Cerium oxide loaded white carbon black filler as well as preparation method and application thereof

Through the use of cerium oxide-laden white carbon black filler, the combination of nano cerium oxide modified with polymer dopamine-modified bio-based white carbon black is solved by the use of cerium oxide-laden white carbon filler and organic material in natural rubber composite materials. The problem of poor performance significantly improves the anti-aging and comprehensive properties of the material.

CN118930980APending Publication Date: 2024-11-12SINO TRUK JINAN POWER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411000139.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The poor compatibility of natural rubber composite materials with inorganic fillers and organic materials leads to insufficient aging resistance and are easily damaged under external forces.

Method used

Using cerium oxide-loaded white carbon black filler, the combination of nano cerium oxide modified with titanate coupling agent and polymerized dopamine-modified bio-based white carbon black is enhanced to enhance the dispersion and binding force of the filler in the rubber matrix, and nano-oxidation is used. The scavenger radical removal ability of cerium slows down the rubber aging reaction.

Benefits of technology

It effectively improves the dispersion of fillers and the anti-aging properties of rubber composite materials, and improves the comprehensive performance and aging resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of rubber materials, in particular to a cerium oxide loaded white carbon black filler as well as a preparation method and application thereof. The cerium oxide loaded white carbon black filler comprises the following raw materials: bio-based white carbon black, nano cerium oxide, dopamine hydrochloride and a titanate coupling agent, the bio-based white carbon black is organically modified by utilizing polydopamine, and then the titanate coupling agent is connected with cerium oxide to form a composite filler; the dispersity of the filler in a rubber matrix can be effectively improved, the binding force of rubber molecules and inorganic filler can be enhanced, and the comprehensive performance of a rubber composite material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber materials, and in particular to a cerium oxide-loaded white carbon black filler and a preparation method and application thereof. Background Art

[0002] Natural rubber (NR) is a natural polymer compound with cis-1,4-polyisoprene as the main component, and 91% to 94% of its components are rubber hydrocarbons (cis-1,4-polyisoprene). Natural rubber has good elasticity and physical and mechanical strength, and is the most commonly used raw material in the rubber products industry. However, natural rubber itself has weak resistance to the external environment and extreme conditions, and is prone to aging, which seriously affects the service life of natural rubber products. Therefore, it is particularly important to improve the anti-aging performance of natural rubber products.

[0003] The aging reaction of rubber is essentially due to the breakage of molecular chains caused by external energy stimulation (light, heat, etc.) and the movement of the rubber's own molecular chains, forming free radicals. The free radicals further attack the molecular chain segments, causing the continued occurrence of the aging reaction.

[0004] Cerium oxide is a commonly used anti-aging inorganic filler in the rubber industry, and white carbon black is a commonly used reinforcing inorganic filler in the rubber industry. However, in the preparation process of inorganic / organic composite materials, due to the poor compatibility between inorganic and organic materials, the performance of the composite materials is often not ideal and the advantages of the composite materials cannot be fully utilized. When the particle size of the inorganic powder is small, it is very easy to agglomerate in the organic matrix, forming more stress concentration points in the composite material. When the composite material is subjected to external force, these stress concentration points become the triggering area for material damage, causing the performance of the composite material to decline. Summary of the invention

[0005] In view of the technical problems such as poor compatibility between inorganic fillers and organic materials affecting the aging resistance of rubber composites during the preparation of natural rubber composites, the present invention provides a cerium oxide-loaded white carbon black filler and a preparation method and application thereof, which can effectively improve the dispersibility of the inorganic filler in the rubber matrix, enhance the bonding force between rubber molecules and the inorganic filler, and help to improve the aging resistance and other properties of the rubber composite.

[0006] In a first aspect, the present invention provides a cerium oxide-loaded white carbon black filler, comprising the following raw materials: bio-based white carbon black, nano-cerium oxide, dopamine hydrochloride, and a titanate coupling agent.

[0007] Furthermore, the preparation method of bio-based silica comprises the following steps: (1) taking bio-based raw materials, removing impurities, pre-treating, calcining, and grinding to obtain bio-based powder; (2) The bio-based powder is added to the alkali solution, stirred for reaction, and then filtered to collect the filtrate, which contains sodium silicate; (3) Add ammonium chloride solution to the filtrate, stir the reaction until the precipitation no longer increases, take the lower layer of precipitation and spray dry it to obtain bio-based silica.

[0008] Furthermore, in step (1), the impurity removal pretreatment of the bio-based raw material includes drying the bio-based raw material and then heating it to boiling with dilute hydrochloric acid to remove impurities; the calcination temperature is 600° C. and the calcination time is 2 hours.

[0009] Furthermore, in step (2), the bio-based powder is the biomass ash remaining after biomass power plants burn biomass fuels to generate electricity or the ash remaining after the incineration of silicon-containing crops. Silicon-containing crops can be obtained from rice husks, straws, etc. The raw material source is wide and pollution-free. At the same time, the resources can be reused, which is environmentally friendly.

[0010] Furthermore, in step (2), the alkali solution is sodium hydroxide solution, the reaction temperature is 60° C., and the reaction time is 1 h.

[0011] Furthermore, the titanate coupling agent is a chelate solution of bis(dioctyloxypyrophosphate)ethylene titanate and triethanolamine. The coupling agent has a good coupling effect in the rubber system and is suitable for coupling inorganic fillers such as silica with organic molecules such as rubber and polydopamine.

[0012] In a second aspect, the present invention provides a method for preparing a cerium oxide-loaded white carbon black filler, comprising the following steps: (1) preparing an ethanol aqueous solution, adding glacial acetic acid to adjust the pH value of the system to 3.5, adding a titanate coupling agent and stirring, then adding nano-cerium oxide powder, stirring at 60°C for 2 hours, centrifuging, washing, and spray drying to obtain modified nano-cerium oxide; (2) Adding bio-based silica into water and stirring, ultrasonic treatment to obtain a bio-based silica dispersion, adding dopamine hydrochloride and tris(hydroxymethyl)aminomethane to the biomass silica dispersion under stirring conditions, controlling the pH value of the system to 8.5-9.0, and stirring the reaction; (3) Adding the modified nano-cerium oxide prepared in step (1) to the reaction product of step (2), continuing the reaction for 1 hour, centrifuging to obtain a precipitate, washing, and spray drying to obtain a cerium oxide-loaded white carbon black filler.

[0013] Furthermore, the mass ratio of titanate coupling agent, nano-cerium oxide, bio-based white carbon black, and dopamine hydrochloride is 10:10:10:1.5.

[0014] In a third aspect, the present invention provides an application of a cerium oxide-loaded white carbon black filler in the preparation of a natural rubber composite material.

[0015] Furthermore, the natural rubber composite material includes the following raw materials in parts by weight: 100 parts of natural rubber, 5 to 8 parts of zinc oxide, 2 to 4 parts of stearic acid, 2 to 10 parts of cerium oxide-loaded white carbon black filler, 30 to 60 parts of carbon black N550, 3 to 5 parts of paraffin oil, 1 to 2 parts of sulfur, and 1.5 to 2.5 parts of N-tert-butyl-2-benzothiazole sulfenamide.

[0016] The principle of the present invention is as follows: the present invention firstly utilizes a titanate coupling agent to modify nano cerium oxide to obtain nano cerium oxide modified by a titanate coupling agent; then utilizes the self-polymerization of dopamine hydrochloride under alkaline conditions (trishydroxymethylaminomethane provides alkaline conditions) to generate polymerized dopamine coated on the surface of bio-based silica to obtain polymerized dopamine-modified bio-based silica; finally, the nano cerium oxide modified by a titanate coupling agent is combined with the bio-based silica modified by polymerized dopamine, and a cerium oxide-loaded silica filler is prepared by connection using a titanate coupling agent, thereby enhancing the dispersibility of the filler in the rubber matrix and the bonding force between the rubber matrix and the filler, thereby improving the anti-aging performance of the rubber composite material.

[0017] The beneficial effects of the present invention are: (1) The present invention uses polydopamine to organically modify bio-based silica, and then uses a titanate coupling agent to connect it with cerium oxide to form a composite filler, which can effectively improve the dispersibility of the filler in the rubber matrix, enhance the bonding force between rubber molecules and inorganic fillers, and help improve the comprehensive performance of the rubber composite material.

[0018] (2) The cerium oxide-loaded white carbon black filler provided by the present invention can remove free radicals generated in the rubber aging reaction by utilizing the free radical scavenging ability of nano-cerium oxide, thereby slowing down the reaction process of rubber aging and improving the anti-aging performance of the rubber composite material.

[0019] (3) In the present invention, bio-based silica is prepared. The raw material of the bio-based silica can be the residual ash after the combustion of biomass materials such as rice husks and straws, or the biomass ash generated after these biomass materials are used as energy, which is helpful for the utilization of resources and reducing waste. At the same time, due to the high organic matter content in the bio-based raw materials, a small amount of active functional groups still remain on the surface of the prepared bio-based silica, which is beneficial to the dispersion of the bio-based silica in the rubber matrix and the formation of a binding rubber, and has a promoting effect on the rubber performance. DETAILED DESCRIPTION

[0020] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0021] The bio-based silica preparation method used in the following examples includes: (1) Take 50 g of bio-based raw material (residual ash after burning rice husk), wash and dry it, add 1 L of 5% dilute hydrochloric acid, heat to boiling and stir for 30 min to remove impurities, place the treated bio-based raw material in a muffle furnace, calcine it at 600 °C for 2 h, and grind and sieve the obtained product for later use.

[0022] (2) Add 100 ml of 10% by mass sodium hydroxide solution to the product of step (1), stir at 60° C. for 1 hour, and then filter and collect the filtrate, which contains sodium silicate.

[0023] (3) Gradually add 10% by mass ammonium chloride solution to the obtained filtrate, stir the reaction until the precipitation no longer increases, then centrifuge, take out the lower layer of precipitate and spray dry it to obtain high-quality bio-based silica.

[0024] The preparation method of the cerium oxide-loaded white carbon black filler used in the following example comprises the following steps: (1) Prepare 1 L of 50% ethanol aqueous solution, add glacial acetic acid to adjust the pH value to 3.5, add 1 g of titanate coupling agent and stir, then add 10 g of nano cerium oxide powder, stir at 60 ° C for 2 h, centrifuge and wash with deionized water, and finally spray dry to obtain titanate coupling agent modified cerium oxide.

[0025] (2) First, 10 g of bio-based silica was added to 1 L of deionized water and stirred. Then, the bio-based silica was dispersed using ultrasound for 1 h to obtain bio-based silica. 1.5 g of dopamine hydrochloride and 1 g of tris(hydroxymethyl)aminomethane were added to the silica dispersion under stirring. The pH value of the solution was adjusted to 8.5-9.0. The solution was stirred at room temperature for 6 h to react.

[0026] (3) After the polydopamine generated by self-polymerization in step (2) is fully coated on the surface of the bio-based silica, 10 g of the cerium oxide powder modified with the titanate coupling agent obtained in step (1) is added to the reaction solution. After reacting for 1 hour, the resulting reaction solution is centrifuged to obtain a precipitate. The precipitate is repeatedly washed with deionized water and ethanol for 3 times, and the resulting product is spray-dried to obtain a cerium oxide-loaded silica filler.

[0027] Example 1 A natural rubber composite material comprises the following raw materials in parts by weight: 100 parts of natural rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 2 parts of cerium oxide-loaded white carbon filler, 50 parts of carbon black N550, 3 parts of paraffin oil, 1 part of sulfur, and 1.5 parts of N-tert-butyl-2-benzothiazole sulfenamide. The above raw materials are mixed evenly on an open mill and then vulcanized at 150° C. according to a positive vulcanization time using a flat vulcanizer to obtain a natural rubber composite material.

[0028] Example 2 A natural rubber composite material includes the following raw materials in parts by weight: 100 parts of natural rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 5 parts of cerium oxide-loaded white carbon black filler, 50 parts of carbon black N550, 3 parts of paraffin oil, 1 part of sulfur, and 1.5 parts of N-tert-butyl-2-benzothiazole sulfenamide. Example 2 The preparation method of the natural rubber composite material is the same as that of Example 1.

[0029] Example 3 A natural rubber composite material includes the following raw materials in parts by weight: 100 parts of natural rubber, 5 parts of zinc oxide, 2 parts of stearic acid, 8 parts of cerium oxide-loaded white carbon filler, 60 parts of carbon black N550, 3 parts of paraffin oil, 1 part of sulfur, and 1.5 parts of N-tert-butyl-2-benzothiazole sulfenamide. Example 3 The preparation method of the natural rubber composite material is the same as that of Example 1.

[0030] Example 4 A natural rubber composite material includes the following raw materials in parts by weight: 100 parts of natural rubber, 6 parts of zinc oxide, 3 parts of stearic acid, 10 parts of cerium oxide-loaded white carbon filler, 50 parts of carbon black N550, 3 parts of paraffin oil, 1 part of sulfur, and 1.5 parts of N-tert-butyl-2-benzothiazole sulfenamide. Example 4 The preparation method of the natural rubber composite material is the same as that of Example 1.

[0031] Example 5 A natural rubber composite material includes the following raw materials in parts by weight: 100 parts of natural rubber, 8 parts of zinc oxide, 4 parts of stearic acid, 5 parts of cerium oxide-loaded white carbon filler, 30 parts of carbon black N550, 5 parts of paraffin oil, 2 parts of sulfur, and 2.5 parts of N-tert-butyl-2-benzothiazole sulfenamide. Example 5 The preparation method of the natural rubber composite material is the same as that of Example 1.

[0032] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the cerium oxide-loaded white carbon black filler in the raw material is replaced by cerium oxide.

[0033] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the raw material does not contain cerium oxide-loaded white carbon black filler.

[0034] The properties of the natural rubber composite materials prepared in the examples and comparative examples were tested, including tensile properties test (GB / T 528-2009) and ozone aging resistance test (GB / T 7762-2014). Specific performance test results are shown in Table 1.

[0035] Table 1 Performance test data of natural rubber composite materials obtained in various embodiments and comparative examples

[0036] Although the present invention has been described in detail by way of preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and such modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily conceive of changes or substitutions within the technical scope disclosed by the present invention, and such changes or substitutions shall be within the scope of protection of the present invention.

Claims

1. A cerium oxide-loaded white carbon black filler, characterized in that: The invention comprises the following raw materials: bio-based white carbon black, nano-cerium oxide, dopamine hydrochloride and titanate coupling agent.

2. The cerium oxide-loaded white carbon black filler according to claim 1, characterized in that: The preparation method of bio-based silica comprises the following steps: (1) taking bio-based raw materials, removing impurities, pre-treating, calcining, and grinding to obtain bio-based powder; (2) Adding the bio-based powder into the alkali solution, stirring the reaction, and then filtering to collect the filtrate; (3) Add ammonium chloride solution to the filtrate, stir the reaction until the precipitation no longer increases, take the lower layer of precipitation and spray dry it to obtain bio-based silica.

3. A cerium oxide-loaded white carbon black filler as claimed in claim 2, characterized in that: In step (1), the pretreatment of the bio-based raw material for removing impurities includes drying the bio-based raw material and then heating it to boiling with dilute hydrochloric acid to remove impurities; the calcination temperature is 600° C. and the calcination time is 2 hours.

4. A cerium oxide-loaded white carbon black filler as claimed in claim 2, characterized in that: In step (2), the bio-based powder is the biomass ash remaining after biomass fuel is burned in a biomass power plant to generate electricity, or the ash remaining after silicon-containing crops are burned.

5. The cerium oxide-loaded white carbon black filler according to claim 2, characterized in that: In step (2), the alkali solution is sodium hydroxide solution, the reaction temperature is 60° C., and the reaction time is 1 h.

6. The cerium oxide-loaded white carbon black filler according to claim 1, characterized in that: The titanate coupling agent is a chelate solution of bis(dioctyloxypyrophosphate)ethylene titanate and triethanolamine.

7. A method for preparing the cerium oxide-loaded white carbon black filler according to claim 1, characterized in that: The steps include: (1) preparing an ethanol aqueous solution, adding glacial acetic acid to adjust the pH value of the system to 3.5, adding a titanate coupling agent and stirring, then adding nano-cerium oxide powder, stirring at 60°C for 2 hours, centrifuging, washing, and spray drying to obtain modified nano-cerium oxide; (2) Adding bio-based silica into water and stirring, ultrasonic treatment to obtain a bio-based silica dispersion, adding dopamine hydrochloride and tris(hydroxymethyl)aminomethane to the biomass silica dispersion under stirring conditions, controlling the pH value of the system to 8.5-9.0, and stirring the reaction; (3) Adding the modified nano-cerium oxide prepared in step (1) to the reaction product of step (2), continuing the reaction for 1 hour, centrifuging to obtain a precipitate, washing, and spray drying to obtain a cerium oxide-loaded white carbon black filler.

8. The preparation method according to claim 7, characterized in that: The mass ratio of titanate coupling agent, nano-cerium oxide, bio-based white carbon black and dopamine hydrochloride is 10:10:10:1.

5.

9. Use of the cerium oxide-loaded white carbon black filler according to claim 1 in preparing a natural rubber composite material.

10. The use according to claim 9, characterized in that The natural rubber composite material comprises the following raw materials in parts by weight: 100 parts of natural rubber, 5-8 parts of zinc oxide, 2-4 parts of stearic acid, 2-10 parts of cerium oxide-loaded white carbon black filler, 30-60 parts of carbon black N550, 3-5 parts of paraffin oil, 1-2 parts of sulfur, and 1.5-2.5 parts of N-tert-butyl-2-benzothiazole sulfenamide.