Lightweight high-viscosity high-folding-resistance foxing rubber and manufacturing method thereof

By combining modified chlorosulfonated polyethylene rubber and materials such as SEBS, along with modified lightweight filler masterbatch and a specific mixing process, a lightweight, high-adhesion-strength sheath rubber was prepared, solving the problems of high density and insufficient viscosity, and achieving improved folding resistance and extended service life.

CN118930988APending Publication Date: 2024-11-12ZHEJIANG ZHONGRUI RUBBER POLYMER MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411251426.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing rubber sashes have high density and insufficient adhesion, making it difficult to solve the problem of delamination and to achieve lightweight and durable rubber sashes.

Method used

Lightweight, high-viscosity, and high-bending-resistance rubber is prepared using modified chlorosulfonated polyethylene rubber, SEBS, modified lightweight filler masterbatch, and other raw materials through a specific mixing process. Low molecular weight liquid rubber is added to improve initial tack, and modified glass microspheres are used to reduce density.

Benefits of technology

It achieves lightweight yet high bonding strength, excellent folding resistance, reduces product density to approximately 1.0 g/cm³, extends service life, and improves wearing comfort.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to lightweight high-viscosity high-folding-resistance foxing rubber and a preparation method thereof. The lightweight high-viscosity high-folding-resistance foxing rubber comprises the following substances in parts by weight: 10-20 parts of modified chlorosulfonated polyethylene rubber; 30 to 40 parts of natural rubber; 20 to 40 parts of SEBS; 40 to 90 parts of modified light filler master batch; 5-10 parts of low molecular weight liquid rubber; 2-4 parts of an activator; 5-10 parts of a softening agent; 2.5 to 3.5 parts of nano zinc oxide; 1-2 parts of stearic acid; 20 to 40 parts of white carbon black; 10 to 15 parts of titanium dioxide; 30-40 parts of nano calcium carbonate, a vulcanizing agent, a vulcanization accelerator and the like; the preparation method comprises the following steps: mixing for multiple times, lifting, cleaning and mixing for three times, mixing and turning over. The cable has good ozone resistance and atmospheric aging resistance, and the service life is prolonged; the material has good anti-ultraviolet stability, oxidation resistance and thermal stability and excellent mechanical properties, and the specific gravity is reduced; the initial viscosity and the bending resistance of the rubber are improved. The modified light filler master batch can be dispersed in the rubber more uniformly and can be well combined with the rubber, so that the density is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a rubber wainscot, and more particularly to a lightweight, high-viscosity, high-folding-resistance wainscot rubber and a manufacturing method thereof. Background Art

[0002] With the rapid development of society, the social division of labor has become more and more detailed. Due to the different living and working environments, social groups have higher and higher requirements for health and safety. As daily necessities, shoes, in addition to being fashionable and beautiful, also have other complex functions. Now, people want shoes to be light and durable, which requires the rubber used in shoes to be very light and have a long wearing life. At present, although vulcanized rubber shoes have made breakthroughs in lightweight rubber outsoles, the density of rubber strips, which account for more than 50% of the rubber used in shoes, is still 1.5g / cm 3 The problem of debonding cannot be solved effectively. 3 Rubber strips with good adhesion on the left and right. Summary of the invention

[0003] In view of the deficiencies in the prior art, the object of the present invention is to provide a lightweight, low-density, high-viscosity and high-folding-resistance rubber strip that is lightweight, low-density and good in viscosity.

[0004] To achieve the above object, the present invention provides the following technical solution: a lightweight, high-viscosity, high-folding-resistance rubber strip, comprising the following material components in parts by weight: Modified chlorosulfonated polyethylene rubber 10-20 parts; 30-40 parts of natural rubber; SEBS 20-40 parts; 40-90 parts of modified lightweight filler masterbatch; 1-2.5 parts of vulcanizing agent; 2-3 parts of vulcanization accelerator; 5-10 parts of low molecular weight liquid rubber; 2-4 parts of activator; Softener 5-10 parts; 2.5-3.5 parts of nano zinc oxide; 1-2 parts of stearic acid; 20-40 parts of white carbon black; 10-15 parts of titanium dioxide; 30-40 parts of nano calcium carbonate.

[0005] As a further improvement of the present invention, the method for preparing the modified lightweight filler masterbatch comprises the following steps: Step 1: Prepare raw materials according to the weight ratio of concentrated phosphoric acid: glass microspheres = (1.0-1.5) : (2.0-3.0), put the glass microspheres into the concentrated phosphoric acid solution and stir and mix, stir at high temperature for 15-25 minutes to obtain a first mixture; then add an equal amount of water to the first mixed solution and continue to stir and mix to obtain a second mixed solution; Step 2: adding the second mixed solution into a centrifuge to remove water and phosphoric acid solution, and drying to obtain surface-corroded glass microbeads; Step 3: respectively prepare raw materials according to weight proportions of 20-30 parts of surface corroded glass microbeads, 2-3 parts of aminosilane coupling agent, 4-6 parts of solution polymerized styrene-butadiene rubber, and 6-9 parts of natural rubber; put the prepared solution polymerized styrene-butadiene rubber and natural rubber into an internal mixer for mixing for 130-180 seconds, then put the prepared surface corroded glass microbeads and aminosilane coupling agent into the internal mixer, mix for 180-220 seconds, discharge the glue at 125-135°C, and cool the sheets under the open mixer after the discharge of glue; Step 4: After standing for 24 hours, mix in the internal mixer for another 250-350 seconds, and then granulate and cool in the preforming machine to make a modified lightweight filler masterbatch.

[0006] As a further improvement of the present invention, the white carbon black is HS260 white carbon black. The model of the SEBS is YH503T, which has a relatively light specific gravity. The modified chlorosulfonated polyethylene rubber is MCSM rubber, which has better compatibility with natural rubber and SEBS and better anti-ozone cracking performance.

[0007] As a further improvement of the present invention, the low molecular weight liquid rubber is a diene liquid rubber with a molecular weight of 2000-5000, which improves the initial viscosity and anti-bending property of the rubber.

[0008] As a further improvement of the present invention, the softener is a mixture of C5 xylene resin and environmentally friendly naphthenic oil. The activator is a mixture of diethylene glycol, polyethylene glycol and a silane coupling agent.

[0009] The method for preparing the lightweight, high-viscosity and high-folding-resistance rubber strip comprises the following steps: S1: Prepare the raw materials according to the set weight proportions, put the modified chlorosulfonated polyethylene rubber, natural rubber, SEBS, and modified lightweight filler masterbatch into an internal mixer and mix them for 40-60 seconds at a mixing temperature of 95-105°C; S2: Then, the set weight portions of activator, softener, low molecular weight liquid rubber and reinforcing filler, nano zinc oxide and stearic acid are added to the internal mixer and continue to be internally kneaded, followed by three times of bolt lifting, cleaning and internal kneading for a total of 120-180s; the temperature of the first bolt lifting is controlled at 90-110°C, and the internal kneading time is 40-60s, the temperature of the second bolt lifting is increased to 100-115°C, and the internal kneading time is 40-60s, and the temperature of the third bolt lifting is increased to 115-125°C, and the internal kneading time is 40-60s; S3: After the lifting bolt is cleaned, continue to mix for 50-70 seconds, discharge the glue at 120-135℃ to obtain the rubber compound; S4: The rubber material is placed for 12-15 hours, and then mixed on an open mill. After mixing evenly, the rubber material is discharged in a uniform sheet shape. S5: The rubber material on the mixing mill is re-preheated evenly, and a set weight portion of vulcanizing agent and vulcanization accelerator is added, and after being evenly mixed, it is rolled up for use; through the above steps, a lightweight, high-viscosity, and high-folding-resistant rubber strip product is obtained.

[0010] The beneficial effects of the present invention are as follows: the present invention is prepared by using natural rubber, modified chlorosulfonated polyethylene rubber, SEBS, and modified lightweight filler masterbatch as raw materials, and adding various additives such as fillers; as one of the innovative points of the present invention, modified chlorosulfonated polyethylene rubber is added, which has good compatibility with rubbers such as natural rubber and SEBS, has good ozone resistance and atmospheric aging resistance, and can improve the service life of the product; in addition, the present invention innovatively adds SEBS in the formula, and SEBS is a linear triblock copolymer with polystyrene as the terminal segment and ethylene-butene copolymer obtained by hydrogenating polybutadiene as the middle elastic block, does not contain unsaturated double bonds, has good UV resistance stability, oxidation resistance and thermal stability and excellent mechanical properties, and has a specific gravity of only 0.91g / cm 3 , while increasing the product life, the product specific gravity is reduced; at the same time, in order to improve the bonding strength of the product, low molecular weight liquid rubber is added. The low molecular weight liquid rubber is a diene liquid rubber with a molecular weight of 2000-5000, which improves the initial viscosity and anti-bending properties of the rubber.

[0011] In addition, in order to further reduce the density of the product to 1.0g / cm 3 The present invention also adds a modified compressive strength of 18000psi and a density of 0.38-0.4g / cm 3The modified lightweight filler masterbatch made of glass microspheres can reduce the specific gravity of the product. As another innovative point of the present invention, in order to solve the negative impact of the surface inertia of glass microspheres on the mechanical properties of the product, the surface is firstly treated with concentrated phosphoric acid for corrosion, and after dehydration and drying, the surface-corroded glass microspheres, aminosilane coupling agent, solution-polymerized styrene-butadiene rubber, and natural rubber are put into a (meshing type) internal mixer at a specific ratio for high-temperature mixing. After the rubber is discharged, the lower sheet of the open mixer is cooled for 24 hours, and then mixed in the (meshing type) internal mixer for another 250-350 seconds, and then the preformer is molded and granulated and cooled to make a modified lightweight filler masterbatch. The modified lightweight filler masterbatch can be dispersed more evenly in the rubber, and can be well combined with the rubber, which solves the problem of the inertia of the glass microspheres and reduces the product density. DETAILED DESCRIPTION

[0012] The examples are as follows: 1. Preparation of modified lightweight filler masterbatch, including the following steps: Step 1: Prepare the raw materials according to the ratio of concentrated phosphoric acid: glass beads = 1:2, put the glass beads into the concentrated phosphoric acid solution and stir and mix, stir at high temperature for 15 minutes to obtain a first mixture; then add an equal amount of water to the first mixture and continue stirring and mixing for 5 minutes to obtain a second mixture; Step 2: Add the second mixed solution into a centrifuge to remove water and phosphoric acid at high speed. Use a dryer to dry the mixture to obtain glass microbeads with corroded surfaces. Step 3: Prepare the raw materials of the surface-corroded glass microbeads, aminosilane coupling agent, solution-polymerized styrene-butadiene rubber and natural rubber in a weight ratio of 10:1:2:3; put the prepared solution-polymerized styrene-butadiene rubber and natural rubber into a meshing type internal mixer for mixing for 150 seconds, then put the prepared surface-corroded glass microbeads and aminosilane coupling agent into the internal mixer for mixing for 200 seconds, discharge the glue at 130°C, and cool the sheets under the open mixer after the discharge; Step 4: After standing for 24 hours, mix in an intermeshing internal mixer for 300 seconds, and then granulate and cool in a preforming machine to produce a modified lightweight filler masterbatch.

[0013] 2. Formula Weight Ratio Each embodiment and control example was weighed according to the following Table 1.

[0014]

[0015] In Table 1, the natural rubber is 3L natural rubber produced in Vietnam. The reinforcing filler is a mixture of white carbon black, nano calcium carbonate, and titanium dioxide. The SEBS brand is Baling Petrochemical YH-503T (thermoplastic rubber). The softener is a mixture of C5 xylene resin and environmentally friendly cyclohexane oil. The activator is a mixture of diethylene glycol, polyethylene glycol, and silane coupling agent. Vulcanization system: the vulcanizing agent is sulfur, the vulcanization accelerators are accelerator DM, anti-yellowing accelerator, and accelerator NS, and the vulcanization activator is nano zinc oxide and stearic acid.

[0016] 3. Production Process 1. Ingredients According to the formula table of the embodiment and the comparative example in Table 1, natural rubber, modified chlorosulfonated polyethylene rubber, SEBS (i.e., the hydrogenated product of SBS), and modified lightweight filler masterbatch are weighed to form material A, and low molecular weight liquid rubber, activator, softener, reinforcing filler, nano zinc oxide, and stearic acid are weighed to form material B; 2. Mixing. It includes the following steps: S1: Put material A into internal mixer and mix for 45 seconds at a mixing temperature of 100°C; S2: Then add material B into the internal mixer and continue to internally mix, then raise the bolt and clean the internal mixer for 3 times for a total of 150 seconds; the temperature of the first time of raising the bolt is controlled at 100℃ for internal mixing for 50 seconds, the temperature of the second time is raised to 105℃ for internal mixing for 50 seconds, and the temperature of the third time is raised to 115℃ for internal mixing for 50 seconds; S3: After the lifting bolt is cleaned, the mixing is continued for 60 seconds, and the rubber is discharged at 125°C to obtain the rubber compound; S4: The rubber material is placed for 12 hours, and then mixed on a two-roll open mill with a roller distance of 1 mm. After mixing evenly, the sheet is produced in a uniform sheet shape; S5: Preheat the rubber on the mixing mill evenly, add the corresponding vulcanizer and vulcanization accelerator, refining evenly and rolling for use; S6: The rolled rubber material is formed into a rubber strip having a certain specification and pattern through an extruder and a three-roll calender; S7: After bonding the molded rubber strip to the upper surface, vulcanize in a vulcanizer at 137 degrees for 45 minutes to finalize the shape.

[0017] 4. Test results of rubber materials for garter strips 1. The mechanical properties, adhesive properties and density test results of Examples 1-3 and Comparative Examples 1-2 are shown in Table 2.

[0018]

[0019] 2. The anti-ozone cracking test results of Examples 1-3 and Comparative Examples 1-2 are shown in Table 3 (B method in GB / T7762-2014, temperature 40°C, ozone concentration [25±5]×10-8 , stretch 20%).

[0020]

[0021] 3. The bending resistance test results of Examples 1-3 and Comparative Examples 1-2 are shown in Table 4 (Method A in HG / T2871-2008, temperature bending angle 45°, bending frequency 250 times / min).

[0022]

[0023] It can be seen from Table 2 that the mechanical properties of the embodiment are much higher than those of the control example, and much higher than the relevant national and industry standards. In particular, the density is reduced by 30-35%, thereby reducing the consumption of rubber by about 30%, reducing energy consumption, and at the same time, the weight of each pair of shoes can be reduced by about 70 grams on average, improving the wearing comfort; in addition, the bonding strength of the embodiment is much higher than that of the control example, which improves the product life. It can be seen from Table 3 that the anti-ozone cracking performance of the embodiment is much higher than that of the control example by 2-4 times, which prolongs the storage and service life of the product. It can be seen from Table 4 that the bending resistance of the embodiment is much higher than that of the control example. The control example has severe debonding and strip breakage at 80,000 times and 120,000 times respectively, while the embodiment has slight debonding at 150,000 times and slight cracks at 200,000 times, and the wearing life is increased by more than 2 times. In summary, the lightweight, high-viscosity and high-folding-resistant rubber strip of the present invention breaks through the design of traditional rubber strips in terms of material application and formula structure. It reduces the weight by 30%, improves the adhesion by more than 30%, and increases the folding resistance by more than 80,000 times. On the basis of extending the service life of the product, it achieves product lightweight and improves wearing comfort.

Claims

1. Lightweight, high-viscosity and high-folding-resistance rubber strip, characterized by: The composition comprises the following parts by weight: Modified chlorosulfonated polyethylene rubber 10-20 parts; 30-40 parts of natural rubber; SEBS 20-40 parts; Modified lightweight filler masterbatch 40-90 parts; 1-2.5 parts of vulcanizing agent; 2-3 parts of vulcanization accelerator; 5-10 parts of low molecular weight liquid rubber; 2-4 parts of activator; 5-10 parts of softener; Nano zinc oxide 2.5-3.5 parts; 1-2 parts of stearic acid; 20-40 parts of white carbon black; 10-15 parts of titanium dioxide; 30-40 parts of nano calcium carbonate.

2. The lightweight, high-viscosity, high-folding-resistance rubber strip according to claim 1, characterized in that: The preparation method of the modified lightweight filler masterbatch comprises the following steps: Step 1: Prepare raw materials according to the weight ratio of concentrated phosphoric acid: glass microspheres = (1.0-1.5) : (2.0-3.0), put the glass microspheres into the concentrated phosphoric acid solution and stir and mix, stir at high temperature for 15-25 minutes to obtain a first mixture; then add an equal amount of water to the first mixed solution and continue to stir and mix to obtain a second mixed solution; Step 2: adding the second mixed solution into a centrifuge to remove water and phosphoric acid solution, and drying to obtain surface-corroded glass microbeads; Step 3: respectively prepare raw materials according to weight proportions of 20-30 parts of surface corroded glass microbeads, 2-3 parts of aminosilane coupling agent, 4-6 parts of solution polymerized styrene-butadiene rubber, and 6-9 parts of natural rubber; put the prepared solution polymerized styrene-butadiene rubber and natural rubber into an internal mixer for mixing for 130-180 seconds, then put the prepared surface corroded glass microbeads and aminosilane coupling agent into the internal mixer, mix for 180-220 seconds, discharge the glue at 125-135°C, and cool the sheets under the open mixer after the discharge of glue; Step 4: After standing for 24 hours, mix in the internal mixer for another 250-350 seconds, and then granulate and cool in the preforming machine to make a modified lightweight filler masterbatch.

3. The lightweight, high-viscosity, high-folding-resistance rubber strip according to claim 1, characterized in that: The white carbon black is HS260 white carbon black.

4. The lightweight, high-viscosity, high-folding-resistance rubber strip according to claim 1, characterized in that: The model of the SEBS is YH503T, and its specific gravity is relatively light.

5. The lightweight, high-viscosity, high-folding-resistance rubber strip according to claim 1 or 2, characterized in that: The low molecular weight liquid rubber is a diene liquid rubber with a molecular weight of 2000-5000.

6. The lightweight, high-viscosity, high-folding-resistance rubber strip according to claim 1, characterized in that: The softener is a mixture of C5 xylene resin and environmentally friendly naphthenic oil.

7. The lightweight, high-viscosity, high-folding-resistance rubber strip according to claim 1 or 6, characterized in that: The activator is a mixture of diethylene glycol, polyethylene glycol and a silane coupling agent.

8. The method for preparing the lightweight, high-viscosity and high-folding-resistance rubber strip according to claim 1 or 2, characterized in that: The following steps are involved: S1: Prepare the raw materials according to the set weight proportions, put the modified chlorosulfonated polyethylene rubber, natural rubber, SEBS, and modified lightweight filler masterbatch into an internal mixer and mix them for 40-60 seconds at a mixing temperature of 95-105°C; S2: Then, the set weight portions of activator, softener, low molecular weight liquid rubber and reinforcing filler, nano zinc oxide and stearic acid are added to the internal mixer and continue to be internally kneaded, followed by three times of bolt lifting, cleaning and internal kneading for a total of 120-180s; the temperature of the first bolt lifting is controlled at 90-110°C, and the internal kneading time is 40-60s, the temperature of the second bolt lifting is increased to 100-115°C, and the internal kneading time is 40-60s, and the temperature of the third bolt lifting is increased to 115-125°C, and the internal kneading time is 40-60s; S3: After the lifting bolt is cleaned, continue to mix for 50-70 seconds, discharge the glue at 120-135℃ to obtain the rubber compound; S4: The rubber material is placed for 12-15 hours, and then mixed on an open mill. After mixing evenly, the rubber material is discharged in a uniform sheet shape. S5: The rubber material on the mixing mill is re-preheated evenly, and a set weight portion of vulcanizing agent and vulcanization accelerator is added, and after being evenly mixed, it is rolled up for use; through the above steps, a lightweight, high-viscosity, and high-folding-resistant rubber strip product is obtained.