High-flame-retardant modified polystyrene material, preparation method thereof and household appliance shell
By using a combination of bromine and antimony flame retardant, silicate mineral and toughening agent in polystyrene materials, combined with the co-direction twin screw extrusion technology, the flame retardant properties of polystyrene materials are solved. , the problem of insufficient impact resistance and weather resistance has achieved efficient flame retardant modification and reduced production costs.
Patent Information
- Application Number
- CN202411118267.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
Polystyrene materials have poor flame retardant effects, high brittleness, poor weather resistance, and high cost or harmful raw materials used during the modification process, which limits their application in the fields of home appliance housing.
Using a combination of bromine flame retardant, antimony flame retardant and flame retardant synergist, combined with specific silicate minerals and a small amount of toughener are blended with polystyrene, and extruded by meshing co-direction twin screws. The machine is injection molded to improve its flame retardancy, impact resistance and weather resistance.
The flame retardant and impact resistance of polystyrene materials are significantly improved, combustion time is shortened, the residual flame existence time is reduced, the yellowing resistance of the material is enhanced, and production costs are reduced.
Smart Images

Figure CN118931059A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of general plastics, and in particular to a highly flame-retardant modified polystyrene material, a preparation method thereof, and a household appliance casing. Background Art
[0002] High-impact polystyrene (PS) refers to a polymer synthesized from styrene monomers through free radical polymerization. Polystyrene is easy to process and has the advantages of transparency, low cost, rigidity, insulation, good printability, etc. It can be widely used in the light industry market, daily decoration, lighting instructions and packaging. In terms of electricity, it is a good insulating material and heat insulation material, and can be used to make various instrument housings, lampshades, optical and chemical instrument parts, transparent films, capacitor dielectric layers, etc.
[0003] However, its brittleness and high flammability have limited its further application. Polystyrene is prone to stress cracking, and decomposes into styrene monomers, styrene dimers and hydrocarbons when exposed to fire. When polystyrene burns, it is easy to produce molten dripping with open flames, which can ignite other flammable materials. Even if the fire source is removed, it can continue to burn, so it is very easy to cause fire during stacking and construction. High-impact polystyrene needs to be added with flame retardants to achieve fire resistance. Usually, halogen compounds, phosphorus-containing compounds and inorganic flame retardants need to be added to enrich the flame retardant properties of styrene resin. Among them, halogen flame retardants, especially brominated flame retardants, are widely used to flame retard styrene resins due to their high flame retardant efficiency.
[0004] However, conventional flame-retardant and high-impact polystyrene has poor yellowing resistance, especially under light, the material is easy to decompose, and the flame retardant is easy to precipitate, resulting in a decrease in material performance and flame retardancy, limiting its application conditions. In addition, for styrene polymers, the flame retardant T3 does not meet the UL effect, so the material needs to be improved.
[0005] CN104974438A discloses a flame retardant polystyrene material and a preparation method thereof, which is made of the following components in parts by weight: 100 parts of polystyrene, 5-20 parts of polyethylene, 3-10 parts of organic montmorillonite, 10-25 parts of intumescent flame retardant, 2-6 parts of compatibilizer, 2-8 parts of polyvinyl butyral, and 1-3 parts of antioxidant. The present invention uses montmorillonite pretreated with hexadecyltrimethylammonium bromide and intumescent flame retardant in combination, and the intumescent flame retardant is optimized for the polystyrene composite material matrix and montmorillonite, and the mutual coordination effect improves the flame retardant efficiency of the polystyrene composite material. For polystyrene recycled materials, the poor impact resistance restricts the application field of recycled polystyrene materials. The traditional means of toughening polystyrene is mostly to add toughening agents containing styrene segments, such as SBS, SEBS, etc., but the prices of these toughening materials are generally high, and when used in recycled polystyrene materials, the cost of recycled materials will increase significantly.
[0006] CN116082782A discloses a weather-resistant flame-retardant styrene polymer, wherein the flame retardant used is ethyl-bis(tetrabromophthalimide) and EP-type brominated epoxy. Among them, EP-type brominated epoxy is a polymer synthesized by the reaction of tetrabromobisphenol A and epichlorohydrin. The composite material can significantly improve the aging resistance and precipitation resistance of the styrene polymer; however, a large amount of flame retardant needs to be added to the material, which reduces the mechanical properties of polystyrene. In addition, tetrabromobisphenol A is controlled by the EU ROHS and cannot be used, which makes it difficult to meet customer needs.
[0007] CN103509268A discloses an anti-aging flame retardant styrene resin composition, wherein the anti-aging performance can be effectively improved by adding ethylidene norbornene to the impact modifier. However, since ethylidene norbornene decomposes during storage, in order to prevent it from deteriorating, it is usually necessary to fill the storage container with high-purity inert gas and add an antioxidant, which is strict with the storage environment and dangerous.
[0008] CN112759851A discloses a flame retardant polystyrene composite material, wherein the flame retardant adopts phosphorus flame retardant and inorganic composite particles to synergistically enhance the flame retardancy and thermal conductivity, and at the same time, the flame retardant polystyrene composite material achieves a good balance in flame retardancy, thermal conductivity, processability and mechanical properties. However, the biggest defect of phosphorus and inorganic fillers is that they interfere with the performance of impact modifiers, and the cost of these two types of flame retardants has been high, which increases the cost of polystyrene resin and cannot achieve mass production.
[0009] In summary, polystyrene has poor flame retardant effect, high brittleness and poor weather resistance, and the raw materials used in the modification process of polystyrene are costly or harmful, or the amount of flame retardant added is large, which will reduce the impact resistance of polystyrene. Therefore, the poor impact resistance, flame retardancy and weather resistance of modified polystyrene are still problems that need to be solved urgently. Summary of the invention
[0010] In view of the above problems, the present invention provides a highly flame-retardant modified polystyrene material, a preparation method thereof and a household appliance casing, which improves the flame retardancy, impact resistance and weather resistance of polystyrene by combining a bromine-based flame retardant, an antimony-based flame retardant and a flame retardant synergist, and adding specific silicate minerals, a small amount of toughening agent and other additives to blend with polystyrene. The modified highly flame-retardant modified polystyrene material has a short burning time and a short afterflame existence time.
[0011] The present invention provides a highly flame-retardant modified polystyrene material, wherein the highly flame-retardant modified polystyrene material is obtained by injection molding a mixed masterbatch; The highly flame-retardant modified polystyrene material has a 25°C Izod notched impact strength of 95-100 J / m, a -30°C Izod notched impact strength of 50-80 J / m, a tensile strength of 20-30 MPa, a breaking strength of 30-40 MPa, and a yellowing resistance ΔE of 0.5-2.5; the highly flame-retardant modified polystyrene material has no surface cracking after the oil resistance test, and has a tensile strength of 18-25 MPa and a breaking strength of 28-35 MPa; The flame retardant property of the highly flame retardant modified polystyrene material is V0; the extinguishing time (T1) of the highly flame retardant modified polystyrene material after the first combustion is 10s is 0-3s; the extinguishing time (T2) of the highly flame retardant modified polystyrene material after the second combustion is 10s after the first combustion is extinguished is 0-3s; the afterflame existence time (T3) of the highly flame retardant modified polystyrene material after the second combustion is extinguished is 0-23s; The ball drop cracking test result of the highly flame retardant modified polystyrene material is 4-6 times; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a brominated flame retardant, an antimony flame retardant, a synergistic flame retardant, a silicate mineral, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant; The structure of the silicate mineral is: , where R1 is C1~C 20 R2 is one or more of an epoxy group, an amide group, an acrylic group and a silanol group; The silicate mineral is prepared from 50-80 parts by weight of silicate, 5-20 parts by weight of aromatic hydrocarbons, 5-20 parts by weight of silanol or epoxy resin or amide or acrylic acid, 0.1-5 parts by weight of cuprous bromide and 0.1-5 parts by weight of azobisisobutyronitrile (AIBN) are added into a reactor and reacted at 50-200° C. for 1-10 hours. After the reaction is completed, the mixture is filtered and washed with deionized water for 3-5 times to obtain the silicate mineral.
[0012] Furthermore, the components and contents in the mixed masterbatch are: Polystyrene: 60-100 parts by weight; Toughening agent: 3-8 parts by weight; Brominated flame retardant: 10-18 parts by weight; Antimony flame retardant: 1-5 parts by weight; Synergistic flame retardant: 1-5 parts by weight; Silicate minerals: 1-5 parts by weight; Antioxidant: 0.3-0.5 parts by weight; Lubricant: 0.3-0.5 parts by weight; Weathering agent: 0.5-0.8 parts by weight; Heat stabilizer: 0.1-0.3 parts by weight; Anti-dripping agent: 0.1-0.3 parts by weight; Colorant: 1-2 parts by weight.
[0013] Furthermore, the melt flow rate of the polystyrene is 3-10 g / min under the condition of 200° C. / 5 kg.
[0014] Furthermore, the toughening agent is one or more of styrene-butadiene block copolymer (SBS) and styrene-ethylene-butadiene-styrene copolymer (SEBS).
[0015] Furthermore, the brominated flame retardant is one or more of tetrabromobisphenol A, decabromodiphenylethane, bromotriazine and bis(2-ethylhexyl)tetrabromophthalate.
[0016] Furthermore, the antimony-based flame retardant is one or more of antimony oxychloride, antimony trioxide and colloidal antimony pentoxide.
[0017] Furthermore, the synergistic flame retardant is talcum powder.
[0018] Furthermore, the antioxidant is one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris[2,4-di-tert-butylphenyl]phosphite.
[0019] Furthermore, the lubricant is one or more of N,N-ethylene-bis-hard amide, silicone oil, white mineral oil and paraffin.
[0020] Furthermore, the weathering agent is one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine.
[0021] Furthermore, the heat stabilizer is dibasic lead stearate.
[0022] Furthermore, the anti-dripping agent is polytetrafluoroethylene.
[0023] Furthermore, the colorant is one or more of titanium dioxide, carbon black and ultramarine blue.
[0024] The present invention also provides a method for preparing the highly flame-retardant modified polystyrene material, wherein each component is weighed according to its content, and the preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, bromide flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant into a high-speed mixer after drying, stirring and mixing to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feeding port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, and pelletizing to obtain a mixed masterbatch; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the highly flame retardant modified polystyrene material.
[0025] Furthermore, the mass ratio of the polystyrene, toughening agent, brominated flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant in step 1 is (60-100): (3-8): (10-18): (1-5): (1-5): (1-5): (0.3-0.5): (0.3-0.5): (0.5-0.8): (0.1-0.3): (0.1-0.3): (1-2).
[0026] Furthermore, the melt flow rate of the polystyrene in step 1 is 3-10 g / min at 200° C. / 5 kg.
[0027] Furthermore, the toughening agent in step 1 is one or more of styrene-butadiene block copolymer (SBS) and styrene-ethylene-butadiene-styrene copolymer (SEBS).
[0028] Furthermore, the brominated flame retardant in step 1 is one or more of tetrabromobisphenol A, decabromodiphenylethane, bromotriazine and bis(2-ethylhexyl)tetrabromophthalate.
[0029] Furthermore, the antimony-based flame retardant in step 1 is one or more of antimony oxychloride, antimony trioxide and colloidal antimony pentoxide.
[0030] Furthermore, the synergistic flame retardant in step 1 is talcum powder.
[0031] Furthermore, the structure of the silicate mineral in step 1 is: , where R1 is C1~C 20 R2 is one or more of an epoxy group, an amide group, an acrylic group and a silanol group; The silicate mineral is prepared from 50-80 parts by weight of silicate, 5-20 parts by weight of aromatic hydrocarbons, 5-20 parts by weight of silanol or epoxy resin or amide or acrylic acid, 0.1-5 parts by weight of cuprous bromide and 0.1-5 parts by weight of azobisisobutyronitrile (AIBN) are added into a reactor and reacted at 50-200° C. for 1-10 hours. After the reaction is completed, the mixture is filtered and washed with deionized water for 3-5 times to obtain the silicate mineral.
[0032] Furthermore, the antioxidant in step 1 is one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and tris[2,4-di-tert-butylphenyl]phosphite.
[0033] Furthermore, the lubricant in step 1 is one or more of silicone oil, white mineral oil, barium stearate and paraffin.
[0034] Furthermore, the weathering agent in step 1 is one or more of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine.
[0035] Furthermore, the heat stabilizer in step 1 is dibasic lead stearate.
[0036] Furthermore, the anti-dripping agent in step 1 is polytetrafluoroethylene.
[0037] Furthermore, the colorant in step 1 is one or more of titanium dioxide, carbon black and ultramarine blue.
[0038] Furthermore, the drying temperature in step 1 is 80-100° C., and the drying time is 60-180 min.
[0039] Furthermore, in step 1, the stirring speed is 200-400 r / min, and the stirring time is 3-10 min.
[0040] Further, the processing temperature of the twin-screw extruder in the step 2 is 180-210°C, which is divided into twelve temperature zones, wherein the first temperature zone is 160-180°C, the second temperature zone is 180-210°C, the third temperature zone is 180-210°C, the fourth temperature zone is 180-210°C, the fifth temperature zone is 180-210°C, the sixth temperature zone is 180-210°C, the seventh temperature zone is 180-210°C, the eighth temperature zone is 190-200°C, the ninth temperature zone is 190-200°C, the tenth temperature zone is 190-200°C, the eleventh temperature zone is 190-200°C, and the twelfth temperature zone is 200-220°C.
[0041] Furthermore, the main engine speed of the twin-screw extruder in step 2 is 300-500rpm.
[0042] Furthermore, the aspect ratio of the twin-screw extruder in step 2 is 40:1.
[0043] Furthermore, the vacuum degree of the twin-screw extruder in step 2 is 1-3 MPa.
[0044] Furthermore, the main engine current of the twin-screw extruder in step 2 is 100-200A.
[0045] Furthermore, the torque of the twin-screw extruder in step 2 is 40-60 N·m.
[0046] Furthermore, the pellets of the mixed masterbatch in step 2 have a length of 3-4 mm and a diameter of 3-4 mm.
[0047] Furthermore, in step 2, the twin-screw extruder is co-directional, and the co-directional twin-screw extruder can generate higher shear stress, provide similar shear amount and thermal history, so that the mixed material is better dispersed in the twin-screw extruder; the co-directional twin-screw extruder can homogenize materials with different melt viscosities and different forms, so that they can be blended or interact with each other during the processing.
[0048] Furthermore, the mixed material in step 2 is fed through a main feeding port so that the mixed material is evenly dispersed in the twin-screw extruder, thereby preventing the mixed material from being incompletely mixed in the twin-screw extruder, resulting in unmelted material in the material and unstable performance.
[0049] Furthermore, after the toughening agent in the mixture in step 2 is blended with polystyrene at high temperature, the toughening agent will increase the distance between polystyrene molecules and form a network structure between the molecular chains of polystyrene, which will hinder the expansion of cracks when the material is impacted, thereby improving its impact resistance.
[0050] Furthermore, the brominated flame retardant in the mixture in step 2 decomposes at high temperature to generate bromine atoms, which react with polystyrene and toughening agent to generate hydrogen bromide, and hydrogen bromide reacts with highly active hydroxyl radicals or hydrogen atoms in the material to generate water or hydrogen, thereby interrupting the chain oxidation process, slowing down the combustion, and even stopping it. In addition, when the brominated flame retardant and the antimony flame retardant burn, volatile antimony chloride and antimony oxychloride are generated on the surface of the combustible, thereby absorbing heat, isolating oxygen and diluting the combustible, and playing a flame retardant role.
[0051] Furthermore, the silicate minerals in the mixture in step 2 have high silicon-oxygen bond energy and good thermal degradation stability, and the silicate minerals can generate a silicon-containing (mainly silicon dioxide) carbon layer under high temperature conditions. The Si-OH in the silicate minerals can also generate stable chemical bonds after being blended with antimony-based flame retardants, thereby enhancing flame retardancy. At the same time, -SiH3 can interact with the vinyl in polystyrene, and synergistically with the anti-dripping agent to improve the adhesion of the material during combustion, making it difficult for the combustible to drip. In addition, the R2 group of the silicate mineral can synergistically with the flame retardant to reduce the duration of the residual flame of the highly flame-retardant modified polystyrene material when the second combustion is extinguished.
[0052] Furthermore, the surface of the talcum powder in the mixture in step 2 has a protective oxide film, which can form a dense molten droplet under high temperature environment, effectively preventing the combustion of combustibles. At the same time, the thermal conductivity of talcum powder is very low, and it can form a heat insulation layer around the combustibles to slow down the combustion rate and inhibit the transfer of heat. It can also adhere to the surface of the combustibles to form a protective layer, forming physical isolation, which has a certain limiting effect on the contact between heat, oxygen and combustible substances.
[0053] Furthermore, the weathering agent in step 2 can absorb ultraviolet light and convert it into harmless heat energy, thereby achieving yellowing resistance. At the same time, the hydroxyl groups in the silicate minerals will adsorb the acidic substances in the highly flame-retardant modified polystyrene material, thereby preventing the material from yellowing.
[0054] Furthermore, in the step 3, the injection molding temperature of the injection molding machine is 100-300° C., the injection molding pressure is 100-200 MPa, and the injection molding speed is 10-30 mm / s.
[0055] Furthermore, in the step 3, the holding pressure of the injection molding machine is 10-30 MPa, the holding speed of the injection molding is 5-20, and the back pressure of the injection molding is 5-20 MPa.
[0056] The present invention also provides a household appliance shell, which is made of the highly flame-retardant modified polystyrene material.
[0057] Beneficial effects of the present invention: 1. Bromine-based flame retardants and toughening agents are added to the highly flame-retardant modified polystyrene material of the present invention, wherein the bromine-based flame retardant will generate bromine atoms under high temperature conditions, and the bromine atoms will generate hydrogen bromide with polystyrene, toughening agents, etc., and hydrogen bromide can generate water or hydrogen with hydroxyl groups or hydrogen atoms, thereby stopping combustion; in addition, antimony-based flame retardants and synergistic flame retardants are also added to the highly flame-retardant modified polystyrene material, wherein the antimony-based flame retardant and the bromine-based flame retardant will generate antimony chloride and antimony oxychloride during the mixing process, which absorb the heat during the combustion process, isolate the external oxygen, and play a flame retardant role, and the talcum powder in the synergistic flame retardant will form a layer of dense molten droplets during the mixing process with polystyrene, etc., and can also form a heat insulation layer around the combustibles, thereby preventing the combustion of the combustibles. The bromine-based flame retardant, antimony-based flame retardant and synergistic flame retardant work synergistically, so that the flame retardancy of the highly flame-retardant modified polystyrene material is significantly improved; 2. The flame retardancy of conventional polystyrene materials can only reach the point where the material is extinguished as soon as possible when ignited, but afterflames will still exist after extinguishment. In the present invention, silicate minerals are added, and the silicon-oxygen bond energy of silicate minerals is relatively high, so the thermal degradation stability is good. Moreover, silicate minerals can generate a silicon-containing (mainly silicon dioxide) carbon layer under high temperature conditions. Si-OH in silicate minerals can also generate stable chemical bonds after being blended with antimony flame retardants, thereby enhancing the flame retardancy. At the same time, SiH3 can interact with the vinyl in polystyrene, and synergistically improve the adhesion of the material during combustion with the anti-dripping agent, so that the combustible is not easy to drip. In addition, the R2 group of the silicate minerals can synergistically reduce the existence time of the afterflame of the highly flame-retardant modified polystyrene material after the second combustion is extinguished, so that the afterflame of the highly flame-retardant modified polystyrene material in the present invention is only 0-23s after being repeatedly ignited and extinguished, and can be extinguished as soon as possible, which is much better than the existing materials. 3. In addition to the flame retardant, the toughening agent in the highly flame-retardant modified polystyrene material of the present invention also improves the cantilever beam notch strength of the highly flame-retardant modified polystyrene material, and the cantilever beam notch strength at low temperature is also improved. In addition, a weathering agent is added to the highly flame-retardant modified polystyrene material, so that the highly flame-retardant modified polystyrene material does not yellow during use; 4. The highly flame-retardant modified polystyrene material described in the present invention is also added with antioxidants, lubricants, heat stabilizers and anti-dripping agents. After the oil resistance test, the highly flame-retardant modified polystyrene material prepared from the above raw materials has no significant change in mechanical properties and will not break. At the same time, it is also ensured that no droplets will fall during the combustion process of the material. In addition, the present invention uses a co-rotating twin-screw extruder for processing, which reduces the unstable performance of the material due to uneven mixing and the presence of unmelted materials in the material. At the same time, the co-rotating twin-screw extruder has excellent exhaust properties and low energy consumption, which improves the safety of the processing process and reduces the cost investment in the production process. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 ] are infrared spectra of the highly flame-retardant modified polystyrene material and the modified polystyrene material described in Example 1 and Comparative Example 1; Figure 2 It is a flame retardant performance diagram of the highly flame retardant modified polystyrene material and the modified polystyrene material described in Example 1 and Comparative Example 1; Figure 3 This is a test diagram of the oil corrosion resistance of the highly flame-retardant modified polystyrene material and the modified polystyrene material described in Examples 1-2 and Comparative Example 1; Figure 4 This is a graph showing the yellowing resistance of the highly flame retardant modified polystyrene material and the modified polystyrene material described in Example 1, Comparative Example 1 and Comparative Example 3. DETAILED DESCRIPTION
[0059] The invention is described in detail below with reference to the embodiments: The present invention provides a highly flame-retardant modified polystyrene material, a preparation method thereof and a home appliance casing. The polystyrene is modified by combining a bromine-based flame retardant, an antimony-based flame retardant and a flame retardant synergist, and adding silicate minerals, thereby greatly improving its weather resistance, flame retardancy, impact resistance and chemical resistance, thereby widely promoting the use of the highly flame-retardant modified polystyrene material.
[0060] Example 1 The present embodiment provides a highly flame-retardant modified polystyrene material, which is obtained by injection molding of a mixed masterbatch; the highly flame-retardant modified polystyrene material has a 25°C cantilever beam notched impact strength of 100 J / m, a -30°C cantilever beam notched impact strength of 50 J / m, a tensile strength of 28 MPa, a breaking strength of 35 MPa, and a yellowing resistance ΔE of 2.2; the highly flame-retardant modified polystyrene material has no cracking on its surface after an oil resistance test, and has a tensile strength of 24 MPa, a breaking strength of 32 MPa; the flame retardant property of the highly flame retardant modified polystyrene material is V0; the extinguishing time (T1) of the highly flame retardant modified polystyrene material after the first combustion is 10s is 2s; the extinguishing time (T2) of the highly flame retardant modified polystyrene material after the second combustion is continued for 10s after the first combustion is extinguished is 1s; the time (T3) of the residual flame of the highly flame retardant modified polystyrene material after the second combustion is extinguished is 1.7s; the falling ball cracking test result of the highly flame retardant modified polystyrene material is 6 times; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a brominated flame retardant, an antimony flame retardant, a synergistic flame retardant, a silicate mineral, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant; The structure of the silicate mineral is: , wherein R1 is a C6 phenyl group, and R2 is an epoxy group; The silicate mineral is prepared from 50 parts by weight of silicate, 5 parts by weight of aromatic hydrocarbons, and 5 parts by weight of epoxy resin, with the addition of 0.2 parts by weight of cuprous bromide and 0.1 parts by weight of azobisisobutyronitrile (AIBN), which are added into a reactor and reacted at 120° C. for 10 hours. After the reaction is completed, the mixture is filtered and washed three times with deionized water to obtain the silicate mineral.
[0061] In this embodiment, the polystyrene is 80 parts by weight, and the melt flow rate of the polystyrene is 5 g / min at 200°C / 5kg; The toughening agent is 5 parts by weight of styrene-butadiene block copolymer (SBS); The brominated flame retardant is 6 parts by weight of decabromodiphenylethane and 6 parts by weight of bromotriazine; The antimony flame retardant is 3.6 parts by weight of antimony trioxide; The synergistic flame retardant is 4 parts by weight of talc; The silicate mineral is 1 part by weight; The antioxidant is 0.2 parts by weight of pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 0.3 parts by weight of tris [2,4-di-tert-butylphenyl] phosphite; The lubricant is 0.3 parts by weight of N,N-ethylene-bis-hard amide; The weathering agent is 0.3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.4 parts by weight of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine; The thermal stabilizer is 0.2 parts by weight of dibasic lead stearate; The anti-dripping agent is 0.15 parts by weight of polytetrafluoroethylene; The colorant is 1 part by weight of titanium dioxide.
[0062] This embodiment also provides a method for preparing the highly flame-retardant modified polystyrene material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, brominated flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant to a high-speed mixer at a stirring speed of 300 r / min after drying at 80° C. for 60 min, and stirring for 5 min to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feed port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, pelletizing to obtain a mixed masterbatch with a length of 3.6 mm and a diameter of 3.2 mm; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the highly flame retardant modified polystyrene material.
[0063] The temperature of the twin-screw extruder in this embodiment is 180-210°C, and the twin-screw extruder is divided into twelve temperature zones, wherein the first temperature zone is 180°C, the second temperature zone is 200°C, the third temperature zone is 200°C, the fourth temperature zone is 200°C, the fifth temperature zone is 200°C, the sixth temperature zone is 200°C, the seventh temperature zone is 200°C, the eighth temperature zone is 190°C, the ninth temperature zone is 190°C, the tenth temperature zone is 190°C, the eleventh temperature zone is 190°C, and the twelfth temperature zone is 210°C; the screw speed of the twin-screw extruder is 300rpm; the aspect ratio of the twin-screw extruder is 40:1, the vacuum degree is 1MPa, the host current is 200A, and the torque is 40N·m.
[0064] In this embodiment, the injection molding temperature of the injection molding machine is 200°C, the injection molding pressure is 135MPa, the injection molding speed is 16mm / s, the injection holding pressure of the injection molding machine is 20MPa, the injection holding speed is 10, and the injection back pressure is 10MPa.
[0065] Example 2 The present embodiment provides a highly flame-retardant modified polystyrene material, which is obtained by injection molding of a mixed masterbatch; the highly flame-retardant modified polystyrene material has a 25°C cantilever beam notched impact strength of 100 J / m, a -30°C cantilever beam notched impact strength of 44 J / m, a tensile strength of 27 MPa, a breaking strength of 35 MPa, and a yellowing resistance ΔE of 0.8; the highly flame-retardant modified polystyrene material has no cracking on its surface after an oil resistance test, and has a tensile strength of 24 MPa, a breaking strength of 3 0MPa; the flame retardant property of the highly flame retardant modified polystyrene material is V0; the extinguishing time (T1) of the highly flame retardant modified polystyrene material after the first combustion is 1s after 10s; the extinguishing time (T2) of the highly flame retardant modified polystyrene material after the second combustion is 10s after the first combustion is extinguished is 1s; the time (T3) of the residual flame of the highly flame retardant modified polystyrene material after the second combustion is extinguished is 0s; the falling ball cracking test result of the highly flame retardant modified polystyrene material is 5 times; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a brominated flame retardant, an antimony flame retardant, a synergistic flame retardant, a silicate mineral, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant; The structure of the silicate mineral is: , wherein R1 is a C6 phenyl group, and R2 is an epoxy group; The silicate mineral is prepared from 50 parts by weight of silicate, 5 parts by weight of aromatic hydrocarbons, and 5 parts by weight of epoxy resin, with the addition of 0.2 parts by weight of cuprous bromide and 0.1 parts by weight of azobisisobutyronitrile (AIBN), which are added into a reactor and reacted at 120° C. for 10 hours. After the reaction is completed, the mixture is filtered and washed three times with deionized water to obtain the silicate mineral.
[0066] In this embodiment, the polystyrene is 80 parts by weight, and the melt flow rate of the polystyrene is 5 g / min at 200°C / 5kg; The toughening agent is 5 parts by weight of styrene-butadiene block copolymer (SBS); The brominated flame retardant is 6 parts by weight of decabromodiphenylethane and 6 parts by weight of bromotriazine; The antimony flame retardant is 3.6 parts by weight of antimony trioxide; The synergistic flame retardant is 4 parts by weight of talc; The silicate mineral is 3 parts by weight; The antioxidant is 0.2 parts by weight of pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 0.3 parts by weight of tris [2,4-di-tert-butylphenyl] phosphite; The lubricant is 0.3 parts by weight of N,N-ethylene-bis-hard amide; The weathering agent is 0.3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.4 parts by weight of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine; The thermal stabilizer is 0.2 parts by weight of dibasic lead stearate; The anti-dripping agent is 0.15 parts by weight of polytetrafluoroethylene; The colorant is 1 part by weight of titanium dioxide.
[0067] This embodiment also provides a method for preparing the highly flame-retardant modified polystyrene material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, brominated flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant to a high-speed mixer at a stirring speed of 400 r / min after drying at 90° C. for 100 min, and stirring for 5 min to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feed port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, pelletizing to obtain a mixed masterbatch with a length of 3.6 mm and a diameter of 3.2 mm; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the highly flame retardant modified polystyrene material.
[0068] The temperature of the twin-screw extruder in this embodiment is 180-210°C, and the twin-screw extruder is divided into twelve temperature zones, wherein the first temperature zone is 180°C, the second temperature zone is 200°C, the third temperature zone is 200°C, the fourth temperature zone is 200°C, the fifth temperature zone is 200°C, the sixth temperature zone is 200°C, the seventh temperature zone is 200°C, the eighth temperature zone is 190°C, the ninth temperature zone is 190°C, the tenth temperature zone is 190°C, the eleventh temperature zone is 190°C, and the twelfth temperature zone is 210°C; the screw speed of the twin-screw extruder is 300rpm; the aspect ratio of the twin-screw extruder is 40:1, the vacuum degree is 1MPa, the host current is 200A, and the torque is 40N·m.
[0069] In this embodiment, the injection molding temperature of the injection molding machine is 200°C, the injection molding pressure is 135MPa, the injection molding speed is 16mm / s, the injection holding pressure of the injection molding machine is 20MPa, the injection holding speed is 10, and the injection back pressure is 10MPa.
[0070] Example 3 The present embodiment provides a highly flame-retardant modified polystyrene material, which is obtained by injection molding of a mixed masterbatch; the highly flame-retardant modified polystyrene material has a 25°C cantilever beam notched impact strength of 100 J / m, a -30°C cantilever beam notched impact strength of 45 J / m, a tensile strength of 27 MPa, a breaking strength of 35 MPa, and a yellowing resistance ΔE of 1.0; the highly flame-retardant modified polystyrene material has no cracking on its surface after an oil resistance test, and has a tensile strength of 26 MPa and a breaking strength of 3 3MPa; the flame retardant performance of the highly flame retardant modified polystyrene material is V0; the extinguishing time (T1) of the highly flame retardant modified polystyrene material after the first combustion is 10s is 2s; the extinguishing time (T2) of the highly flame retardant modified polystyrene material after the second combustion is continued for 10s after the first combustion is extinguished is 3s; the time (T3) of the residual flame of the highly flame retardant modified polystyrene material after the second combustion is extinguished is 23s; the falling ball cracking test result of the highly flame retardant modified polystyrene material is 5 times; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a brominated flame retardant, an antimony flame retardant, a synergistic flame retardant, a silicate mineral, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant; The structure of the silicate mineral is: , wherein R1 is a C6 phenyl group, and R2 is an epoxy group; The silicate mineral is prepared from 50 parts by weight of silicate, 5 parts by weight of aromatic hydrocarbons, and 5 parts by weight of epoxy resin, with the addition of 0.2 parts by weight of cuprous bromide and 0.1 parts by weight of azobisisobutyronitrile (AIBN), which are added into a reactor and reacted at 120° C. for 10 hours. After the reaction is completed, the mixture is filtered and washed three times with deionized water to obtain the silicate mineral.
[0071] In this embodiment, the polystyrene is 80 parts by weight, and the melt flow rate of the polystyrene is 5 g / min at 200°C / 5kg; The toughening agent is 3 parts by weight of styrene-butadiene block copolymer (SBS); The brominated flame retardant is 5 parts by weight of decabromodiphenylethane and 5 parts by weight of bromotriazine; The antimony flame retardant is 3.6 parts by weight of antimony trioxide; The synergistic flame retardant is 4 parts by weight of talc; The silicate mineral is 3 parts by weight; The antioxidant is 0.2 parts by weight of pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 0.3 parts by weight of tris [2,4-di-tert-butylphenyl] phosphite; The lubricant is 0.3 parts by weight of N,N-ethylene-bis-hard amide; The weathering agent is 0.3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.4 parts by weight of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine; The thermal stabilizer is 0.2 parts by weight of dibasic lead stearate; The anti-dripping agent is 0.15 parts by weight of polytetrafluoroethylene; The colorant is 1 part by weight of titanium dioxide.
[0072] This embodiment also provides a method for preparing the highly flame-retardant modified polystyrene material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, brominated flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant to a high-speed mixer at a stirring speed of 350 r / min after drying at 100° C. for 120 min, stirring for 5 min to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feed port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, pelletizing to obtain a mixed masterbatch with a length of 3.6 mm and a diameter of 3.2 mm; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the highly flame retardant modified polystyrene material.
[0073] The temperature of the twin-screw extruder in this embodiment is 180-210°C, and the twin-screw extruder is divided into twelve temperature zones, wherein the first temperature zone is 180°C, the second temperature zone is 200°C, the third temperature zone is 200°C, the fourth temperature zone is 200°C, the fifth temperature zone is 200°C, the sixth temperature zone is 200°C, the seventh temperature zone is 200°C, the eighth temperature zone is 190°C, the ninth temperature zone is 190°C, the tenth temperature zone is 190°C, the eleventh temperature zone is 190°C, and the twelfth temperature zone is 210°C; the screw speed of the twin-screw extruder is 300rpm; the aspect ratio of the twin-screw extruder is 40:1, the vacuum degree is 1MPa, the host current is 200A, and the torque is 40N·m.
[0074] In this embodiment, the injection molding temperature of the injection molding machine is 200°C, the injection molding pressure is 135MPa, the injection molding speed is 16mm / s, the injection holding pressure of the injection molding machine is 20MPa, the injection holding speed is 10, and the injection back pressure is 10MPa.
[0075] Example 4 The present embodiment provides a highly flame-retardant modified polystyrene material, which is obtained by injection molding of a mixed masterbatch; the highly flame-retardant modified polystyrene material has a 25°C cantilever beam notched impact strength of 100 J / m, a -30°C cantilever beam notched impact strength of 45 J / m, a tensile strength of 27 MPa, a breaking strength of 35 MPa, and a yellowing resistance ΔE of 1.0; the highly flame-retardant modified polystyrene material has no cracking on its surface after an oil resistance test, and has a tensile strength of 25 MPa and a breaking strength of 3 3MPa; the flame retardant performance of the highly flame retardant modified polystyrene material is V0; the extinguishing time (T1) of the highly flame retardant modified polystyrene material after the first combustion is 10s is 3s; the extinguishing time (T2) of the highly flame retardant modified polystyrene material after the second combustion is continued for 10s after the first combustion is extinguished is 2s; the time (T3) of the residual flame of the highly flame retardant modified polystyrene material after the second combustion is extinguished is 20s; the falling ball cracking test result of the highly flame retardant modified polystyrene material is 5 times; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a brominated flame retardant, an antimony flame retardant, a synergistic flame retardant, a silicate mineral, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant; The structure of the silicate mineral is: , wherein R1 is a C6 phenyl group, and R2 is an epoxy group; The silicate mineral is prepared from 50 parts by weight of silicate, 5 parts by weight of aromatic hydrocarbons, and 5 parts by weight of epoxy resin, with the addition of 0.2 parts by weight of cuprous bromide and 0.1 parts by weight of azobisisobutyronitrile (AIBN), which are added into a reactor and reacted at 120° C. for 10 hours. After the reaction is completed, the mixture is filtered and washed three times with deionized water to obtain the silicate mineral.
[0076] In this embodiment, the polystyrene is 80 parts by weight, and the melt flow rate of the polystyrene is 5 g / min at 200°C / 5kg; The toughening agent is 3 parts by weight of styrene-butadiene block copolymer (SBS); The brominated flame retardant is 5 parts by weight of decabromodiphenylethane and 5 parts by weight of bromotriazine; The antimony flame retardant is 2 parts by weight of antimony trioxide; The synergistic flame retardant is 2 parts by weight of talc; The silicate mineral is 5 parts by weight; The antioxidant is 0.2 parts by weight of pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 0.3 parts by weight of tris [2,4-di-tert-butylphenyl] phosphite; The lubricant is 0.3 parts by weight of N,N-ethylene-bis-hard amide; The weathering agent is 0.3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.4 parts by weight of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine; The thermal stabilizer is 0.2 parts by weight of dibasic lead stearate; The anti-dripping agent is 0.15 parts by weight of polytetrafluoroethylene; The colorant is 1 part by weight of titanium dioxide.
[0077] This embodiment also provides a method for preparing the highly flame-retardant modified polystyrene material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, brominated flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant to a high-speed mixer at a stirring speed of 350 r / min after drying at 100° C. for 120 min, stirring for 5 min to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feed port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, pelletizing to obtain a mixed masterbatch with a length of 3.6 mm and a diameter of 3.2 mm; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the highly flame retardant modified polystyrene material.
[0078] The temperature of the twin-screw extruder in this embodiment is 180-210°C, and the twin-screw extruder is divided into twelve temperature zones, wherein the first temperature zone is 180°C, the second temperature zone is 200°C, the third temperature zone is 200°C, the fourth temperature zone is 200°C, the fifth temperature zone is 200°C, the sixth temperature zone is 200°C, the seventh temperature zone is 200°C, the eighth temperature zone is 190°C, the ninth temperature zone is 190°C, the tenth temperature zone is 190°C, the eleventh temperature zone is 190°C, and the twelfth temperature zone is 210°C; the screw speed of the twin-screw extruder is 300rpm; the aspect ratio of the twin-screw extruder is 40:1, the vacuum degree is 1MPa, the host current is 200A, and the torque is 40N·m.
[0079] In this embodiment, the injection molding temperature of the injection molding machine is 200°C, the injection molding pressure is 135MPa, the injection molding speed is 16mm / s, the injection holding pressure of the injection molding machine is 20MPa, the injection holding speed is 10, and the injection back pressure is 10MPa.
[0080] Comparative Example 1 The comparative example provides a modified polystyrene material, which is obtained by injection molding of a mixed masterbatch; the modified polystyrene material has a 25°C notched cantilever beam impact strength of 65 J / m, a -30°C notched cantilever beam impact strength of 40 J / m, a tensile strength of 27 MPa, a fracture strength of 30 MPa, and a yellowing resistance ΔE of 3.8; the surface of the modified polystyrene material cracks after an oil resistance test, and the tensile strength is 18 MPa and the fracture strength is 10 MPa; the extinguishing time (T1) of the modified polystyrene material after the first combustion is 1 s after 10 s; the extinguishing time (T2) of the modified polystyrene material after the second combustion is continued for 10 s after the first combustion is extinguished is 1 s; the afterflame existence time (T3) of the modified polystyrene material after the second combustion is extinguished is 35 s; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a brominated flame retardant, an antimony flame retardant, a synergistic flame retardant, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant.
[0081] In this comparative example, the polystyrene is 80 parts by weight, and the melt flow rate of the polystyrene is 5 g / min at 200°C / 5kg; The toughening agent is 5 parts by weight of styrene-butadiene block copolymer (SBS); The brominated flame retardant is 8 parts by weight of decabromodiphenylethane and 6 parts by weight of bromotriazine; The antimony flame retardant is 3.6 parts by weight of antimony trioxide; The synergistic flame retardant is 4 parts by weight of talc; The antioxidant is 0.2 parts by weight of pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 0.3 parts by weight of tris [2,4-di-tert-butylphenyl] phosphite; The lubricant is 0.3 parts by weight of N,N-ethylene-bis-hard amide; The weathering agent is 0.3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.4 parts by weight of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine; The thermal stabilizer is 0.2 parts by weight of dibasic lead stearate; The anti-dripping agent is 0.15 parts by weight of polytetrafluoroethylene; The colorant is 1 part by weight of titanium dioxide.
[0082] This comparative example also provides a method for preparing the modified polystyrene material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, brominated flame retardant, antimony flame retardant, synergistic flame retardant, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant to a high-speed mixer at a stirring speed of 300 r / min after drying at 80° C. for 60 min, and stirring for 5 min to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feed port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, pelletizing to obtain a mixed masterbatch with a length of 3.6 mm and a diameter of 3.2 mm; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the modified polystyrene material.
[0083] The temperature of the twin-screw extruder in this comparative example is 180-210°C, and the twin-screw extruder is divided into twelve temperature zones, wherein the first temperature zone is 180°C, the second temperature zone is 200°C, the third temperature zone is 200°C, the fourth temperature zone is 200°C, the fifth temperature zone is 200°C, the sixth temperature zone is 200°C, the seventh temperature zone is 200°C, the eighth temperature zone is 190°C, the ninth temperature zone is 190°C, the tenth temperature zone is 190°C, the eleventh temperature zone is 190°C, and the twelfth temperature zone is 210°C; the screw speed of the twin-screw extruder is 300rpm; the aspect ratio of the twin-screw extruder is 40:1, the vacuum degree is 1MPa, the host current is 200A, and the torque is 40N·m.
[0084] In this comparative example, the injection molding temperature of the injection molding machine is 200°C, the injection molding pressure is 135MPa, the injection molding speed is 16mm / s, the injection molding holding pressure of the injection molding machine is 20MPa, the injection molding holding speed is 10, and the injection molding back pressure is 10MPa.
[0085] like Figure 1 The infrared spectra of the highly flame retardant modified polystyrene material and the modified polystyrene material in Example 1 and Comparative Example 1 are shown in FIG. 1. Compared with Comparative Example 1, Example 1 has a higher infrared spectroscopy value at 1371.4 cm -1 ±0.01cm -1 The absorption peak at 638.14 cm is weakened because the amount of brominated flame retardant added in Example 1 is small and the absorption peak at 638.14 cm is -1 ±0.01cm -1 and 610.37cm -1 ±0.01cm -1 An absorption peak relative to silicate minerals appears.
[0086] like Figure 2 The flame retardant performance diagram of the highly flame retardant modified polystyrene material and the modified polystyrene material in Example 1 and Comparative Example 1 is shown. It can be seen from the figure that the highly flame retardant modified polystyrene material in this embodiment disappears after the second combustion is extinguished, while the modified polystyrene material in Comparative Example 1 still has an afterflame after the second combustion is extinguished.
[0087] like Figure 3 Shown is the oil corrosion resistance test diagram of the highly flame retardant modified polystyrene material and the modified polystyrene material described in the present embodiment 1-2 and the comparative example 1. As shown in the figure, the highly flame retardant modified polystyrene material in the present embodiment 1-2 did not crack after the oil corrosion resistance test, while the modified polystyrene material in the comparative example 1 cracked.
[0088] Comparative Example 2 The comparative example provides a modified polystyrene material, which is obtained by injection molding of a mixed masterbatch; the modified polystyrene material has a 25°C notched cantilever beam impact strength of 75 J / m, a -30°C notched cantilever beam impact strength of 40 J / m, a tensile strength of 28 MPa, a fracture strength of 30 MPa, and a yellowing resistance ΔE of 2.0; the modified polystyrene material has no surface cracking after an oil resistance test, and has a tensile strength of 18 MPa and a fracture strength of 10 MPa; the extinguishing time (T1) of the modified polystyrene material after the first combustion is 10 seconds is 4 seconds; the extinguishing time (T2) of the modified polystyrene material after the second combustion is continued for 10 seconds after the first combustion is extinguished is 4 seconds; the afterflame existence time (T3) of the modified polystyrene material after the second combustion is extinguished is 12 seconds; The mixed masterbatch is prepared by mixing polystyrene, polyphenylene ether, a toughening agent, a phosphorus flame retardant, an antimony flame retardant, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant.
[0089] In this embodiment, the polystyrene is 60 parts by weight, and the melt flow rate of the polystyrene is 5 g / min at 200°C / 5kg; The polyphenylene ether is 20 parts by weight; The toughening agent is 5 parts by weight of styrene-butadiene block copolymer (SBS); The phosphorus-based flame retardant is 12 parts by weight of 1,3-phenylene tetrakis(2,6-dimethylphenyl)phosphate; The antimony flame retardant is 3.6 parts by weight of antimony trioxide; The antioxidant is 0.2 parts by weight of pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 0.3 parts by weight of tris [2,4-di-tert-butylphenyl] phosphite; The lubricant is 0.3 parts by weight of N,N-ethylene-bis-hard amide; The weathering agent is 0.3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.4 parts by weight of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine; The thermal stabilizer is 0.2 parts by weight of dibasic lead stearate; The anti-dripping agent is 0.15 parts by weight of polytetrafluoroethylene; The colorant is 1 part by weight of titanium dioxide.
[0090] This comparative example also provides a method for preparing the modified polystyrene material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, adding polystyrene, polyphenylene ether, toughening agent, phosphorus flame retardant, antimony flame retardant, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant to a high-speed mixer at a stirring speed of 300 r / min after drying at 80° C. for 60 minutes, and stirring for 5 minutes to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feed port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, pelletizing to obtain a mixed masterbatch with a length of 3.6 mm and a diameter of 3.2 mm; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the modified polystyrene material.
[0091] The temperature of the twin-screw extruder in this comparative example is 180-210°C, and the twin-screw extruder is divided into twelve temperature zones, wherein the first temperature zone is 180°C, the second temperature zone is 200°C, the third temperature zone is 200°C, the fourth temperature zone is 200°C, the fifth temperature zone is 200°C, the sixth temperature zone is 200°C, the seventh temperature zone is 200°C, the eighth temperature zone is 190°C, the ninth temperature zone is 190°C, the tenth temperature zone is 190°C, the eleventh temperature zone is 190°C, and the twelfth temperature zone is 210°C; the screw speed of the twin-screw extruder is 300rpm; the aspect ratio of the twin-screw extruder is 40:1, the vacuum degree is 1MPa, the host current is 200A, and the torque is 40N·m.
[0092] In this comparative example, the injection molding temperature of the injection molding machine is 200°C, the injection molding pressure is 135MPa, the injection molding speed is 16mm / s, the injection molding holding pressure of the injection molding machine is 20MPa, the injection molding holding speed is 10, and the injection molding back pressure is 10MPa.
[0093] Comparative Example 3 The comparative example provides a modified polystyrene material, which is obtained by injection molding of a mixed masterbatch; the modified polystyrene material has a 25°C notched cantilever beam impact strength of 70 J / m, a -30°C notched cantilever beam impact strength of 40 J / m, a tensile strength of 29 MPa, a fracture strength of 30 MPa, and a yellowing resistance ΔE of 4.3; the modified polystyrene material has no surface cracking after an oil resistance test, and has a tensile strength of 15 MPa and a fracture strength of 8 MPa; the extinguishing time (T1) of the modified polystyrene material after the first combustion is 10 seconds is 2 seconds; the extinguishing time (T2) of the modified polystyrene material after the second combustion is continued for 10 seconds after the first combustion is extinguished is 2 seconds; the afterflame existence time (T3) of the modified polystyrene material after the second combustion is extinguished is 30 seconds; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a brominated flame retardant, a phosphorus flame retardant, an antimony flame retardant, a flame retardant synergist, a silicate mineral, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant; The structure of the silicate mineral is: , wherein R1 is a C6 phenyl group, and R2 is an epoxy group; The silicate mineral is prepared from 50 parts by weight of silicate, 5 parts by weight of aromatic hydrocarbons, and 5 parts by weight of epoxy resin, with the addition of 0.2 parts by weight of cuprous bromide and 0.1 parts by weight of azobisisobutyronitrile (AIBN), which are added into a reactor and reacted at 120° C. for 10 hours. After the reaction is completed, the mixture is filtered and washed three times with deionized water to obtain the silicate mineral.
[0094] In this comparative example, the polystyrene is 80 parts by weight, and the melt flow rate of the polystyrene is 5 g / min at 200°C / 5kg; The toughening agent is 5 parts by weight of styrene-butadiene block copolymer (SBS); The brominated flame retardant is 11 parts by weight of decabromodiphenylethane; The phosphorus-based flame retardant is 8 parts by weight of 1,3-phenylene tetrakis(2,6-dimethylphenyl)phosphate; The antimony flame retardant is 3.6 parts by weight of antimony trioxide; The synergistic flame retardant is 4 parts by weight of talc; The silicate mineral is 5 parts by weight; The antioxidant is 0.2 parts by weight of pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 0.3 parts by weight of tris [2,4-di-tert-butylphenyl] phosphite; The lubricant is 0.3 parts by weight of N,N-ethylene-bis-hard amide; The weathering agent is 0.3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.4 parts by weight of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine; The thermal stabilizer is 0.2 parts by weight of dibasic lead stearate; The anti-dripping agent is 0.15 parts by weight of polytetrafluoroethylene; The colorant is 1 part by weight of titanium dioxide.
[0095] This comparative example also provides a method for preparing the modified polystyrene material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, bromide flame retardant, phosphorus flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant to a high-speed mixer at a stirring speed of 300 r / min after drying at 80° C. for 60 min, and stirring for 5 min to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feed port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, pelletizing to obtain a mixed masterbatch with a length of 3.6 mm and a diameter of 3.2 mm; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the modified polystyrene material.
[0096] The temperature of the twin-screw extruder in this comparative example is 180-210°C, and the twin-screw extruder is divided into twelve temperature zones, wherein the first temperature zone is 180°C, the second temperature zone is 200°C, the third temperature zone is 200°C, the fourth temperature zone is 200°C, the fifth temperature zone is 200°C, the sixth temperature zone is 200°C, the seventh temperature zone is 200°C, the eighth temperature zone is 190°C, the ninth temperature zone is 190°C, the tenth temperature zone is 190°C, the eleventh temperature zone is 190°C, and the twelfth temperature zone is 210°C; the screw speed of the twin-screw extruder is 300rpm; the aspect ratio of the twin-screw extruder is 40:1, the vacuum degree is 1MPa, the host current is 200A, and the torque is 40N·m.
[0097] In this comparative example, the injection molding temperature of the injection molding machine is 200°C, the injection molding pressure is 135MPa, the injection molding speed is 16mm / s, the injection molding holding pressure of the injection molding machine is 20MPa, the injection molding holding speed is 10, and the injection molding back pressure is 10MPa.
[0098] like Figure 4 It is a yellowing resistance performance diagram of the highly flame retardant modified polystyrene materials described in Example 1, Comparative Example 1 and Comparative Example 3. It can be seen from the figure that the highly flame retardant modified polystyrene material in Example 1 did not turn yellow after 500 hours of ultraviolet light irradiation, while the modified polystyrene materials in Comparative Example 1 and Comparative Example 3 all turned yellow.
[0099] Comparative Example 4 The comparative example provides a modified polystyrene material, which is obtained by injection molding of a mixed masterbatch; the modified polystyrene material has a 25°C notched cantilever beam impact strength of 65 J / m, a -30°C notched cantilever beam impact strength of 40 J / m, a tensile strength of 25 MPa, a fracture strength of 20 MPa, and a yellowing resistance ΔE of 3.6; the modified polystyrene material has no surface cracking after an oil resistance test, and has a tensile strength of 15 MPa and a fracture strength of 5 MPa; the extinguishing time (T1) of the modified polystyrene material after the first combustion is 1 s after 10 s; the extinguishing time (T2) of the modified polystyrene material after the second combustion is continued for 10 s after the first combustion is extinguished is 1 s; the afterflame existence time (T3) of the modified polystyrene material after the second combustion is extinguished is 46 s; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a halogen flame retardant, an antimony flame retardant, a synergistic flame retardant, a silicate mineral, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant; The structure of the silicate mineral is: , wherein R1 is a C6 phenyl group, and R2 is an epoxy group; The silicate mineral is prepared from 50 parts by weight of silicate, 5 parts by weight of aromatic hydrocarbons, and 5 parts by weight of epoxy resin, with the addition of 0.2 parts by weight of cuprous bromide and 0.1 parts by weight of azobisisobutyronitrile (AIBN), which are added into a reactor and reacted at 120° C. for 10 hours. After the reaction is completed, the mixture is filtered and washed three times with deionized water to obtain the silicate mineral.
[0100] In this comparative example, the polystyrene is 80 parts by weight, and the melt flow rate of the polystyrene is 5 g / min at 200°C / 5kg; The toughening agent is 5 parts by weight of styrene-butadiene block copolymer (SBS); The 5.6 parts by weight of ethylbis(tetrabromophthalimide) and 8.4 parts by weight of EP type brominated epoxy resin; The EP type brominated epoxy resin has a bromine content of 46-50wt%, a molecular weight of 800, and a specific gravity of 1.8g / cm 3 , softening point temperature is 65-75℃; The antimony flame retardant is 2 parts by weight of antimony trioxide; The synergistic flame retardant is 2 parts by weight of talc; The silicate mineral is 5 parts by weight; The antioxidant is 0.2 parts by weight of pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and 0.3 parts by weight of tris [2,4-di-tert-butylphenyl] phosphite; The lubricant is 0.3 parts by weight of N,N-ethylene-bis-hard amide; The weathering agent is 0.3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and 0.4 parts by weight of poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine; The thermal stabilizer is 0.2 parts by weight of dibasic lead stearate; The anti-dripping agent is 0.15 parts by weight of polytetrafluoroethylene; The colorant is 1 part by weight of titanium dioxide.
[0101] This comparative example also provides a method for preparing the modified polystyrene material. Each component is weighed according to its content. The preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, halogen flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant to a high-speed mixer at a stirring speed of 300 r / min after drying at 80° C. for 60 minutes, and stirring for 5 minutes to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feed port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, pelletizing to obtain a mixed masterbatch with a length of 3.6 mm and a diameter of 3.2 mm; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the modified polystyrene material.
[0102] The temperature of the twin-screw extruder in this comparative example is 180-210°C, and the twin-screw extruder is divided into twelve temperature zones, wherein the first temperature zone is 180°C, the second temperature zone is 200°C, the third temperature zone is 200°C, the fourth temperature zone is 200°C, the fifth temperature zone is 200°C, the sixth temperature zone is 200°C, the seventh temperature zone is 200°C, the eighth temperature zone is 190°C, the ninth temperature zone is 190°C, the tenth temperature zone is 190°C, the eleventh temperature zone is 190°C, and the twelfth temperature zone is 210°C; the screw speed of the twin-screw extruder is 300rpm; the aspect ratio of the twin-screw extruder is 40:1, the vacuum degree is 1MPa, the host current is 200A, and the torque is 40N·m.
[0103] In this comparative example, the injection molding temperature of the injection molding machine is 200°C, the injection molding pressure is 135MPa, the injection molding speed is 16mm / s, the injection molding holding pressure of the injection molding machine is 20MPa, the injection molding holding speed is 10, and the injection molding back pressure is 10MPa.
[0104] Based on the above, it can be seen that the highly flame-retardant modified polystyrene material described in this patent has a wide range of applications, low cost, and extremely high market prospects.
[0105] The above description is only a preferred embodiment of the present invention and does not constitute any other form of limitation to the present invention. Any modification or equivalent change made based on the technical essence of the present invention still falls within the scope of protection required by the present invention.
[0106] Table 1 shows the components and their contents in Examples 1-4.
[0107] Table 2 shows the components and their contents in Comparative Examples 1-4.
[0108] Antioxidant 1010 in Table 1 and Table 2 is pentaerythritol [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, antioxidant 168 is tris[2,4-di-tert-butylphenyl] phosphite, UV770 is bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and UV944 is poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-bis[(2,2,6,6,-tetramethyl-piperidinyl)]}imine.
[0109] Table 3 shows the performance test of the modified polystyrene materials described in Examples 1-4 and Comparative Examples 1-4.
[0110] As shown in Table 3, the highly flame-retardant modified polystyrene materials described in Examples 1-4 of the present invention have high impact strength at both room temperature and low temperature, and can maintain high tensile strength and breaking strength after the oil resistance test. At the same time, the highly flame-retardant modified polystyrene materials in the present invention have good yellowing resistance and flame retardancy, especially flame retardancy, and can maintain the existence time of the residual flame at 0-23s after the second combustion is extinguished; while in Comparative Example 1, no silicate minerals are added, and its mechanical properties and yellowing resistance are reduced, and after cracking occurs on the surface of the material after the oil resistance test, and the flame retardancy is also significantly reduced; Comparative Example 1 In Example 2, polyphenylene ether is added, and phosphorus flame retardants and antimony flame retardants are used for modification. The burning time of its flame retardancy is significantly prolonged, and the nature of polyphenylene ether is unstable, and yellowing will occur during the injection molding process; in Comparative Example 3, bromine flame retardants, antimony flame retardants, phosphorus flame retardants and synergistic flame retardants are used for combination, but its flame retardancy is still poor; in Comparative Example 4, ethyl bis(tetrabromophthalimide) and EP type brominated epoxy resin are used for modification, and the bromine content is low. In order to achieve the same effect, a large amount needs to be added, resulting in a landslide decline in the overall performance of the material, resulting in failure to meet the performance of the product.
[0111] The cantilever beam notched impact strength test, tensile strength and breaking strength test in the present invention meet the standard "ASTM D256", and the size of the sample is 127*64*3.2mm; the flame retardant performance test meets the standard of "UL94" vertical combustion, and the sample is tested in the DPK-310 horizontal vertical combustion tester of De Rui Ke during the test, and the sample size is 125*13*1.5mm; the yellowing resistance test conditions are: put the sample into 340nm, 0.89W / m 2 The test cycle is 500 hours in the UV aging instrument. After completion, the surface color difference of the sample is tested with a standard colorimeter and compared with the initial value to calculate the color difference value △E of the sample. The conditions of the falling ball cracking test are: the ball weight is 1kg and the falling ball height is 1m.
Claims
1. A highly flame retardant modified polystyrene material, It is characterized in that The highly flame-retardant modified polystyrene material is obtained by injection molding of a mixed masterbatch; The highly flame-retardant modified polystyrene material has a 25°C Izod notched impact strength of 95-100 J / m, a -30°C Izod notched impact strength of 50-80 J / m, a tensile strength of 20-30 MPa, a breaking strength of 30-40 MPa, and a yellowing resistance ΔE of 0.5-2.5; the highly flame-retardant modified polystyrene material has no surface cracking after the oil resistance test, and has a tensile strength of 18-25 MPa and a breaking strength of 28-35 MPa; The flame retardant property of the highly flame retardant modified polystyrene material is V0; the extinguishing time of the highly flame retardant modified polystyrene material after the first combustion is 10s is 0-3s; the extinguishing time of the highly flame retardant modified polystyrene material after the second combustion is 10s after the first combustion is extinguished is 0-3s; the afterflame of the highly flame retardant modified polystyrene material after the second combustion is extinguished is 0-23s; The ball drop cracking test result of the highly flame retardant modified polystyrene material is 4-6 times; The mixed masterbatch is prepared by mixing polystyrene, a toughening agent, a brominated flame retardant, an antimony flame retardant, a synergistic flame retardant, a silicate mineral, an antioxidant, a lubricant, a weathering agent, a heat stabilizer, an anti-dripping agent and a colorant; The structure of the silicate mineral is: , where R 1 C 1 ~C 20 One of the phenyl groups, R 2 It is one or more of epoxy group, amide group, acrylic group and silanol group; The silicate mineral is prepared from 50-80 parts by weight of silicate, 5-20 parts by weight of aromatic hydrocarbons, 5-20 parts by weight of silanol or epoxy resin or amide or acrylic acid, 0.1-5 parts by weight of cuprous bromide and 0.1-5 parts by weight of azobisisobutyronitrile are added to a reactor and reacted at 50-200° C. for 1-10 hours. After the reaction is completed, the mixture is filtered and washed with deionized water for 3-5 times to obtain the silicate mineral.
2. The highly flame retardant modified polystyrene material according to claim 1, It is characterized in that The components and contents in the mixed masterbatch are: Polystyrene: 60-100 parts by weight; Toughening agent: 3-8 parts by weight; Brominated flame retardant: 10-18 parts by weight; Antimony flame retardant: 1-5 parts by weight; Synergistic flame retardant: 1-5 parts by weight; Silicate minerals: 1-5 parts by weight; Antioxidant: 0.3-0.5 parts by weight; Lubricant: 0.3-0.5 parts by weight; Weathering agent: 0.5-0.8 parts by weight; Heat stabilizer: 0.1-0.3 parts by weight; Anti-dripping agent: 0.1-0.3 parts by weight; Colorant: 1-2 parts by weight.
3. The highly flame retardant modified polystyrene material according to claim 1, It is characterized in that The brominated flame retardant is one or more of tetrabromobisphenol A, decabromodiphenylethane, bromotriazine and bis(2-ethylhexyl)tetrabromophthalate.
4. The highly flame retardant modified polystyrene material according to claim 1, It is characterized in that The synergistic flame retardant is talc.
5. A method for preparing the highly flame-retardant modified polystyrene material according to any one of claims 1 to 4, It is characterized in that Each component is weighed according to its content, and the preparation method comprises the following steps: Step 1, adding polystyrene, toughening agent, bromide flame retardant, antimony flame retardant, synergistic flame retardant, silicate mineral, antioxidant, lubricant, weathering agent, heat stabilizer, anti-dripping agent and colorant into a high-speed mixer after drying, stirring and mixing to obtain a mixture; Step 2, adding the mixed material into the twin-screw extruder through the main feeding port of the meshing co-directional twin-screw extruder, after melt mixing and extrusion, water cooling to room temperature and then naturally air drying, and pelletizing to obtain a mixed masterbatch; Step 3: placing the mixed masterbatch into an injection molding machine for injection molding to obtain the highly flame retardant modified polystyrene material.
6. The method for preparing the highly flame-retardant modified polystyrene material according to claim 5, It is characterized in that The processing temperature of the twin-screw extruder in the step 2 is 180-210°C, which is divided into twelve temperature zones, wherein the first temperature zone is 160-180°C, the second temperature zone is 180-210°C, the third temperature zone is 180-210°C, the fourth temperature zone is 180-210°C, the fifth temperature zone is 180-210°C, the sixth temperature zone is 180-210°C, the seventh temperature zone is 180-210°C, the eighth temperature zone is 190-200°C, the ninth temperature zone is 190-200°C, the tenth temperature zone is 190-200°C, the eleventh temperature zone is 190-200°C, and the twelfth temperature zone is 200-220°C.
7. The method for preparing the highly flame-retardant modified polystyrene material according to claim 5, It is characterized in that The aspect ratio of the twin-screw extruder in step 2 is 40:
1.
8. The method for preparing the highly flame-retardant modified polystyrene material according to claim 5, It is characterized in that The pellets of the mixed masterbatch in step 2 have a length of 3-4 mm and a diameter of 3-4 mm.
9. The method for preparing the highly flame-retardant modified polystyrene material according to claim 5, It is characterized in that In the step 3, the injection molding temperature of the injection molding machine is 100-300° C., the injection molding pressure is 100-200 MPa, and the injection molding speed is 10-30 mm / s.
10. A housing for household appliances, It is characterized in that The housing of the household appliance is made of the highly flame-retardant modified polystyrene material according to any one of claims 1 to 4.
Citation Information
Patent Citations
Anti-aging flame-retardant styrene resin composition
CN103509268A
Flame retardant polystyrene material and preparation method thereof
CN104974438A
Flame-retardant polystyrene composite material as well as preparation method and application thereof
CN112759851A
Weather-resistant flame-retardant styrene polymer
CN116082782A