Butyl rubber waterproof roll as well as preparation method and application thereof
By adding specific additives and modified materials to the butyl rubber waterproof roll material, its waterproof, aging resistance and bonding properties are improved, and the aging performance and bonding problems in the existing technology are solved, thus achieving the extreme environment Highly efficient waterproofing effect.
Patent Information
- Application Number
- CN202411169602.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-24
- Publication Date
- 2024-11-12
AI Technical Summary
The aging performance and bonding performance of existing butyl rubber waterproof coils still need to be improved in extreme environments, and clear water affects the bonding during construction.
Using butyl rubber as the basic material, add stearic acid surface modified nanoscale calcium carbonate, carbon black, zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer and promoter, through specific formulas and Preparation method to improve waterproofing, aging resistance and bonding properties.
It has achieved excellent waterproofing performance, excellent aging resistance and excellent bonding performance of butyl rubber waterproof coils, which can effectively prevent moisture penetration in long-term water-soaked environments and underground projects and extend service life.
Smart Images

Figure BDA0005008844950000071 
Figure BDA0005008844950000081 
Figure BDA0005008844950000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of waterproofing coiled materials, and in particular to a butyl rubber waterproofing coiled material and a preparation method and application thereof. Background Art
[0002] Waterproof membrane is a rollable sheet-like waterproof material, mainly used in building walls, roofs, tunnels, roads, landfills, etc., to resist the seepage of external rainwater and groundwater. It is the first barrier to waterproofing the entire project and plays a vital role in the entire project.
[0003] At present, the waterproofing membranes on the market mainly include asphalt waterproofing membranes, polymer modified asphalt waterproofing membranes and synthetic polymer waterproofing membranes. Among them, asphalt waterproofing membranes, as traditional waterproofing membranes, are low in cost but have obvious performance shortcomings, such as low tensile strength and elongation, poor temperature stability, easy to flow at high temperatures, easy to crack at low temperatures, poor aging resistance, and short service life, which limits its application in high-quality projects. Polymer modified asphalt waterproofing membranes are modified by adding a certain proportion of synthetic polymers (such as SBS, APP, etc.) on the basis of traditional asphalt to improve the performance of asphalt. Compared with asphalt waterproofing membranes, polymer modified asphalt waterproofing membranes have improved tensile strength, heat resistance and low-temperature flexibility, and have better impermeability and corrosion resistance. However, the aging problem of this type of material in extreme environments still exists. Synthetic polymer waterproofing membranes are made of synthetic polymer materials, such as PVC, TPO, EPDM, etc. They do not contain asphalt components and rely on the characteristics of the polymer material itself to achieve the waterproof effect. They have higher chemical corrosion resistance, weather resistance, high and low temperature resistance and mechanical properties, and have a long service life.
[0004] As a type of synthetic polymer waterproofing membrane, butyl rubber waterproofing membrane has excellent air tightness and waterproofing effect, as well as good ozone resistance and chemical stability. Its good bonding properties and self-healing function solve the problem of overlapping treatment of traditional materials and simplify the construction process. However, the existing butyl rubber waterproofing membrane still faces some challenges, such as water leakage at the overlapping joints of waterproofing membranes; aging resistance still needs to be improved; when there is clear water on the construction surface, it will affect the bonding.
[0005] Therefore, there is an urgent need to develop a butyl rubber waterproof membrane with excellent waterproof performance, excellent aging resistance and excellent bonding performance. Summary of the invention
[0006] In order to solve at least one of the above technical problems, a butyl rubber waterproof membrane with excellent waterproof performance, excellent aging resistance and excellent bonding performance is developed. The present application provides a butyl rubber waterproof membrane and a preparation method and application thereof.
[0007] On the one hand, the present application provides a butyl rubber waterproofing membrane, whose raw material composition, measured by weight, includes: 70 to 90 parts of butyl rubber, 5 to 20 parts of stearic acid surface-modified nano-calcium carbonate, 10 to 20 parts of carbon black, 1 to 5 parts of zinc oxide, 2 to 10 parts of epoxy soybean oil acrylate, 0.5 to 3 parts of glucomannan, 0.1 to 1 parts of light stabilizer, 0.5 to 3 parts of accelerator, and 0.5 to 3 parts of antioxidant.
[0008] By adopting the above technical scheme, the present application adopts specific raw materials and formulas to obtain butyl rubber waterproofing coiled materials with excellent waterproof performance, excellent aging resistance and excellent bonding performance. The present application uses butyl rubber as the base material, which has excellent air tightness and water tightness, and good aging resistance. Adding stearic acid surface-modified nano-scale calcium carbonate can improve the physical strength and rigidity of the material, improve the fineness and waterproofness of the material, and enhance the aging resistance of the material; carbon black can improve the aging resistance of the material, and together with the light stabilizer, can effectively resist the damage of ultraviolet rays to the material.
[0009] The application adds epoxy soybean oil acrylate, which can improve the aging resistance of the material and enhance the bonding strength of the material; the addition of glucomannan can enhance the waterproof sealing performance of the waterproof membrane, improve the flexibility of the material, and enhance the stability.
[0010] Optionally, the raw material composition includes, by weight: 75-85 parts of butyl rubber, 10-15 parts of stearic acid surface modified nano-scale calcium carbonate, 12-18 parts of carbon black, 2-4 parts of zinc oxide, 4-8 parts of epoxy soybean oil acrylate, 1-2 parts of glucomannan, 0.3-0.7 parts of light stabilizer, 1-2 parts of accelerator, and 1-2 parts of antioxidant.
[0011] Optionally, the raw material composition includes, by weight: 80 parts of butyl rubber, 12 parts of stearic acid surface modified nano-scale calcium carbonate, 15 parts of carbon black, 3 parts of zinc oxide, 6 parts of epoxy soybean oil acrylate, 1.5 parts of glucomannan, 0.5 parts of light stabilizer, 1.5 parts of accelerator, and 1.5 parts of antioxidant.
[0012] Optionally, the content of stearic acid in the stearic acid surface-modified nano-scale calcium carbonate is 1% to 3%.
[0013] Optionally, the weight ratio of the epoxy soybean oil acrylate to glucomannan is 3 to 5:1.
[0014] By adopting the above technical solution, epoxy soybean oil acrylate is a polymer material with excellent flexibility and weather resistance, and glucomannan is a natural polysaccharide that can effectively improve the stability and biocompatibility of the material. The two are mixed in a specific ratio to achieve a balance between flexibility and stability, and improve the aging resistance of the material.
[0015] Optionally, the light stabilizer is selected from at least one of Tinuvin 770 and light stabilizer 2020.
[0016] By adopting the above technical solution, the light stabilizer of the present application can effectively absorb and quench ultraviolet energy, prevent the material from aging due to ultraviolet radiation, protect butyl rubber from damage by photochemical reactions, and improve aging resistance.
[0017] Optionally, the accelerator is selected from at least one of zinc diethyldithiocarbamate, 2-mercaptobenzothiazole and tetramethylthiuram disulfide.
[0018] Optionally, the antioxidant is selected from at least one of antioxidant A, antioxidant AW and antioxidant RD.
[0019] By adopting the above technical solution, the antioxidant of the present application can enhance the aging resistance of the waterproof membrane and extend its service life in harsh environments.
[0020] In a second aspect, the present application provides a method for preparing the above-mentioned butyl rubber waterproof membrane, comprising the following steps: S1, putting the butyl rubber, stearic acid surface modified nano-scale calcium carbonate and carbon black into an internal mixer, mixing and preparing a premix; S2, adding zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer, accelerator and antioxidant to the premix in sequence, mixing and kneading to obtain a rubber material; S3, extruding the rubber material into a sheet, laying a release paper on it and rolling it up to obtain a butyl rubber waterproofing roll.
[0021] By adopting the above technical solution, the preparation method adopted in this application has a simple process, convenient operation, improved production efficiency, reduced energy consumption and environmental protection. Step-by-step mixing helps dispersion and reduces the risk of large particle agglomeration.
[0022] On the third aspect, the present application provides the application of the above-mentioned butyl rubber waterproof membrane in long-term water immersion environments and underground projects.
[0023] By adopting the above technical solution, the butyl rubber waterproofing coiled material prepared in the present application has excellent waterproofing performance, excellent aging resistance, and excellent bonding performance. The coiled material can still maintain an excellent waterproof barrier to prevent water penetration during long-term immersion. Therefore, the butyl rubber waterproofing coiled material prepared in the present application can be used in long-term immersion environments and underground projects.
[0024] In summary, the present invention includes at least one of the following beneficial technical effects: 1. This application adopts specific raw materials and formulas to produce butyl rubber waterproof membrane with excellent waterproof performance, excellent aging resistance and excellent bonding performance.
[0025] 2. The application adds epoxy soybean oil acrylate, which can improve the aging resistance of the material and enhance the bonding strength of the material; the addition of glucomannan can enhance the waterproof sealing performance of the waterproof membrane.
[0026] 3. The preparation method adopted in this application has a simple process, is easy to operate, improves production efficiency, reduces energy consumption and is environmentally friendly. Step-by-step mixing helps dispersion and reduces the risk of large particle agglomeration. DETAILED DESCRIPTION
[0027] The present application is further described in detail below with reference to the embodiments.
[0028] The present application designs a butyl rubber waterproofing membrane, and its raw material composition includes, by weight: 70 to 90 parts of butyl rubber, 5 to 20 parts of stearic acid surface-modified nano-scale calcium carbonate, 10 to 20 parts of carbon black, 1 to 5 parts of zinc oxide, 2 to 10 parts of epoxy soybean oil acrylate, 0.5 to 3 parts of glucomannan, 0.1 to 1 parts of light stabilizer, 0.5 to 3 parts of accelerator, and 0.5 to 3 parts of antioxidant.
[0029] The butyl rubber waterproofing membrane of the present application is prepared by the following method, comprising the following steps: S1, putting the butyl rubber, stearic acid surface modified nano-scale calcium carbonate and carbon black into an internal mixer, mixing and preparing a premix; S2, adding zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer, accelerator and antioxidant to the premix in sequence, mixing and kneading to obtain a rubber material; S3, extruding the rubber material into a sheet, laying a release paper on it and rolling it up to obtain a butyl rubber waterproofing roll.
[0030] The butyl rubber waterproofing membrane of the present application can be used in long-term water immersion environments and underground projects.
[0031] The applicant has designed the technical solution of the present application in view of the problem that the waterproof performance and aging resistance of existing waterproof membranes still need to be improved.
[0032] The raw materials used in this application are as follows: Stearic acid: CAS: 57-11-4.
[0033] Nano-scale calcium carbonate: Foshan Bozhen Chemical Co., Ltd., product number: 2020728.
[0034] Butyl rubber: CAS: 9010-85-9.
[0035] Carbon black: CAS: 1333-86-4.
[0036] Zinc oxide: CAS: 1314-13-2.
[0037] Epoxidized soybean oil acrylate: Huainan Kedi Chemical Technology Co., Ltd.
[0038] Glucomannan: CAS: 11078-31-2.
[0039] Tinuvin 770: CAS: 52829-07-9.
[0040] Light Stabilizer 2020: CAS: 192268-64-7.
[0041] Zinc diethyldithiocarbamate: CAS: 14324-55-1.
[0042] 2-Mercaptobenzothiazole: CAS: 149-30-4.
[0043] Antioxidant AW: CAS: 5891-53-2.
[0044] Antioxidant RD: CAS: 26780-96-1. Specific embodiments
[0045] The preparation method of stearic acid surface-modified nano-scale calcium carbonate used in Examples 1 to 5 is: Step 1: dissolving stearic acid in ethanol to prepare a stearic acid solution; Step 2: Disperse nano-scale calcium carbonate in stearic acid solution, heat to 70° C., react for 1 hour, filter, wash, and dry to obtain stearic acid surface-modified nano-scale calcium carbonate.
[0046] Examples 1 to 5 Example 1 The present embodiment provides a butyl rubber waterproofing coiled material, and its raw material composition includes, by weight: 90 parts of butyl rubber, 5 parts of stearic acid surface-modified nano-scale calcium carbonate, 10 parts of carbon black, 1 part of zinc oxide, 10 parts of epoxy soybean oil acrylate, 3 parts of glucomannan, 0.1 parts of light stabilizer, 0.5 parts of accelerator, and 3 parts of antioxidant; The content of stearic acid in the stearic acid surface-modified nano-scale calcium carbonate is 3%; the light stabilizer is Tinuvin 770; the accelerator is zinc diethyldithiocarbamate; and the antioxidant is antioxidant AW.
[0047] The preparation method comprises the following steps: S1, putting butyl rubber, stearic acid surface modified nano-scale calcium carbonate and carbon black into an internal mixer, and mixing at 120° C. for 15 min to prepare a premix; S2, adding zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer, accelerator and antioxidant to the premix in sequence, and mixing at 100° C. for 30 minutes to obtain a rubber compound; S3, extruding the rubber into a sheet, laying a release paper and rolling it up to obtain a butyl rubber waterproofing membrane.
[0048] The butyl rubber waterproofing membrane prepared in this embodiment can be used in a long-term water immersion environment.
[0049] Example 2 The present embodiment provides a butyl rubber waterproofing coiled material, and its raw material composition includes, by weight: 75 parts of butyl rubber, 15 parts of stearic acid surface-modified nano-scale calcium carbonate, 18 parts of carbon black, 4 parts of zinc oxide, 4 parts of epoxy soybean oil acrylate, 1 part of glucomannan, 0.3 parts of light stabilizer, 2 parts of accelerator, and 1 part of antioxidant; The content of stearic acid in the stearic acid surface-modified nano-scale calcium carbonate is 3%; the light stabilizer is Tinuvin 770; the accelerator is zinc diethyldithiocarbamate; and the antioxidant is antioxidant AW.
[0050] The preparation method comprises the following steps: S1, putting butyl rubber, stearic acid surface modified nano-scale calcium carbonate and carbon black into an internal mixer, and mixing at 120° C. for 15 min to prepare a premix; S2, adding zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer, accelerator and antioxidant to the premix in sequence, and mixing at 100° C. for 30 minutes to obtain a rubber compound; S3, extruding the rubber into a sheet, laying a release paper and rolling it up to obtain a butyl rubber waterproofing membrane.
[0051] The butyl rubber waterproofing membrane prepared in this embodiment can be used in underground projects.
[0052] Example 3 The present embodiment provides a butyl rubber waterproofing coiled material, and its raw material composition includes, by weight: 80 parts of butyl rubber, 12 parts of stearic acid surface-modified nano-scale calcium carbonate, 15 parts of carbon black, 3 parts of zinc oxide, 6 parts of epoxy soybean oil acrylate, 1.5 parts of glucomannan, 0.5 parts of light stabilizer, 1.5 parts of accelerator, and 1.5 parts of antioxidant; The content of stearic acid in the stearic acid surface-modified nano-scale calcium carbonate is 3%; the light stabilizer is Tinuvin 770; the accelerator is zinc diethyldithiocarbamate; and the antioxidant is antioxidant AW.
[0053] The preparation method comprises the following steps: S1, putting butyl rubber, stearic acid surface modified nano-scale calcium carbonate and carbon black into an internal mixer, and mixing at 120° C. for 15 min to prepare a premix; S2, adding zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer, accelerator and antioxidant to the premix in sequence, and mixing at 100° C. for 30 minutes to obtain a rubber compound; S3, extruding the rubber into a sheet, laying a release paper and rolling it up to obtain a butyl rubber waterproofing membrane.
[0054] Example 4 The present embodiment provides a butyl rubber waterproofing coiled material, and its raw material composition includes, by weight: 85 parts of butyl rubber, 10 parts of stearic acid surface-modified nano-scale calcium carbonate, 12 parts of carbon black, 2 parts of zinc oxide, 8 parts of epoxy soybean oil acrylate, 2 parts of glucomannan, 0.7 parts of light stabilizer, 1 part of accelerator, and 2 parts of antioxidant; The content of stearic acid in the stearic acid surface-modified nano-scale calcium carbonate is 3%; the light stabilizer is Tinuvin 770; the accelerator is zinc diethyldithiocarbamate; and the antioxidant is antioxidant AW.
[0055] The preparation method comprises the following steps: S1, putting butyl rubber, stearic acid surface modified nano-scale calcium carbonate and carbon black into an internal mixer, and mixing at 120° C. for 15 min to prepare a premix; S2, adding zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer, accelerator and antioxidant to the premix in sequence, and mixing at 100° C. for 30 minutes to obtain a rubber compound; S3, extruding the rubber into a sheet, laying a release paper and rolling it up to obtain a butyl rubber waterproofing membrane.
[0056] Example 5 The present embodiment provides a butyl rubber waterproofing coiled material, and its raw material composition includes, by weight: 70 parts of butyl rubber, 20 parts of stearic acid surface-modified nano-scale calcium carbonate, 20 parts of carbon black, 5 parts of zinc oxide, 2 parts of epoxy soybean oil acrylate, 0.5 parts of glucomannan, 1 part of light stabilizer, 3 parts of accelerator, and 0.5 parts of antioxidant; The content of stearic acid in the stearic acid surface-modified nano-scale calcium carbonate is 3%; the light stabilizer is Tinuvin 770; the accelerator is zinc diethyldithiocarbamate; and the antioxidant is antioxidant AW.
[0057] The preparation method comprises the following steps: S1, putting butyl rubber, stearic acid surface modified nano-scale calcium carbonate and carbon black into an internal mixer, and mixing at 120° C. for 15 min to prepare a premix; S2, adding zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer, accelerator and antioxidant to the premix in sequence, and mixing at 100° C. for 30 minutes to obtain a rubber compound; S3, extruding the rubber into a sheet, laying a release paper and rolling it up to obtain a butyl rubber waterproofing membrane.
[0058] Comparative Examples 1 to 4 Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that in Comparative Example 1, stearic acid surface-modified nano-scale calcium carbonate is not added.
[0059] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is that epoxy soybean oil acrylate and glucomannan are not added in Comparative Example 2.
[0060] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that no epoxy soybean oil acrylate is added in Comparative Example 3.
[0061] Comparative Example 4 The difference between Comparative Example 4 and Example 3 is that no glucomannan is added in Comparative Example 4.
[0062] Experimental testing Test items and test methods Waterproof performance: According to GB 55030-2022 "General Specification for Waterproofing of Buildings and Municipal Engineering", the waterproofness of the lap joints of the butyl rubber waterproof membrane is tested.
[0063] Aging resistance: According to GB / T 16422.3-2014, the prepared butyl rubber waterproof membrane was subjected to an artificial climate aging test to observe whether there were cracks.
[0064] Adhesion performance: According to GB / T 328.23-2007 "Test methods for building waterproof membranes Part 23", the joint shear performance of butyl rubber waterproof membranes is tested; The seam peeling performance of butyl rubber waterproof membrane is tested according to GB / T 328.21-2007 "Test methods for building waterproof membranes Part 21".
[0065] The butyl rubber waterproof membranes prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were tested for lap seam impermeability, aging resistance, seam shear performance and seam peeling performance. The test results are shown in Table 1.
[0066] Table 1 From the test results in Table 1, it can be seen that the butyl rubber waterproof membranes prepared in Examples 1 to 5 are impermeable, have excellent waterproof performance, have no cracks after the artificial climate aging test, have excellent aging resistance, good shear performance and peeling performance, and therefore have excellent bonding performance.
[0067] In Comparative Example 1, no stearic acid surface-modified nano-scale calcium carbonate was added, and the aging resistance of the obtained butyl rubber waterproof membrane was inferior to that of Example 3.
[0068] In Comparative Example 2, epoxy soybean oil acrylate and glucomannan were not added, and the waterproof performance, aging resistance and bonding performance of the prepared butyl rubber waterproof membrane were significantly reduced.
[0069] In Comparative Example 3, no epoxy soybean oil acrylate was added, and the aging resistance and bonding strength of the prepared butyl rubber waterproof membrane were not as good as those in Example 3.
[0070] In Comparative Example 4, no glucomannan was added, and the waterproof performance of the prepared butyl rubber waterproof membrane was significantly reduced.
[0071] Embodiments 6 to 10 Example 6 The difference between Example 6 and Example 3 is that in Example 6, the weight ratio of epoxy soybean oil acrylate to glucomannan is 3:1, and the total weight of epoxy soybean oil acrylate and glucomannan is 7.5 parts.
[0072] Example 7 The difference between Example 7 and Example 3 is that in Example 7, the weight ratio of epoxy soybean oil acrylate to glucomannan is 5:1, and the total weight of epoxy soybean oil acrylate and glucomannan is 7.5 parts.
[0073] Example 8 The difference between Example 8 and Example 3 is that in Example 8, the light stabilizer is light stabilizer 2020.
[0074] Example 9 The difference between Example 9 and Example 3 is that in Example 9, the accelerator is 2-mercaptobenzothiazole.
[0075] Example 10 The difference between Example 10 and Example 3 is that in Example 10, the antioxidant is antioxidant RD.
[0076] The butyl rubber waterproof membranes prepared in Examples 6 to 10 were tested for lap seam impermeability, aging resistance, seam shear performance, and seam peeling performance. The test results are shown in Table 2.
[0077] Table 2 From the test results in Table 2, it can be seen that the difference between Example 6 and Example 7 and Example 3 is that the weight ratios of epoxy soybean oil acrylate and glucomannan are different. Among them, the butyl rubber waterproof membrane prepared in Example 3 has the best waterproof performance, aging resistance and bonding performance.
[0078] In Example 8, Example 9 and Example 10, different light stabilizers, accelerators and antioxidants are selected respectively, and the waterproof performance, aging resistance and bonding performance of the prepared butyl rubber waterproof membrane are similar to those of Example 3.
[0079] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A butyl rubber waterproofing coiled material, characterized in that: The raw materials include, by weight: 70-90 parts of butyl rubber, 5-20 parts of stearic acid surface-modified nano-scale calcium carbonate, 10-20 parts of carbon black, 1-5 parts of zinc oxide, 2-10 parts of epoxy soybean oil acrylate, 0.5-3 parts of glucomannan, 0.1-1 parts of light stabilizer, 0.5-3 parts of accelerator and 0.5-3 parts of antioxidant.
2. The butyl rubber waterproofing membrane according to claim 1, characterized in that: The raw material composition includes, by weight: 75-85 parts of butyl rubber, 10-15 parts of stearic acid surface modified nano-scale calcium carbonate, 12-18 parts of carbon black, 2-4 parts of zinc oxide, 4-8 parts of epoxy soybean oil acrylate, 1-2 parts of glucomannan, 0.3-0.7 parts of light stabilizer, 1-2 parts of accelerator, and 1-2 parts of antioxidant.
3. The butyl rubber waterproofing membrane according to claim 1, characterized in that: The raw materials include, by weight: 80 parts of butyl rubber, 12 parts of stearic acid surface-modified nano-scale calcium carbonate, 15 parts of carbon black, 3 parts of zinc oxide, 6 parts of epoxy soybean oil acrylate, 1.5 parts of glucomannan, 0.5 parts of light stabilizer, 1.5 parts of accelerator, and 1.5 parts of antioxidant.
4. The butyl rubber waterproofing membrane according to claim 1, characterized in that: The content of stearic acid in the stearic acid surface-modified nano-scale calcium carbonate is 1% to 3%.
5. The butyl rubber waterproofing membrane according to claim 1, characterized in that: The weight ratio of the epoxy soybean oil acrylate to glucomannan is 3-5:
1.
6. The butyl rubber waterproofing membrane according to claim 1, characterized in that: The light stabilizer is selected from at least one of Tinuvin 770 and light stabilizer 2020.
7. The butyl rubber waterproofing membrane according to claim 1, characterized in that: The accelerator is selected from at least one of zinc diethyldithiocarbamate, 2-mercaptobenzothiazole and tetramethylthiuram disulfide.
8. The butyl rubber waterproofing membrane according to claim 1, characterized in that: The antioxidant is selected from at least one of antioxidant A, antioxidant AW and antioxidant RD.
9. A method for preparing the butyl rubber waterproofing coiled material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, putting the butyl rubber, stearic acid surface modified nano-scale calcium carbonate and carbon black into an internal mixer, mixing and preparing a premix; S2, adding zinc oxide, epoxy soybean oil acrylate, glucomannan, light stabilizer, accelerator and antioxidant to the premix in sequence, mixing and kneading to obtain a rubber material; S3, extruding the rubber material into a sheet, laying a release paper on it and rolling it up to obtain a butyl rubber waterproofing roll.
10. Use of the butyl rubber waterproofing membrane according to any one of claims 1 to 8 in long-term water immersion environments and underground projects.