Preparation process of flexible plastic sports field material

Through the cross-linking reaction between high-molecular-weight butadiene-propylene copolymer and low-molecular-propylene copolymer, combined with PP, EVA, PS and fillers, the flexibility and mechanical strength of existing plastic sports field materials are solved. The problem of this problem achieves higher flexibility and mechanical strength, and extends the service life through cross-linking reactions and the use of additives, meeting higher sports needs.

CN118930990AInactive Publication Date: 2024-11-12DAOYI HIGH POLYMERS (NINGBO) CO LTD

Patent Information

Application Number
CN202411405489.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The flexibility and mechanical strength of existing plastic sports field materials are difficult to meet the growing demand for sports, and the preparation process is complex and performance is limited.

Method used

The cross-linking reaction of high molecular weight butadiene-ethylene propylene copolymer and low molecular weight butadiene-ethylene propylene copolymer was prepared by extrusion granulation process to improve flexibility and Materials with mechanical strength use cross-linking reactions of active groups such as isocyanate groups and amino groups to form a stable structure, and combine compatibility, antioxidant and lubricant to improve the compatibility and oxidation resistance of the material.

Benefits of technology

It significantly improves flexibility and mechanical strength, extends the service life of the material, and forms a stable and high-strength adhesion structure during laying to prevent disengagement and meets higher sports needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation process of a flexible plastic sports field material, and relates to the technical field of high-molecular compounds, and the preparation process comprises a raw material preparation part, a mixed melting part and an extrusion granulation part; the raw material preparation part comprises the step of preparing a butadiene-ethylene-propylene copolymer, PP (polypropylene), EVA (ethylene-vinyl acetate), PS (polystyrene), a filler and an auxiliary agent which serve as raw materials; the mixing and melting part comprises the following steps: preliminarily stirring 40-50 parts by weight of butadiene-ethylene-propylene copolymer, then adding 8-12 parts by weight of PP, 2-5 parts by weight of EVA, 4-7 parts by weight of PS, 26-32 parts by weight of filler and 1.5-9 parts by weight of auxiliaries into the preliminarily stirred butadiene-ethylene-propylene copolymer, and continuously stirring to form a mixed material; controlling the temperature of the mixed material to be 78-82 DEG C, and introducing the mixed material into a stock bin of an extruder; and the extrusion granulation part comprises the steps of extruding a molten mixed material by adopting an extruder die head and cutting the molten mixed material by adopting an underwater granulator blade to obtain material particles. The method has the effect of solving the problems of insufficient mechanical strength and low flexibility caused by non-uniform dispersion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer compounds, and in particular to a preparation process of a flexible plastic sports field material. Background Art

[0002] Plastic sports fields are generally paved with polyurethane prepolymers, mixed polyethers, waste tire rubber, EPDM rubber particles or PU particles, pigments, additives and fillers. The plastic sports field can produce an appropriate rebound force for athletes through appropriate elasticity, while also protecting the joints and ligaments of athletes and reducing the risk of injury. The plastic track also has excellent wear resistance, which can ensure the long-term stability of the plastic track structure.

[0003] A Chinese patent with announcement number CN105801758B discloses an environmentally friendly resin for use in plastic sports fields and a preparation method thereof. The environmentally friendly resin for use in plastic sports fields is prepared by polymerization using acrylate monomers as the main component, assisted by cross-linking monomers, hydroxyl monomers containing double bonds, functional monomers, etc. in an emulsifier and deionized water environment.

[0004] However, the reaction components of the environmentally friendly resin used in plastic sports fields are complex, the overall preparation process is difficult, and from a performance perspective, its maximum flexibility is 147.07% of the elongation at break, and the corresponding maximum tensile strength is 1.42MPa, which is difficult to match the growing demand for sports and needs to be improved. Summary of the invention

[0005] In view of this, the purpose of this application is to provide a preparation process of a flexible plastic sports field material to achieve the purpose of improving flexibility and mechanical strength. The specific scheme is as follows: A preparation process of a flexible plastic sports field material, comprising a raw material preparation part, a mixing and melting part, and an extrusion granulation part; The raw material preparation part includes preparing butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials; The mixed melting part comprises preliminarily stirring 40-50 parts by weight of a butadiene-propylene copolymer, adding 8-12 parts by weight of PP, 2-5 parts by weight of EVA, 4-7 parts by weight of PS, 26-32 parts by weight of a filler and 1.5-9 parts by weight of an auxiliary agent to the preliminarily stirred butadiene-propylene copolymer, continuing to stir to form a mixed material, and controlling the temperature of the mixed material to reach 78-82° C. before introducing the mixed material into a silo of an extruder; The extrusion granulation part includes using an extruder die head to extrude the molten mixture and an underwater pelletizer blade to cut to obtain material particles; The butadiene-propylene copolymer is formed by mixing a high molecular weight butadiene-propylene copolymer having a molecular weight greater than 20,000 and a low molecular weight butadiene-propylene copolymer having a molecular weight less than 2,000 in a mass percentage of 27.5-32.5:12.5-17.5; and the high molecular weight butadiene-propylene copolymer is obtained by grafting and modifying a base resin and a first active grafting monomer and a second active grafting monomer and has a first active group and a second active group; the low molecular weight butadiene-propylene copolymer is composed of a base resin grafted with a third active group; the first active group and the second active group are cross-linked with each other, the first active group and the third active group are cross-linked with each other, and the second active group and the third active group are cross-linked with each other.

[0006] Preferably: the first reactive group is an isocyanate group; and the second reactive group is an amino group.

[0007] Preferably, the grafting modification is melt grafting modification, and the grafting rate is 0.1-2%.

[0008] Preferably, the third reactive group is a hydroxyl group, a carboxyl group, a sulfonic acid group or an acyl chloride group.

[0009] Preferably, the grafting modification is copolymerization or melt grafting modification, and the grafting rate is 1-5%.

[0010] Preferably, the auxiliary agent includes 1.5-2.5 parts by weight of a compatibilizer.

[0011] Preferably, the auxiliary agent further comprises 2-3.5 parts by weight of an antioxidant UV, 1.5-2.5 parts by weight of a lubricant and 0-1 part by weight of white oil.

[0012] Preferably: in the mixed molten part, the high molecular weight butadiene-propylene copolymer and the low molecular weight butadiene-propylene copolymer are first stirred and mixed for 10-20 minutes, then white oil is added and stirred until completely absorbed, and finally PP, EVA, PS, fillers and additives are added.

[0013] Preferably: the number of die holes of the extruder is 20-40, the hole diameter is 2-3 mm, the rotation speed is 300-400 r / min, the feeding is 15 Hz, the current is 150 V, and the number of blades of the underwater pelletizer is 6, and the rotation speed is 360-420 r / min.

[0014] Preferably: the filler is calcium powder.

[0015] It can be seen from the above scheme that the present application provides a preparation process of a flexible plastic sports field material, and the preparation process of the flexible plastic sports field material has the following beneficial effects: 1. Through the mutual cross-linking reaction between the first active group and the second active group on the high molecular weight butadiene-propylene copolymer and the third active group on the low molecular weight butadiene-propylene copolymer, the problem of insufficient mechanical strength and low flexibility caused by uneven dispersion between butadiene-propylene copolymer, PP, EVA, PS and filler is solved; 2. A butadiene-propylene copolymer obtained by mixing a high molecular weight butadiene-propylene copolymer having a molecular weight greater than 20,000 and a low molecular weight butadiene-propylene copolymer having a molecular weight less than 2,000 is mixed with PP, EVA, PS and filler in corresponding proportions, thereby significantly improving flexibility and mechanical strength; 3. Through the cross-linking and condensation reaction between isocyanate groups and amino groups, as well as the cross-linking and condensation reaction between hydroxyl groups, carboxyl groups, sulfonic acid groups or acyl chloride groups, the components are mixed to form a stable structure, and a stable and high-strength adhesion structure is formed with the paved ground during laying, which plays a role in preventing detachment; 4. The mixing uniformity and compatibility between the components are further improved through compatibilizers, antioxidants UV and lubricants, and the antioxidant properties are effectively improved, thereby extending the service life. DETAILED DESCRIPTION

[0016] The following will be clearly and completely described in conjunction with the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0017] It should be mentioned that the compatibilizer of this application is purchased from the maleic anhydride grafted compatibilizer of Nanjing Sutai Polymer Technology Co., Ltd., the antioxidant UV is the antioxidant UV-531 purchased from Jinan Huifengda Chemical Co., Ltd., the lubricant is Durepol PBT HL NTLA010 BT314 purchased from Dongguan Yuhong Plastic Co., Ltd., the white oil is purchased from POWER OIL of Wuhu Xinnuo Lubrication Technology Co., Ltd., the calcium powder is commercially available calcium carbonate, PP, EVA and PS are all commercially available materials, which will not be elaborated here.

[0018] At the same time, in order to complete the grafting modification treatment of the first active group, the second active group and the third active group, the monomers containing the corresponding isocyanate groups, such as toluene diisocyanate, cyclohexyl isocyanate or 2-isopropyl-6-methylphenyl isocyanate, can be subjected to melt grafting reaction, and the monomers containing amino groups, such as aniline, 4-bromo-1,2-phenylenediamine, 2-bromo-5-aminobenzoic acid ethyl ester, etc. can be subjected to melt grafting reaction, which will not be elaborated here.

[0019] The following is a detailed description of the preparation process of the flexible plastic sports field material of the present application.

[0020] A preparation process of a flexible plastic sports field material comprises a raw material preparation part, a mixing and melting part and an extrusion granulation part.

[0021] in: The raw material preparation part includes preparing butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials; The mixed melting part includes preliminarily stirring 40-50 parts by weight of butadiene-propylene copolymer, adding 8-12 parts by weight of PP, 2-5 parts of EVA, 4-7 parts of PS, 26-32 parts of fillers and 1.5-9 parts of additives to the preliminarily stirred butadiene-propylene copolymer, continuing to stir to form a mixed material, and controlling the temperature of the mixed material to reach 78-82° C. before introducing it into the silo of the extruder. The filler is selected to be calcium powder, which has the effect of low cost and significantly improving the mechanical strength of the flexible plastic sports field material.

[0022] The extrusion granulation part includes using an extruder die to extrude the molten mixed material and using an underwater pelletizer blade to cut the material particles.

[0023] It should be noted that in order to improve the dispersibility and mutual affinity between the butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials, so as to effectively improve the mechanical properties and achieve the purpose of improving flexibility, the butadiene-propylene copolymer used is a mixture of a high molecular weight butadiene-propylene copolymer with a molecular weight greater than 20,000 and a low molecular weight butadiene-propylene copolymer with a molecular weight less than 2,000 at a mass percentage of 27.5-32.5:12.5-17.5. And the high molecular weight butadiene-propylene copolymer is obtained by grafting and modifying the base resin and the first active grafting monomer and the second active grafting monomer and has the first active group and the second active group. The low molecular weight butadiene-propylene copolymer is composed of the base resin grafted with the third active group. It should be mentioned that the first active group and the second active group are cross-linked with each other, the first active group and the third active group are cross-linked with each other, and the second active group and the third active group are cross-linked with each other.

[0024] Therefore, while the first active group and the second active group on the high molecular weight butadiene-propylene copolymer are cross-linked to form a ring structure, the first active group and the third active group, and the second active group and the third active group are cross-linked to form a cross-linked network space structure. On the premise of achieving effective mechanical improvement, the mixed combination with PP, EVA, PS, fillers and additives can achieve the effect of effectively improving flexibility.

[0025] In the embodiment of the present application, the first reactive group is an isocyanate group; the second reactive group is an amino group. Of course, the first reactive group and the second reactive group can also be other reactive groups that can cross-link with each other, and can respectively cross-link with the third reactive group.

[0026] Specifically, the third active group is a hydroxyl group, a carboxyl group, a sulfonic acid group or an acyl chloride group. In the high molecular weight butadiene-propylene copolymer, the grafting modification is a melt grafting modification, and the grafting rate is 0.1-2%. In the low molecular weight butadiene-propylene copolymer, the grafting modification is a copolymerization or a melt grafting modification, and the grafting rate is 1-5%.

[0027] In the embodiment of the present application, the auxiliary agent includes 1.5-2.5 parts by weight of a compatibilizer. The compatibilizer has the effect of improving the interaction between incompatible polymers, and thus significantly improves the compatibility and affinity during the mixing process of the high molecular weight butadiene-propylene copolymer, the low molecular weight butadiene-propylene copolymer, and PP, EVA, PS and fillers in the embodiment of the present application.

[0028] At the same time, in order to further improve the service life of the flexible plastic sports field material prepared by the preparation process of the flexible plastic sports field material, the additive also includes 2-3.5 parts by weight of antioxidant UV, 1.5-2.5 parts of lubricant and 0-1 part of white oil.

[0029] White oil has the effect of adjusting color, improving reflection and extending service life. In the mixed molten part, the high molecular weight butadiene-propylene copolymer and the low molecular weight butadiene-propylene copolymer are first stirred and mixed for 10-20 minutes, then the white oil is added and stirred until completely absorbed, and finally PP, EVA, PS, fillers and additives are added and stirred and mixed evenly. In the machine equipment used, the number of die holes of the extruder is controlled to be 20-40, the aperture is 2-3mm, the speed is 300-400r / min, the feed is 15Hz, the current is 150V, and the number of blades of the underwater pelletizer is controlled to be 6, and the speed is 360-420r / min, so as to obtain material particles with regular shapes and specifications. The filler is calcium powder.

[0030] Embodiment 1 A preparation process of a flexible plastic sports field material comprises a raw material preparation part, a mixing and melting part and an extrusion granulation part.

[0031] in: The raw material preparation part includes preparing butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials; The mixed molten part includes preliminary stirring of 40 parts by weight of butadiene-propylene copolymer, and then adding 8 parts by weight of PP, 2 parts of EVA, 4 parts of PS, 26 parts of calcium powder and 1.5 parts of compatibilizer to the preliminary stirred butadiene-propylene copolymer, and continuing to stir to form a mixed material, and controlling the temperature of the mixed material to reach 78°C before introducing it into the silo of the extruder. Calcium powder has the effect of low cost and significantly improving the mechanical strength of the flexible plastic sports field material. The compatibilizer has the effect of improving the interaction between incompatible polymers, thereby significantly improving the compatibility and affinity during the mixing process of the high molecular weight butadiene-propylene copolymer, the low molecular weight butadiene-propylene copolymer, and PP, EVA, PS and filler in Example 1 of the present application.

[0032] The extrusion granulation part includes using an extruder die head to extrude the molten mixture and an underwater pelletizer blade to cut the material particles. In Example 1 of the present application, the number of die holes of the extruder is controlled to be 20, the aperture is 2 mm, the rotation speed is 300 r / min, the feeding is 15 Hz, the current is 150 V, and the number of blades of the underwater pelletizer is controlled to be 6, and the rotation speed is 360 r / min, so as to obtain material particles with regular shapes and specifications.

[0033] It should be noted that in order to improve the dispersibility and mutual affinity between the butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials, so as to effectively improve the mechanical properties and achieve the purpose of improving flexibility, the butadiene-propylene copolymer used is a mixture of a high molecular weight butadiene-propylene copolymer with a molecular weight greater than 20,000 and a low molecular weight butadiene-propylene copolymer with a molecular weight less than 2,000 at a mass percentage of 27.5:12.5. And the high molecular weight butadiene-propylene copolymer is obtained by grafting and modifying the base resin and the first active grafting monomer and the second active grafting monomer and has the first active group and the second active group. The low molecular weight butadiene-propylene copolymer is composed of the base resin grafted with the third active group. It should be mentioned that the first active group and the second active group are cross-linked with each other, the first active group and the third active group are cross-linked with each other, and the second active group and the third active group are cross-linked with each other.

[0034] Therefore, while the first active group and the second active group on the high molecular weight butadiene-propylene copolymer are cross-linked to form a ring structure, the first active group and the third active group, and the second active group and the third active group are cross-linked to form a cross-linked network space structure. On the premise of achieving effective mechanical improvement, the mixed combination with PP, EVA, PS, fillers and additives can achieve the effect of effectively improving flexibility.

[0035] In the first embodiment of the present application, the first reactive group is an isocyanate group, and the second reactive group is an amino group. Of course, the first reactive group and the second reactive group may also be other reactive groups that can cross-link with each other, and can cross-link with the third reactive group respectively, which will not be described in detail here. However, it is preferred that the isocyanate group is used as the first reactive group, and the amino group is used as the second reactive group.

[0036] Specifically, the third active group is a sulfonic acid group. In the high molecular weight butadiene-propylene copolymer, the grafting modification is melt grafting modification, and the grafting rate of the first active group is 0.1%, and the grafting rate of the second active group is 0.3%. In the low molecular weight butadiene-propylene copolymer, the grafting modification is copolymerization grafting modification, and the grafting rate is 1%.

[0037] Embodiment 2 A preparation process of a flexible plastic sports field material comprises a raw material preparation part, a mixing and melting part and an extrusion granulation part.

[0038] in: The raw material preparation part includes preparing butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials; The mixed molten part includes preliminary stirring of 45 parts by weight of butadiene-propylene copolymer, and then adding 10 parts by weight of PP, 3 parts of EVA, 5 parts of PS, 30 parts of calcium powder and 2 parts of compatibilizer to the preliminary stirred butadiene-propylene copolymer, and continuing to stir to form a mixed material, and controlling the temperature of the mixed material to reach 80°C before introducing it into the silo of the extruder. Calcium powder has the effect of low cost and significantly improving the mechanical strength of the flexible plastic sports field material. The compatibilizer has the effect of improving the interaction between incompatible polymers, and thus in the mixing process of the high molecular weight butadiene-propylene copolymer, the low molecular weight butadiene-propylene copolymer, and PP, EVA, PS and filler in Example 2 of the present application, the compatibility and affinity will be significantly improved.

[0039] The extrusion granulation part includes using an extruder die head to extrude the molten mixture and an underwater pelletizer blade to cut the material particles. In Example 2 of the present application, the number of die holes of the extruder is controlled to be 30, the aperture is 2.5 mm, the rotation speed is 350 r / min, the feeding is 15 Hz, the current is 150 V, and the number of blades of the underwater pelletizer is controlled to be 6, and the rotation speed is 400 r / min, so as to obtain material particles with regular shapes and specifications.

[0040] It should be noted that in order to improve the dispersibility and mutual affinity between the butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials, so as to effectively improve the mechanical properties and achieve the purpose of improving flexibility, the butadiene-propylene copolymer used is a mixture of a high molecular weight butadiene-propylene copolymer with a molecular weight greater than 20,000 and a low molecular weight butadiene-propylene copolymer with a molecular weight less than 2,000 at a mass percentage of 30:15. The high molecular weight butadiene-propylene copolymer is obtained by grafting and modifying the base resin and the first active grafting monomer and the second active grafting monomer and has a first active group and a second active group. The low molecular weight butadiene-propylene copolymer is composed of a base resin grafted with a third active group. It should be mentioned that the first active group and the second active group are cross-linked with each other, the first active group and the third active group are cross-linked with each other, and the second active group and the third active group are cross-linked with each other.

[0041] Therefore, while the first active group and the second active group on the high molecular weight butadiene-propylene copolymer are cross-linked to form a ring structure, the first active group and the third active group, and the second active group and the third active group are cross-linked to form a cross-linked network space structure. On the premise of achieving effective mechanical improvement, the mixed combination with PP, EVA, PS, fillers and additives can achieve the effect of effectively improving flexibility.

[0042] In the second embodiment of the present application, the first reactive group is an isocyanate group, and the second reactive group is an amino group. Of course, the first reactive group and the second reactive group may also be other reactive groups that can cross-link with each other, and can cross-link with the third reactive group respectively, which will not be described in detail here. However, it is preferred that the isocyanate group is used as the first reactive group, and the amino group is used as the second reactive group.

[0043] Specifically, the third active group is a hydroxyl group. In the high molecular weight butadiene-propylene copolymer, the grafting modification is melt grafting modification, and the grafting rate of the first active group is 0.8%, and the grafting rate of the second active group is 1.2%. In the low molecular weight butadiene-propylene copolymer, the grafting modification is melt grafting modification, and the grafting rate is 2.5%.

[0044] Embodiment 3 A preparation process of a flexible plastic sports field material comprises a raw material preparation part, a mixing and melting part and an extrusion granulation part.

[0045] in: The raw material preparation part includes preparing butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials; The mixed molten part includes preliminary stirring of 50 parts by weight of butadiene-propylene copolymer, and then adding 12 parts by weight of PP, 5 parts of EVA, 7 parts of PS, 32 parts of calcium powder and 2.5 parts of compatibilizer to the preliminary stirred butadiene-propylene copolymer, and continuing to stir to form a mixed material, and controlling the temperature of the mixed material to reach 78-82°C before introducing it into the silo of the extruder. Calcium powder has the effect of low cost and significantly improving the mechanical strength of the flexible plastic sports field material. The compatibilizer has the effect of improving the interaction between incompatible polymers, thereby significantly improving the compatibility and affinity during the mixing process of the high molecular weight butadiene-propylene copolymer, the low molecular weight butadiene-propylene copolymer, and PP, EVA, PS and filler in Example 3 of the present application.

[0046] The extrusion granulation part includes using an extruder die head to extrude the molten mixture and an underwater pelletizer blade to cut the material particles. In Example 3 of the present application, the number of die holes of the extruder is controlled to be 40, the aperture is 3 mm, the rotation speed is 400 r / min, the feed is 15 Hz, the current is 150 V, and the number of blades of the underwater pelletizer is controlled to be 6, and the rotation speed is 420 r / min, so as to obtain material particles with regular shapes and specifications.

[0047] It should be noted that, in order to improve the dispersibility and mutual affinity between the butadiene-propylene copolymer, PP, EVA, PS, filler and auxiliary agent as raw materials, so as to effectively improve the mechanical properties and achieve the purpose of improving flexibility, the butadiene-propylene copolymer used is a mixture of a high molecular weight butadiene-propylene copolymer with a molecular weight greater than 20,000 and a low molecular weight butadiene-propylene copolymer with a molecular weight less than 2,000 at a mass percentage of 32.5: 17.5. And the high molecular weight butadiene-propylene copolymer is obtained by grafting and modifying the base resin and the first active grafting monomer and the second active grafting monomer and has the first active group and the second active group. The low molecular weight butadiene-propylene copolymer is composed of the base resin grafted with the third active group. It should be mentioned that the first active group and the second active group are cross-linked with each other, the first active group and the third active group are cross-linked with each other, and the second active group and the third active group are cross-linked with each other.

[0048] Therefore, while the first active group and the second active group on the high molecular weight butadiene-propylene copolymer are cross-linked to form a ring structure, the first active group and the third active group, and the second active group and the third active group are cross-linked to form a cross-linked network space structure. On the premise of achieving effective mechanical improvement, the mixed combination with PP, EVA, PS, fillers and additives can achieve the effect of effectively improving flexibility.

[0049] In the third embodiment of the present application, the first reactive group is an isocyanate group, and the second reactive group is an amino group. Of course, the first reactive group and the second reactive group may also be other reactive groups that can cross-link with each other, and can cross-link with the third reactive group respectively, which will not be described in detail here. However, it is preferred that the isocyanate group is used as the first reactive group, and the amino group is used as the second reactive group.

[0050] Specifically, the third active group is an acyl chloride group. In the high molecular weight butadiene-propylene copolymer, the grafting modification is melt grafting modification, and the grafting rate of the first active group is 2%, and the grafting rate of the second active group is 1.4%. In the low molecular weight butadiene-propylene copolymer, the grafting modification is melt grafting modification, and the grafting rate is 5%.

[0051] Embodiment 4 The difference between Example 4 and Example 2 is that the auxiliary agent in Example 4 further includes 2 parts by weight of an antioxidant UV and 1.5 parts by weight of a lubricant.

[0052] Corresponding weight portions of compatibilizer, UV antioxidant and lubricant are simultaneously introduced into the mixed material.

[0053] Embodiment 5 The difference between Example 5 and Example 2 is that the additives in Example 5 further include 3 parts by weight of antioxidant UV, 2 parts of lubricant and 0.2 parts of white oil. White oil has the effect of color adjustment, improving reflection and increasing service life, and in the mixed molten part, the high molecular weight butadiene-propylene copolymer and the low molecular weight butadiene-propylene copolymer are first stirred and mixed for 16 minutes, then the white oil is added and stirred until completely absorbed, and finally PP, EVA, PS, filler and additives are added and stirred and mixed evenly.

[0054] Embodiment 6 The difference between Example 6 and Example 2 is that the additives in Example 6 also include 3.5 parts of antioxidant UV, 2.5 parts of lubricant and 1 part of white oil by weight. White oil has the effect of adjusting color, improving reflection and increasing service life, and in the mixed molten part, the high molecular weight butadiene-propylene copolymer and the low molecular weight butadiene-propylene copolymer are first stirred and mixed for 20 minutes, then the white oil is added and stirred until completely absorbed, and finally PP, EVA, PS, fillers and additives are added and stirred and mixed evenly.

[0055] Comparative Example 1 The difference between Comparative Example 1 and Example 2 is that the high molecular weight butadiene-propylene copolymer in Comparative Example 1 has only the first active group.

[0056] Comparative Example 2 The difference between Comparative Example 2 and Example 2 is that the high molecular weight butadiene-propylene copolymer in Comparative Example 2 has only the first active group, and the third active group is an amino group.

[0057] Comparative Example 3 The difference between Comparative Example 3 and Example 2 is that the first active group in Comparative Example 3 is a carboxyl group.

[0058] Comparative Example 4 The difference between Comparative Example 4 and Example 2 is that the second active group in Comparative Example 4 is a hydroxyl group.

[0059] Comparative Example 5 The difference between Comparative Example 5 and Example 2 is that the butadiene-propylene copolymer in Comparative Example 5 is a high molecular weight butadiene-propylene copolymer without the first active group and the second active group.

[0060] Comparative Example 6 The difference between Comparative Example 6 and Example 2 is that EVA is not added in Comparative Example 6.

[0061] Performance Testing: A flexible plastic sports field material experimental block is prepared by the preparation process of the flexible plastic sports field material of the above-mentioned Examples 1 to 6 and Comparative Examples 1 to 6. The flexible plastic sports field material experimental block has a thickness of 13 mm and is in a square shape of 6 cm×6 cm.

[0062] 1. Flexibility test, determined by elongation at break, in accordance with GB / T 10654-2001, definition 3.2; 2. Tensile strength test, judged by breaking strength, according to GB / T 10654-2001, definition 3.1; 3. Wear test: friction treatment is carried out using a wear tester, and the evaluations are given as excellent, good, poor, and relatively poor according to the degree and scope of damage; 4. Adhesion test: Use a tensile tester to test the tensile strength, and give excellent, good, poor, and relatively poor evaluations based on the tensile strength.

[0063] Table 1 Performance test results

[0064] As shown in Table 1 above, the cross-linking effect between the high molecular weight butadiene-propylene copolymer grafted with the first active group and the second active group and the low molecular weight butadiene-propylene copolymer grafted with the third active group is better than that of the high molecular weight butadiene-propylene copolymer lacking the first active group and / or the second active group in the preparation process. The obtained flexible plastic sports venue material has the effect of significantly improving flexibility, tensile strength, wear resistance and adhesion, especially when the grafting rate of the first active group and the second active group is between 0.8-2%, achieving effective wear resistance and high adhesion, thereby significantly extending the service life of the flexible plastic sports venue material prepared by the preparation process of the flexible plastic sports venue material. It should be mentioned that antioxidant UV, lubricant and white oil have certain side effects on the flexibility and tensile strength of the prepared flexible plastic sports venue material, but will achieve the effect of anti-oxidation and prolonging service life. At the same time, the combination of EVA and butadiene-propylene copolymer has a certain effect of improving flexibility.

[0065] In summary, the present application provides a preparation process for a flexible plastic sports field material, which solves the problem of insufficient mechanical strength and low flexibility caused by uneven dispersion between butadiene-propylene copolymer, PP, EVA, PS and filler through the mutual cross-linking reaction between the first active group and the second active group on the high molecular weight butadiene-propylene copolymer and the third active group on the low molecular weight butadiene-propylene copolymer. At the same time, since the butadiene-propylene copolymer is obtained by mixing a high molecular weight butadiene-propylene copolymer with a molecular weight greater than 20,000 and a low molecular weight butadiene-propylene copolymer with a molecular weight less than 2,000, the butadiene-propylene copolymer can achieve the effect of significantly improving flexibility and mechanical strength when further mixed with PP, EVA, PS and filler in corresponding proportions. In the selection of the first active group, the second active group and the third active group, innovative crosslinking and condensation reactions between isocyanate groups and amino groups, as well as crosslinking and condensation reactions between isocyanate groups and amino groups and hydroxyl groups, carboxyl groups, sulfonic acid groups or acyl chloride groups are used, so that the components form a stable structure after mixing, and form a stable and high-strength adhesion structure with the paved ground during laying, which plays a role in preventing detachment. In view of the fact that the flexible plastic sports field material is conventionally used outdoors, the auxiliary agent formed by the combination of compatibilizer, antioxidant UV and lubricant is selected to further improve the mixing uniformity and mutual compatibility between the components, and effectively improve the antioxidant property, thereby achieving the effect of extending the service life.

[0066] The "first", "second", "third", "fourth", etc. (if any) referred to in this application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments described herein can be implemented in an order other than that described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods or devices.

[0067] It should be noted that the descriptions involving "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.

[0068] Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A preparation process of a flexible plastic sports field material, Features: It includes raw material preparation part, mixing and melting part and extrusion granulation part; The raw material preparation part includes preparing butadiene-propylene copolymer, PP, EVA, PS, fillers and additives as raw materials; The mixed melting part comprises preliminarily stirring 40-50 parts by weight of a butadiene-propylene copolymer, adding 8-12 parts by weight of PP, 2-5 parts by weight of EVA, 4-7 parts by weight of PS, 26-32 parts by weight of a filler and 1.5-9 parts by weight of an auxiliary agent to the preliminarily stirred butadiene-propylene copolymer, continuing to stir to form a mixed material, and controlling the temperature of the mixed material to reach 78-82° C. before introducing the mixed material into a silo of an extruder; The extrusion granulation part includes using an extruder die head to extrude the molten mixture and an underwater pelletizer blade to cut to obtain material particles; The butadiene-propylene copolymer is formed by mixing a high molecular weight butadiene-propylene copolymer having a molecular weight greater than 20,000 and a low molecular weight butadiene-propylene copolymer having a molecular weight less than 2,000 in a mass percentage of 27.5-32.5:12.5-17.5; and the high molecular weight butadiene-propylene copolymer is obtained by grafting and modifying a base resin and a first active grafting monomer and a second active grafting monomer and has a first active group and a second active group; the low molecular weight butadiene-propylene copolymer is composed of a base resin grafted with a third active group; the first active group and the second active group are cross-linked with each other, the first active group and the third active group are cross-linked with each other, and the second active group and the third active group are cross-linked with each other.

2. A process for preparing a flexible plastic sports field material according to claim 1, Features: The first reactive group is an isocyanate group; the second reactive group is an amino group.

3. A process for preparing a flexible plastic sports field material according to claim 2, Features: The grafting modification is melt grafting modification, and the grafting rate is 0.1-2%.

4. A process for preparing a flexible plastic sports field material according to claim 1, Features: The third active group is a hydroxyl group, a carboxyl group, a sulfonic acid group or an acyl chloride group.

5. A process for preparing a flexible plastic sports field material according to claim 4, Features: The grafting modification is copolymerization or melt grafting modification, and the grafting rate is 1-5%.

6. A process for preparing a flexible plastic sports field material according to claim 1, Features: The auxiliary agent includes 1.5-2.5 parts by weight of a compatibilizer.

7. A process for preparing a flexible plastic sports field material according to claim 6, Features: The auxiliary agent also includes 2-3.5 parts by weight of an antioxidant UV, 1.5-2.5 parts by weight of a lubricant and 0-1 part by weight of white oil.

8. A process for preparing a flexible plastic sports field material according to claim 7, Features: In the mixed molten part, the high molecular weight butadiene-propylene copolymer and the low molecular weight butadiene-propylene copolymer are first stirred and mixed for 10-20 minutes, then white oil is added and stirred until completely absorbed, and finally PP, EVA, PS, fillers and additives are added.

9. The process for preparing a flexible plastic sports field material according to claim 1, Features: The number of die holes of the extruder is 20-40, the aperture is 2-3 mm, the rotation speed is 300-400 r / min, the feeding is 15 Hz, the current is 150 V, and the number of blades of the underwater pelletizer is 6, and the rotation speed is 360-420 r / min.

10. The process for preparing a flexible plastic sports field material according to claim 1, Features: The filler is calcium powder.

Citation Information

Patent Citations

  • Polybutylene terephthalate composite material and preparation method and application thereof

    CN103450647A

  • Waterborne polyurethane for plastic particle super-weather-resistant adhesive and preparation method of waterborne polyurethane

    CN116903824A

  • Plastic track surface layer coating material and preparation method thereof

    CN118165635A

  • Use of a thermoplastic elastomer composition to produce a flooring surface, and flooring surface

    WO2020212138A1

Cited By

  • Preparation process of flexible plastic sports field material

    CN120349576A