Modified aluminum oxide flame retardant and flame-retardant epoxy resin
Patent Information
- Application Number
- CN202411066591.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-12
AI Technical Summary
The existing flame retardants have environmental pollution problems and inefficiency in epoxy resins, resulting in a decrease in viscosity and mechanical properties of epoxy resins, making it difficult to meet the safety needs in the field of fire proneness.
Modified alumina flame retardant is used to mix strong acid, ethanol and potassium permanganate and react with alumina powder, and further process with amine reagents and coupling agents to form a carboxy and amine-modified alumina flame retardant. , combined with phenolic resin, reduce the amount of addition and improve the flame retardant performance.
The modified alumina flame retardant has good compatibility with epoxy resin, has little influence on mechanical properties, has significantly improved flame retardant performance, has increased oxygen index by 20.4%, the UL-94 grade reaches V0 level, and the carbon residue rate at 800℃ is significantly increased. Environmentally friendly.
Smart Images

Figure CN118930976A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a flame retardant and a flame retardant epoxy resin, in particular to a modified alumina flame retardant and a flame retardant epoxy resin. Background Art
[0002] Epoxy resin is one of the most common thermosetting polymers, with excellent chemical resistance, mechanical and adhesion properties, and is widely used in many engineering fields and in our daily lives. However, epoxy resin is highly flammable, and when burned, it releases a lot of heat and toxic fumes, causing death to humans and animals, thus hindering its practical application in many fields.
[0003] In practical applications, especially in fire-prone fields such as electronic appliances, it is necessary to reduce the fire risk of material parts by improving the flame retardant properties of epoxy resin. However, there are still many problems with the application of flame retardants in the prior art to epoxy resin: first, halogen flame retardants pollute the environment; second, halogen-free flame retardants are not efficient enough and often require a larger addition amount to achieve the same flame retardant level compared to halogen flame retardants, which has a great impact on other properties of epoxy resin, such as increased viscosity and decreased mechanical properties.
[0004] Therefore, it is necessary to further develop new environmentally friendly flame retardant products with high flame retardant efficiency, good compatibility with epoxy resin and excellent comprehensive performance of flame retardant products to meet the development requirements of epoxy resin. In view of this, the present invention is proposed. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a modified alumina flame retardant and a flame retardant epoxy resin. The modified alumina flame retardant provided by the present invention is a halogen-free flame retardant, which is environmentally friendly, and the modified alumina has good flame retardant properties, good compatibility with the epoxy resin matrix, and has little effect on the mechanical properties of the epoxy resin after addition; and after being combined with the phenolic resin, the flame retardant property is better, and the amount of flame retardant added is less.
[0006] The technical solution of the present invention:
[0007] A modified alumina flame retardant is prepared by the following method:
[0008] Step 1: Mix strong acid, ethanol and potassium permanganate to obtain a modified solution;
[0009] Step 2: adding alumina powder to the modified solution for reaction;
[0010] Step 3: filtering the reaction product of step 2, washing and drying the solid matter to obtain carboxyl-modified alumina;
[0011] Step 4: adding carboxyl-modified alumina to a mixed solution of an amine reagent and a coupling agent to react;
[0012] Step 5: Filter the reaction product of step 4, wash and dry the solid matter to obtain a carboxyl- and amine-modified alumina flame retardant.
[0013] Preferably, in the aforementioned modified alumina flame retardant, the strong acid in step 1 is a mixed acid of sulfuric acid and nitric acid, wherein the volume ratio of sulfuric acid to nitric acid is 3:0.5-3:1.5.
[0014] Preferably, in the aforementioned modified alumina flame retardant, the mixing volume ratio of the strong acid, ethanol and potassium permanganate in step 1 is 5:3-5:5-7.
[0015] Preferably, for the aforementioned modified alumina flame retardant, the reaction time of step 2 is 0.5h-1h, and the solid-liquid ratio of alumina powder and modified solution is 1kg:4-6L.
[0016] Preferably, in the aforementioned modified alumina flame retardant, the mixing mass ratio of the carboxyl-modified alumina, the amine reagent and the coupling agent in step 4 is 1:0.3-0.7:0.3-0.7.
[0017] Preferably, in the aforementioned modified alumina flame retardant, the amine reagent is one or any combination of ethylenediamine, propylenediamine or aminopyridine.
[0018] Preferably, in the aforementioned modified alumina flame retardant, the coupling agent is one or more of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a metal composite coupling agent, a phosphate coupling agent or a borate coupling agent.
[0019] A flame retardant epoxy resin comprising the modified alumina flame retardant according to any one of claims 1 to 7.
[0020] Preferably, the aforementioned flame retardant epoxy resin comprises, by weight, 100 parts of epoxy resin, 5-20 parts of phenolic resin, 0.4-5 parts of modified alumina flame retardant and 10-25 parts of curing agent.
[0021] Preferably, the aforementioned flame retardant epoxy resin is prepared by the following method: epoxy resin, phenolic resin, modified alumina flame retardant and curing agent are mixed and ultrasonically vibrated at 50-70°C for 20-40 minutes, then kept warm and stirred for 0.5-1.5 hours, and then poured into a mold while hot, and kept warm at 70-90°C for 0.5-1.5 hours and 90-110°C for 1-3 hours, respectively, to obtain a flame retardant epoxy resin.
[0022] Beneficial effects of the present invention:
[0023] 1. The modified alumina of the present invention is modified by carboxyl and amine groups, which, on the one hand, improves the compatibility with the epoxy resin matrix and reduces the influence of alumina on the mechanical properties of the epoxy resin, and on the other hand, improves the flame retardant properties of alumina.
[0024] 2. The modified alumina flame retardant of the present invention is a halogen-free flame retardant, is environmentally friendly, and is suitable for wide promotion and application.
[0025] 3. After the modified alumina flame retardant of the present invention is used in combination with phenolic resin, the required addition amount is very small, and the flame retardant performance is good, and the mechanical properties of the epoxy resin are excellent. Experiments have shown that the epoxy resin of the present invention has an oxygen index of up to 29.5 when the flame retardant content is low, which is 20.4% higher than that of pure epoxy resin, and the UL-94 grade is V0. The residual carbon rate at 800°C is up to 25.75, which is 193.94% higher than that of pure epoxy resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Attached Figure 1 This is a SEM image of the carbon layer of the flame retardant epoxy resin prepared in Example 3 of the present invention;
[0027] Attached Figure 2 This is a SEM image of the carbon layer of the flame retardant epoxy resin obtained in Comparative Example 1 of the present invention.
[0028] Figure 1 and Figure 2 This is the corresponding carbon layer after the epoxy resin is burned. Figure 1 and Figure 2 It can be seen that Figure 1 The carbon layer of the modified epoxy resin has better density after combustion, indicating that a better flame retardant modification effect has been achieved. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.
[0030] Embodiments of the present invention
[0031] The epoxy resin used in the following examples of the present invention is E51 epoxy resin, and the viscosity at room temperature is 11000-14000 mPa·s.
[0032] The phenolic resin used in the following examples of the present invention is a common phenolic resin having a viscosity of 25000-30000 mPa·s at room temperature.
[0033] Example 1
[0034] This embodiment is a flame retardant modified epoxy resin, which is prepared from the following raw materials in parts by weight:
[0035] 100 parts of epoxy resin, 0.4 parts of modified alumina powder, 10 parts of phenolic resin, and 25 parts of curing agent.
[0036] The preparation method of the flame retardant modified epoxy resin comprises the following steps:
[0037] (a) Preparation of modified alumina powder: Weigh alumina powder and place it in a strong acid (H 2 SO 4 :HNO 3 =3:1), a mixed solution of strong acid, ethanol and potassium permanganate, wherein the mixed volume ratio of strong acid, ethanol and potassium permanganate is 5:4:6, and the solid-liquid ratio of alumina powder and solution is 1kg:5L, and ultrasonic treatment is performed at room temperature for 45min, and finally the alumina powder is washed several times with anhydrous ethanol and deionized water, and dried to constant weight, thereby obtaining an alumina powder grafted with carboxyl groups; the alumina powder with carboxyl groups is ultrasonically dispersed in a propylene diamine reagent and a silane coupling agent, wherein the mass ratio of the alumina powder, the propylene diamine reagent and the silane coupling agent is 1:0.5:0.5, and then washed several times with anhydrous ethanol and deionized water, and dried to constant weight, thereby obtaining a modified alumina powder grafted with amino groups and carboxyl groups.
[0038] (b) Modified alumina powder, phenolic resin and epoxy resin are weighed in proportion, mixed and ultrasonically shaken at 60° C. for 30 min, and then stirred at 60° C. for 1 h to obtain a flame retardant modified epoxy resin.
[0039] (c) Pour the modified epoxy resin and the curing agent in the stated proportion into a mold while hot, and heat and cure at 80° C. / 1 h and 100° C. / 2 h.
[0040] The prepared flame retardant modified epoxy resin has an oxygen index of 28.2, a flame retardant grade of V1, and a carbon residue rate of 19.1 at 800°C.
[0041] Example 2
[0042] This embodiment is a flame retardant modified epoxy resin, which is prepared from the following raw materials in parts by weight:
[0043] 100 parts of epoxy resin, 0.6 parts of modified alumina powder, 10 parts of phenolic resin, and 25 parts of curing agent.
[0044] The preparation method of the flame retardant modified epoxy resin comprises the following steps:
[0045] (a) Preparation of modified alumina powder: Weigh alumina powder and place it in a strong acid (H 2 SO 4 :HNO 3=3:0.5), a mixed solution of ethanol and potassium permanganate, wherein the mixed volume ratio of strong acid, ethanol and potassium permanganate is 5:3:5, and the solid-liquid ratio of alumina powder and the solution is 1kg:4L, and ultrasonic treatment is performed at room temperature for 30min, and finally the alumina powder is washed with anhydrous ethanol and deionized water for several times, and dried to constant weight, thereby obtaining an alumina powder grafted with carboxyl groups; the alumina powder with carboxyl groups is ultrasonically dispersed in ethylenediamine reagent and titanate coupling agent, wherein the mass ratio of alumina powder, ethylenediamine reagent and titanate coupling agent is 1:0.3:0.3, and then washed with anhydrous ethanol and deionized water for several times, and dried to constant weight, thereby obtaining a modified alumina powder grafted with amino groups and carboxyl groups.
[0046] (b) Modified alumina powder, phenolic resin and epoxy resin are weighed in proportion, mixed and ultrasonically shaken at 50° C. for 40 min, and then stirred at 50° C. for 1.5 h to obtain a flame retardant modified epoxy resin.
[0047] (c) Pour the modified epoxy resin and the curing agent in the stated proportion into a mold while hot, and heat and cure at 70°C / 1.5h and 90°C / 3h.
[0048] The prepared flame retardant modified epoxy resin has an oxygen index of 28.9, a flame retardant grade of V1, and a carbon residue rate of 22.26 at 800°C.
[0049] Example 3
[0050] This embodiment is a flame retardant modified epoxy resin, which is prepared from the following raw materials in parts by weight:
[0051] 100 parts of epoxy resin, 0.8 parts of modified alumina powder, 10 parts of phenolic resin, and 25 parts of curing agent.
[0052] The preparation method of the flame retardant modified epoxy resin comprises the following steps:
[0053] (a) Preparation of modified alumina powder: Weigh alumina powder and place it in a strong acid (H 2 SO 4 :HNO 3=3:1), a mixed solution of strong acid, ethanol and potassium permanganate, wherein the mixed volume ratio of strong acid, ethanol and potassium permanganate is 5:4:6, and the solid-liquid ratio of alumina powder and solution is 1kg:5L, and ultrasonic treatment is carried out at room temperature for 45min, and finally the alumina powder is washed several times with anhydrous ethanol and deionized water, and dried to constant weight, thereby obtaining an alumina powder grafted with carboxyl groups; the alumina powder with carboxyl groups is ultrasonically dispersed in ethylenediamine reagent and silane coupling agent, wherein the mass ratio of alumina powder, ethylenediamine reagent and silane coupling agent is 1:0.5:0.5, and then washed several times with anhydrous ethanol and deionized water, and dried to constant weight, thereby obtaining a modified alumina powder grafted with amino groups and carboxyl groups.
[0054] (b) Modified alumina powder, phenolic resin and epoxy resin are weighed in proportion, mixed and ultrasonically shaken at 60° C. for 30 min, and then stirred at 60° C. for 1 h to obtain a flame retardant modified epoxy resin.
[0055] (c) Pour the modified epoxy resin and the curing agent in the stated proportion into a mold while hot, and heat and cure at 80° C. / 1 h and 100° C. / 2 h.
[0056] The prepared flame retardant modified epoxy resin has an oxygen index of 29.5, a flame retardant grade of V0, and a carbon residue rate of 25.75 at 800°C.
[0057] Example 4
[0058] This embodiment is a flame retardant modified epoxy resin, which is prepared from the following raw materials in parts by weight:
[0059] 100 parts of epoxy resin, 1.0 parts of modified alumina powder, 10 parts of phenolic resin, and 25 parts of curing agent.
[0060] The preparation method of the flame retardant modified epoxy resin comprises the following steps:
[0061] (a) Preparation of modified alumina powder: Weigh alumina powder and place it in a strong acid (H 2 SO 4 :HNO 3=3:1), a mixed solution of strong acid, ethanol and potassium permanganate, wherein the mixed volume ratio of strong acid, ethanol and potassium permanganate is 5:5:7, and the solid-liquid ratio of alumina powder and solution is 1kg:6L, and ultrasonic treatment is performed at room temperature for 60min, and finally the alumina powder is washed several times with anhydrous ethanol and deionized water, and dried to constant weight, thereby obtaining an alumina powder grafted with carboxyl groups; the alumina powder with carboxyl groups is ultrasonically dispersed in aminopyridine and a phosphate coupling agent, wherein the mass ratio of the alumina powder, aminopyridine and the phosphate coupling agent is 1:0.7:0.7, and then washed several times with anhydrous ethanol and deionized water, and dried to constant weight, thereby obtaining a modified alumina powder grafted with amino and carboxyl groups.
[0062] (b) Modified alumina powder, phenolic resin and epoxy resin are weighed in proportion, mixed and ultrasonically shaken at 70° C. for 20 min, and then stirred at 70° C. for 0.5 h to obtain a flame retardant modified epoxy resin.
[0063] (c) Pour the modified epoxy resin and the curing agent in the stated proportion into a mold while hot, and heat and cure at 90° C. / 0.5 h and 110° C. / 1 h.
[0064] The prepared flame retardant modified epoxy resin has an oxygen index of 29.3, a flame retardant grade of V0, and a carbon residue rate of 24.36 at 800°C.
[0065] Example 5
[0066] This embodiment is a flame retardant modified epoxy resin, which is prepared from the following raw materials in parts by weight:
[0067] 100 parts of epoxy resin, 5 parts of modified alumina powder, 20 parts of phenolic resin, and 10 parts of curing agent.
[0068] The preparation method of the flame retardant modified epoxy resin comprises the following steps:
[0069] (a) Preparation of modified alumina powder: Weigh alumina powder and place it in a strong acid (H 2 SO 4 :HNO 3=3:1.5), a mixed solution of ethanol and potassium permanganate, wherein the mixed volume ratio of strong acid, ethanol and potassium permanganate is 5:5:7, and the solid-liquid ratio of alumina powder and solution is 1kg:6L, and ultrasonic treatment is carried out at room temperature for 50min, and finally the alumina powder is washed several times with anhydrous ethanol and deionized water, and dried to constant weight, thereby obtaining an alumina powder grafted with carboxyl groups; the alumina powder with carboxyl groups is ultrasonically dispersed in an aluminate coupling agent reagent and a silane coupling agent, wherein the mass ratio of the alumina powder, the aluminate coupling agent reagent and the silane coupling agent is 1:0.6:0.6, and then washed several times with anhydrous ethanol and deionized water, and dried to constant weight, thereby obtaining a modified alumina powder grafted with amino groups and carboxyl groups.
[0070] (b) Modified alumina powder, phenolic resin and epoxy resin are weighed in proportion, mixed and ultrasonically shaken at 60° C. for 30 min, and then stirred at 60° C. for 1 h to obtain a flame retardant modified epoxy resin.
[0071] (c) Pour the modified epoxy resin and the curing agent in the stated proportion into a mold while hot, and heat and cure at 80° C. / 1 h and 100° C. / 2 h.
[0072] The prepared flame retardant modified epoxy resin has an oxygen index of 29.2, a flame retardant grade of V0, and a carbon residue rate of 23.37 at 800°C.
[0073] Comparative Example 1
[0074] This comparative example is a flame retardant modified epoxy resin, which is prepared from the following raw materials in parts by weight:
[0075] 100 parts of epoxy resin and 25 parts of curing agent.
[0076] The preparation method comprises the following steps:
[0077] Pour 100 parts of epoxy resin and 25 parts of curing agent into the mold while hot, and heat to cure at 80°C / 1h and 100°C / 2h.
[0078] The prepared flame retardant modified epoxy resin has an oxygen index of 24.5, no flame retardant grade, and a carbon residue rate of 8.76 at 800°C.
[0079] Comparative Example 2
[0080] This comparative example is a flame retardant modified epoxy resin, which is prepared from the following raw materials in parts by weight:
[0081] 100 parts of epoxy resin, 10 parts of phenolic resin, and 25 parts of curing agent.
[0082] The preparation method comprises the following steps:
[0083] Pour 100 parts of epoxy resin, 10 parts of phenolic resin and 25 parts of curing agent into the mold while hot, and heat and cure at 80°C / 1h and 100°C / 2h.
[0084] The prepared flame retardant modified epoxy resin has an oxygen index of 26.4, no flame retardant grade, and a carbon residue rate of 15.16 at 800°C.
[0085] Comparative Example 3
[0086] 100 parts of epoxy resin, 0.8 parts of alumina powder, 10 parts of phenolic resin, and 25 parts of curing agent.
[0087] The preparation method of the flame retardant modified epoxy resin comprises the following steps:
[0088] (a) Weigh alumina powder, phenolic resin and epoxy resin, mix them, and ultrasonically vibrate them at 60° C. for 30 min. After the vibration, stir them at 60° C. for 1 h to obtain a flame-retardant modified epoxy resin.
[0089] (b) Pour the modified epoxy resin and curing agent into the mold while hot, and heat and cure at 80°C / 1h and 100°C / 2h.
[0090] The prepared flame retardant modified epoxy resin has an oxygen index of 26.8, a flame retardant grade of V1, and a carbon residue rate of 16.5 at 800°C.
[0091] The flame retardant properties of the epoxy resins obtained in the above Examples 1-5 and Comparative Examples 1-3 are shown in Table 1.
[0092] Table 1 Flame retardant properties of epoxy resin
[0093]
[0094]
[0095] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A modified alumina flame retardant, characterized in that: Prepared by the following method: Step 1: Mix strong acid, ethanol and potassium permanganate to obtain a modified solution; Step 2: adding alumina powder to the modified solution for reaction; Step 3: filtering the reaction product of step 2, washing and drying the solid matter to obtain carboxyl-modified alumina; Step 4: adding carboxyl-modified alumina to a mixed solution of an amine reagent and a coupling agent to react; Step 5: Filter the reaction product of step 4, wash and dry the solid matter to obtain a carboxyl- and amine-modified alumina flame retardant.
2. The modified alumina flame retardant according to claim 1, characterized in that: The strong acid in step 1 is a mixed acid of sulfuric acid and nitric acid, wherein the volume ratio of sulfuric acid to nitric acid is 3:0.5-1.
5.
3. The modified alumina flame retardant according to claim 1, characterized in that: The mixing volume ratio of the strong acid, ethanol and potassium permanganate in step 1 is 5:3-5:5-7.
4. The modified alumina flame retardant according to claim 1, characterized in that: The reaction time of step 2 is 0.5h-1h, and the solid-liquid ratio of alumina powder to modified solution is 1kg:4-6L.
5. The modified alumina flame retardant according to claim 1, characterized in that: In step 4, the mixing mass ratio of the carboxyl-modified alumina, the amine reagent and the coupling agent is 1:0.3-0.7:0.3-0.
7.
6. The modified alumina flame retardant according to claim 1, characterized in that: The amine reagent is one or more of ethylenediamine, propylenediamine or aminopyridine.
7. The modified alumina flame retardant according to claim 1, characterized in that: The coupling agent is one or more of a silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a metal composite coupling agent, a phosphate coupling agent or a borate coupling agent.
8. A flame retardant epoxy resin, characterized in that: The modified alumina flame retardant comprises the modified alumina flame retardant according to any one of claims 1 to 7.
9. The flame retardant epoxy resin according to claim 8, characterized in that: Calculated by weight, it comprises 100 parts of epoxy resin, 5-20 parts of phenolic resin, 0.4-5 parts of modified alumina flame retardant and 10-25 parts of curing agent.
10. The flame retardant epoxy resin according to claim 9, characterized in that: The preparation method is as follows: epoxy resin, phenolic resin and modified alumina flame retardant are mixed and ultrasonically vibrated at 50-70°C for 20-40 minutes, then kept warm and stirred for 0.5-1.5 hours, and then poured into a mold together with a curing agent while hot, and kept warm at 70-90°C for 0.5-1.5 hours and 90-110°C for 1-3 hours, respectively, to obtain a flame retardant epoxy resin.
Citation Information
Cited By
Functionalized aluminum oxide as well as preparation method and application thereof
CN120699327A