed system of N,N-dimethylacetamide and dichloromethane was used as solvent with a volume ratio of N,N-dimethylacetamide to dichloromethane of 3.4:1 to prepare a polysulfoneamide spinning solution with a concentration of 23%. The polysulfoneamide spinning solution was electrospun to prepare polysulfoneamide fibers with a diameter of 270±21 nm.
[0059] (2) Preparation of silver nanowires Silver nitrate particles were dissolved in ethylene glycol to prepare a 0.3 mol / L silver nitrate ethylene glycol solution; magnesium chloride was dissolved in ethylene glycol to prepare a 0.15 mol / L magnesium chloride ethylene glycol solution.
[0060] Dissolve polyvinyl pyrrolidone with a molecular weight of 100,000 in ethylene glycol and stir to dissolve; dissolve polyethylene glycol with a molecular weight of 600 in ethylene glycol and stir to dissolve; then blend the polyvinyl pyrrolidone solution and the polyethylene glycol solution according to the mass ratio of solute polyvinyl pyrrolidone to polyethylene glycol of 9.9:0.1. Put the mixed solution into an oil bath and slowly heat it to 160°C, then add magnesium chloride solution and silver nitrate solution to the mixed solution in turn, with a drop rate of 1.0 mL / min, and keep it at 160°C for 30 minutes.
[0061] The mixed solution after the reaction was cooled to room temperature, acetone was added dropwise to precipitate the silver nanowires, the supernatant was removed by centrifugation, the silver nanowire precipitate was repeatedly washed with ethanol, and dried to obtain high-purity silver nanowires. The average size of the nanowires was 35 μm.
[0062] (3) Aerogel preparation 0.7 g of polysulfoneamide fiber and 0.3 g of silver nanowire were dispersed in a solution system of tert-butanol and water in sequence, with the volume mixing ratio of tert-butanol and water being 4:1, to obtain a homogeneous dispersion.
[0063] Vinyltrimethoxysilane was dissolved in water to prepare a solution with a concentration of 60 mg / mL, and then added dropwise to the homogeneous dispersion and mixed for reaction for 2 h.
[0064] The homogeneous dispersion was slowly frozen at -50°C, the freezing time was controlled at 30 min, and then placed in a freeze dryer for freeze drying. The parameters of the freeze dryer were set as follows: freezing temperature -20°C, freeze drying time 24 h, and vacuum degree 0.5 Pa.
[0065] After freeze drying, the density of the aerogel was measured to be 27.2 mg / cm 3 The total electromagnetic shielding effectiveness in the frequency band of 8.2-12.4GHz is 90 dB.
[0066] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.
Claims
1. A method for preparing polysulfoneamide silver nanowire aerogel, characterized in that: include (1) Preparation of polysulfoneamide fiber: Using a mixed system of N, N-dimethylacetamide and dichloromethane as a solvent, preparing a polysulfoneamide spinning solution; and electrospinning the polysulfoneamide spinning solution to prepare polysulfoneamide fibers; (2) Preparation of silver nanowires: Silver nitrate solution was prepared by dissolving silver nitrate particles in ethylene glycol; Dissolving magnesium chloride in ethylene glycol to prepare a magnesium chloride solution; Dissolve polyvinyl pyrrolidone and polyethylene glycol in ethylene glycol respectively, stir and dissolve to obtain a mixed solution, and heat the mixed solution to 130-180°C; Adding magnesium chloride solution and silver nitrate solution dropwise to the mixed solution in sequence, and keeping the mixture warm for reaction; The reaction system after the reaction is cooled to room temperature, and a precipitate is obtained by filtering; acetone is added to the precipitate to precipitate the silver nanowires, the supernatant is removed by centrifugation, the silver nanowire precipitate is repeatedly washed with ethanol, and the silver nanowire is dried to obtain the silver nanowires; (3) Aerogel preparation: Dispersing polysulfoneamide fibers and silver nanowires in a mixed solution system of tert-butyl alcohol and water in sequence to obtain a homogeneous dispersion; Vinyltrimethoxysilane is dissolved in water, and then added dropwise into a homogeneous dispersion to carry out an in-situ hydrolysis-condensation reaction; the product of the in-situ hydrolysis-condensation reaction is freeze-formed and freeze-dried to obtain a polysulfoneamide silver nanowire aerogel.
2. The method for preparing polysulfoneamide silver nanowire aerogel according to claim 1, characterized in that: In the step (1), the volume ratio of N,N-dimethylacetamide to dichloromethane is (3-4):1; The concentration of polysulfoneamide spinning solution is 20%-30%, and the diameter of polysulfoneamide fiber is 100-400nm.
3. The method for preparing polysulfoneamide silver nanowire aerogel according to claim 1, characterized in that: In the step (2), the concentration of the silver nitrate solution is 0.01 mol / L-0.5 mol / L, and the concentration of the magnesium chloride solution is 0.01 mol / L-0.5 mol / L.
4. The method for preparing polysulfoneamide silver nanowire aerogel according to claim 1, characterized in that: In step (2), the molecular weight of polyvinyl pyrrolidone is 10,000-100,000, and the molecular weight of polyethylene glycol is 200-7000; The mass ratio of polyvinyl pyrrolidone to polyethylene glycol in the mixed solution is 9.9:0.1-9:
1.
5. The method for preparing polysulfoneamide silver nanowire aerogel according to claim 1, characterized in that: In the step (2), the silver nitrate solution and the magnesium chloride solution are added at a rate of 0.5 mL / min to 10 mL / min, the magnesium chloride solution is added first, and then the silver nitrate solution is added; and the insulation time is 15 min to 60 min.
6. The method for preparing polysulfoneamide silver nanowire aerogel according to claim 1, characterized in that: In the step (2), the length of the silver nanowire is 0.1 μm-100 μm.
7. The method for preparing polysulfoneamide silver nanowire aerogel according to claim 1, characterized in that: In the step (3), tert-butyl alcohol and water are mixed in a volume ratio of 4:
1. The mass ratio of polysulfoneamide fiber to silver nanowire in the dispersion is 9.9:0.1-5:
5. The concentration of vinyltrimethoxysilane solution is 5-100 mg / mL, and the mixing reaction time is 15min-6h.
8. The method for preparing polysulfoneamide silver nanowire aerogel according to claim 1, characterized in that: In step (3), the freezing molding process parameters are: freezing temperature -50°C to -5°C, freezing time 15min-120min; The freeze-drying process parameters are: freeze-drying machine temperature is -20℃ to -50℃, freeze-drying time is 12h-72h, and vacuum degree is 0.5Pa-10Pa.
9. The method for preparing polysulfoneamide silver nanowire aerogel according to claim 1, characterized in that: In step (3), the density of the polysulfoneamide silver nanowire aerogel is 5-100 mg / cm 3 The total electromagnetic shielding effectiveness of polysulfoneamide silver nanowire aerogel in the frequency band of 8.2-12.4GHz is ≥80dB.
10. Application of the aerogel prepared by the method for preparing polysulfoneamide silver nanowire aerogel according to any one of claims 1 to 9 in the fields of electromagnetic shielding, antibacterial and antimicrobial inhibition, intelligent sensing, filtration and separation.
Citation Information
Cited By
Preparation method of environment-friendly electromagnetic wave-absorbing aerogel
CN119978532A