Antistatic modifier, preparation method of antistatic modifier, antistatic modified nylon and preparation method of antistatic modified nylon

By mixing the composite of polystyrene sulfonate with cationic surfactant with nylon to form antistatic modified nylon, the existing antistatic technology has solved the problem of poor effect in low humidity environments and difficulty in industrial production, and achieved the The excellent antistatic and durability of nylon materials are suitable for large-scale production.

CN118931061APending Publication Date: 2024-11-12CHANGCHUN INSTITUTE OF APPLIED CHEMISTRY CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202411174592.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing antistatic technology has poor effect in low humidity environments and is difficult to achieve long-term preservation and large-scale industrial production. In particular, the polyamide antistatic method has complex operation and is unstable.

Method used

The polystyrene sodium sulfonate-surfactant composite formed by combining sodium polystyrene sulfonate and cationic surfactant is used as an antistatic modifier. The antistatic modified nylon is formed by mixing with nylon and melting extruding. , significantly improve antistatic efficiency and durability.

Benefits of technology

This method achieves excellent antistatic and durability of nylon materials, high temperature resistance, avoids high temperature decomposition, simplifies the preparation process, is suitable for large-scale continuous production, and is pollution-free to the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005010363530000071
    Figure BDA0005010363530000071
  • Figure BDA0005010363530000081
    Figure BDA0005010363530000081
Patent Text Reader

Abstract

The invention relates to the technical field of nylon, in particular to an antistatic modifier, a preparation method of the antistatic modifier, antistatic modified nylon and a preparation method of the antistatic modified nylon. The antistatic modifier provided by the invention is a sodium polystyrenesulfonate-surfactant compound formed by combining sodium polystyrenesulfonate and a cationic surfactant. The antistatic modifier provided by the invention is good in compatibility with a nylon matrix, uniform in dispersion, not easy to separate out, good in antistatic property and lasting in antistatic property, and the antistatic efficiency can be remarkably improved; in addition, the antistatic modifier is resistant to high temperature, so that side reactions such as high-temperature decomposition in the process of preparing the antistatic material can be avoided, and the problem of antistatic property inactivation is further avoided; in addition, the preparation method of the antistatic modifier is simple and easy to implement, has no pollution to the environment, and is easy to realize large-scale continuous production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nylon, and in particular to an antistatic modifier, a preparation method thereof, antistatic modified nylon and a preparation method thereof. Background Art

[0002] The phenomenon of static electricity is mainly caused by friction (contact-separation) or induction of objects. After static electricity is generated, like charges repel each other and opposite charges attract each other, causing static interference in production and life. In life, dust with opposite charges will adhere to the surface of fabrics due to static electricity. When the top and pants are made of different materials, charges of different polarities attract each other, resulting in the phenomenon of clothes entangled with each other and clothes entangled with the human body. Fibers with amide bonds such as wool, nylon, and artificial hair tend to be positively charged, while polyester, polyacrylonitrile, etc. tend to be negatively charged. The charging phenomenon generated by fiber friction is caused by the movement of charges between the rubbed fibers. The amount of charge accumulated on the surface of the polymer depends on the nature of the polymer itself to discharge the charge. The main discharge methods are: surface conduction, bulk conduction, and radiation to the surrounding air, with surface conduction as the main way. Because the surface conductivity is generally greater than the volume conductivity, the static electricity on the surface of the polymer material is mainly dominated by the surface conductivity of the polymer. The accumulation of static electricity can be prevented by increasing the surface conductivity or volume conductivity of the polymer to discharge the polymer material quickly.

[0003] The existing polyamide antistatic technologies include: (1) hydrophilic treatment with surfactants to improve the hygroscopicity of the material, thereby reducing its resistivity and accelerating the dissipation of charge. This method is simple to operate, but its antistatic effect is difficult to preserve for a long time, and its antistatic performance is poor in low-humidity environments. (2) Development and utilization of conductive fiber technology. Conductive fibers have stable performance, excellent effects, and are not restricted by climatic conditions. They are the most promising method, but due to the physical and mechanical processing involved, they are currently limited by process conditions and the possibility of large-scale industrial production is very small. (3) Polymers are blended, copolymerized or grafted to introduce hydrophilic polar groups to prepare antistatic fibers. This method is achieved by blending hydrophilic polymers with resin matrix in the form of alloys, or by polymerization with the matrix, uniformly and finely dispersing them into linear or mesh-like "conductive channels". Therefore, this method is a major method currently used to develop permanent antistatic polymers. Summary of the invention

[0004] In view of this, the object of the present invention is to provide an antistatic modifier, a preparation method thereof, antistatic modified nylon and a preparation method thereof. The antistatic modifier provided by the present invention can make nylon have excellent antistatic properties and good antistatic durability.

[0005] The invention provides an antistatic modifier, which is a sodium polystyrene sulfonate-surfactant complex formed by combining sodium polystyrene sulfonate with a cationic surfactant.

[0006] Preferably, the number average molecular weight of the sodium polystyrene sulfonate is 2,000 to 200,000.

[0007] Preferably, the cationic surfactant is selected from one or more of quaternary ammonium salt type, quaternary phosphonium salt type and guanidine type.

[0008] Preferably, the molecular weight of the cationic surfactant is 50-3000.

[0009] Preferably, the mass ratio of the sodium polystyrene sulfonate to the cationic surfactant is 1:(0.1-2).

[0010] The present invention provides a method for preparing the antistatic modifier described in the above technical solution, comprising the following steps:

[0011] The sodium polystyrene sulfonate aqueous solution is mixed with the cationic surfactant aqueous solution to form a water-insoluble sodium polystyrene sulfonate-surfactant complex.

[0012] Preferably, the mass percentage concentration of the sodium polystyrene sulfonate aqueous solution is 0.1-5%; the mass percentage concentration of the cationic surfactant aqueous solution is 0.1-5%.

[0013] The present invention provides an antistatic modified nylon, the components of the antistatic modified nylon include: an antistatic modifier and nylon;

[0014] The antistatic modifier is the antistatic modifier described in the above technical solution or the antistatic modifier prepared by the preparation method described in the above technical solution;

[0015] The mass percentage of the antistatic modifier in the antistatic modified nylon is 1-10%.

[0016] Preferably, the nylon includes one or more of nylon 6, nylon 6 elastomer, nylon 66, nylon 66 elastomer, nylon 11, nylon 11 elastomer, nylon 12, nylon 12 elastomer, nylon 610, nylon 610 elastomer, nylon 612 and nylon 612 elastomer.

[0017] The present invention provides a method for preparing the antistatic modified nylon described in the above technical solution, comprising the following steps:

[0018] The antistatic modifier is mixed with nylon and melt-extruded to obtain antistatic modified nylon.

[0019] Compared with the prior art, the present invention provides an antistatic modifier, a preparation method thereof, antistatic modified nylon and a preparation method thereof. The antistatic modifier provided by the present invention is a sodium polystyrene sulfonate-surfactant complex formed by combining sodium polystyrene sulfonate with a cationic surfactant. The antistatic modifier provided by the present invention has good compatibility with the nylon matrix, is evenly dispersed, is not easy to precipitate, has good antistatic properties and long-lasting antistatic performance, and can significantly improve the antistatic efficiency; in addition, the antistatic modifier is resistant to high temperatures, which can avoid side reactions such as high-temperature decomposition during the preparation of antistatic materials, thereby avoiding the problem of antistatic inactivation; in addition, the preparation method of the antistatic modifier is simple and easy, has no pollution to the environment, and is easy to achieve large-scale continuous production. The test results show that the antistatic modifier provided by the present invention can make the initial antistatic property of nylon reach 3.5x10 7 Ω, the sample was placed in a constant temperature and humidity chamber at 60±2℃ and 95±2% for 96 hours, and the resistance data was tested again. The antistatic property remained at 4.8x10 8 Ω, showing excellent antistatic properties and antistatic persistence. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The invention provides an antistatic modifier, which is a sodium polystyrene sulfonate-surfactant complex formed by combining sodium polystyrene sulfonate with a cationic surfactant.

[0022] In the antistatic modifier provided by the present invention, the number average molecular weight of the sodium polystyrene sulfonate is preferably 2000-200000, specifically 2000, 5000, 8000, 10000, 20000, 50000, 80000, 100000 or 200000.

[0023] In the antistatic modifier provided by the present invention, the cationic surfactant is preferably selected from one or more of quaternary ammonium salt type, quaternary phosphonium salt type and guanidine type, and the molecular weight is preferably 50 to 3000, and more preferably 50 to 1000. In the present invention, the quaternary ammonium salt type cationic surfactant is preferably one or more of quaternary ammonium salt type cationic surfactants of C12 to C18, and more preferably one or more of quaternary ammonium salt type cationic surfactants of C16 to C18; the quaternary phosphonium salt type cationic surfactant is preferably one or more of tributyl n-hexyl phosphonium bromide, tributyl n-octyl phosphonium bromide, tributyl dodecyl phosphonium bromide and tributyl hexadecyl phosphonium bromide, and more preferably tributyl hexadecyl phosphonium bromide; the guanidine type cationic surfactant is preferably one or more of C5 to C20 alkylguanidine cationic surfactants and substituted C4 to C22 alkylguanidine cationic surfactants, and the number average molecular weight of the guanidine type cationic surfactant is more preferably 150 to 3000.

[0024] In the antistatic modifier provided by the present invention, the mass ratio of the sodium polystyrene sulfonate to the cationic surfactant is preferably 1:(0.1-2), more preferably 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2.

[0025] The present invention also provides a method for preparing the antistatic modifier described in the above technical solution, comprising the following steps:

[0026] The sodium polystyrene sulfonate aqueous solution is mixed with the cationic surfactant aqueous solution to form a water-insoluble sodium polystyrene sulfonate-surfactant complex.

[0027] In the preparation method of the antistatic modifier provided by the present invention, the mass percentage concentration of the sodium polystyrene sulfonate aqueous solution is preferably 0.1-5%, specifically 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%; the mass percentage concentration of the cationic surfactant aqueous solution is preferably 0.1-5%, specifically 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%. In the present invention, controlling the concentrations of the two solutions within the above range can produce good water solubility, and after the two solutions are mixed, the sodium polystyrene sulfonate-surfactant complex can be successfully and efficiently precipitated.

[0028] In the preparation method of the antistatic modifier provided by the present invention, the mixing temperature is preferably 0-50°C, specifically 0°C, 5°C, 10°C, 15°C, 20°C, 25°C (room temperature), 30°C, 35°C, 40°C, 45°C or 50°C; the mixing time is preferably 0.5-10 min, specifically 0.5 min, 1 min, 1.5 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min.

[0029] In the method for preparing the antistatic modifier provided by the present invention, after the mixing, preferably solid-liquid separation is also performed. The present invention has no special restrictions on the means of solid-liquid separation, and the sodium polystyrene sulfonate-surfactant complex precipitate in the mixed solution can be fully separated, such as solid-liquid separation by centrifugation. In the present invention, after the solid-liquid separation, preferably water washing and drying are performed to obtain the sodium polystyrene sulfonate-surfactant complex.

[0030] The present invention also provides an antistatic modified nylon, wherein the components of the antistatic modified nylon include: an antistatic modifier and nylon.

[0031] In the antistatic modified nylon provided by the present invention, there is no particular limitation on the type of nylon, including but not limited to one or more of nylon 6, nylon 6 elastomer, nylon 66, nylon 66 elastomer, nylon 11, nylon 11 elastomer, nylon 12, nylon 12 elastomer, nylon 610, nylon 610 elastomer, nylon 612 and nylon 612 elastomer.

[0032] In the antistatic modified nylon provided by the present invention, the antistatic modifier is the antistatic modifier described in the above technical solution or the antistatic modifier prepared by the preparation method described in the above technical solution; the mass percentage of the antistatic modifier in the antistatic modified nylon is preferably 1-10%, specifically 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%. In the present invention, within the above ratio range, the combination of the antistatic modifier and the nylon matrix can reach the best state, the antistatic modifier is evenly distributed in the nylon matrix and forms a dominant dispersion structure with the nylon matrix, which can ensure both good antistatic performance and physical and mechanical properties of the nylon product.

[0033] The present invention also provides a method for preparing the antistatic modified nylon described in the above technical solution, comprising the following steps:

[0034] The antistatic modifier is mixed with nylon and melt-extruded to obtain antistatic modified nylon.

[0035] In the preparation method of antistatic modified nylon provided by the present invention, the temperature of the melt extrusion is preferably 160-240°C, specifically 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C or 240°C; the time of the melt extrusion is preferably 1-6 min, specifically 1 min, 1.5 min, 2 min, 2.5 min, 3 min, 3.5 min, 4 min, 4.5 min, 5 min, 5.5 min or 6 min.

[0036] In the preparation method of antistatic modified nylon provided by the present invention, the melt extrusion can be carried out by equipment familiar to those skilled in the art, such as a twin-screw extruder. Through melt extrusion, the antistatic modifier is evenly dispersed in the nylon elastic matrix, and the antistatic modified nylon material formed not only has good antistatic properties but also has long-lasting antistatic properties; moreover, the antistatic modifier provided by the present invention is resistant to high temperatures, and during the above-mentioned melt extrusion process, the antistatic agent will not undergo side reactions such as high-temperature decomposition, thereby overcoming the problem that the antistatic agent is difficult to melt-process in the past; moreover, the antistatic agent of the obtained antistatic modified nylon has no toxic side effects. In addition, the preparation method is simple and easy to implement, has no pollution to the environment, and is easy to realize large-scale continuous production.

[0037] For the purpose of greater clarity, the invention is described in detail through the following embodiments.

[0038] Example 1

[0039] A 2.0 wt% sodium polystyrene sulfonate aqueous solution (the number average molecular weight of sodium polystyrene sulfonate is 8000) and a 2.0 wt% tributyl hexadecylphosphonium bromide aqueous solution are prepared respectively, and the two solutions are mixed at room temperature for 1 minute according to a mass ratio of sodium polystyrene sulfonate: tributyl hexadecylphosphonium bromide = 1:1 to rapidly form a water-insoluble precipitate, which is centrifuged, washed three times with water and freeze-dried to obtain a sodium polystyrene sulfonate-tributyl hexadecylphosphonium bromide complex antistatic modifier.

[0040] Take 30g of the above antistatic modifier and 970g of nylon 6 (model BASF B3WG5 BK00564, melt flow rate 50cm 3 / 10min, test conditions are: 10kg, 220℃), after being evenly mixed in a high-speed stirrer, melt-extruded in a twin-screw extruder, the extrusion temperature is 220℃, the screw speed is 130rpm, the material residence time is 1.5min, and after melt-extrusion, antistatic modified nylon is obtained.

[0041] Example 2

[0042] A 2.0 wt% sodium polystyrene sulfonate aqueous solution (the number average molecular weight of sodium polystyrene sulfonate is 8000) and a 2.0 wt% tributyl hexadecylphosphonium bromide aqueous solution are prepared respectively, and the two solutions are mixed at room temperature for 1 minute according to a mass ratio of sodium polystyrene sulfonate: tributyl hexadecylphosphonium bromide = 1:1 to rapidly form a water-insoluble precipitate, which is centrifuged, washed three times with water and freeze-dried to obtain a sodium polystyrene sulfonate-tributyl hexadecylphosphonium bromide complex antistatic modifier.

[0043] Take 50g of the above antistatic modifier and 950g of nylon 6 (model BASF B3WG5 BK00564, melt flow rate 50cm 3 / 10min, test conditions are: 10kg, 220℃), after being evenly mixed in a high-speed stirrer, melt-extruded in a twin-screw extruder, the extrusion temperature is 220℃, the screw speed is 130rpm, the material residence time is 1.5min, and after melt-extrusion, antistatic modified nylon is obtained.

[0044] Example 3

[0045] A 1.0 wt% sodium polystyrene sulfonate aqueous solution (the number average molecular weight of sodium polystyrene sulfonate is 8000) and a 1.0 wt% tributyl hexadecylphosphonium bromide aqueous solution are prepared respectively, and the two solutions are mixed at room temperature for 1 minute according to a mass ratio of sodium polystyrene sulfonate: tributyl hexadecylphosphonium bromide = 1:1 to rapidly form a water-insoluble precipitate, which is centrifugally separated, washed three times with water and freeze-dried to obtain a sodium polystyrene sulfonate-tributyl hexadecylphosphonium bromide complex antistatic modifier.

[0046] Take 30g of the above antistatic modifier and 970g of nylon 6 (model BASF B3WG5 BK00564, melt flow rate 50cm 3 / 10min, test conditions are: 10kg, 220℃), after being evenly mixed in a high-speed stirrer, melt-extruded in a twin-screw extruder, the extrusion temperature is 220℃, the screw speed is 130rpm, the material residence time is 1.5min, and after melt-extrusion, antistatic modified nylon is obtained.

[0047] Example 4

[0048] A 1.0 wt% sodium polystyrene sulfonate aqueous solution (the number average molecular weight of sodium polystyrene sulfonate is 8000) and a 1.0 wt% tributyl hexadecylphosphonium bromide aqueous solution are prepared respectively, and the two solutions are mixed at room temperature for 1 minute according to a mass ratio of sodium polystyrene sulfonate: tributyl hexadecylphosphonium bromide = 1:1 to rapidly form a water-insoluble precipitate, which is centrifugally separated, washed three times with water and freeze-dried to obtain a sodium polystyrene sulfonate-tributyl hexadecylphosphonium bromide complex antistatic modifier.

[0049] Take 50g of the above antistatic modifier and 950g of nylon 6 (model BASF B3WG5 BK00564, melt flow rate 50cm 3 / 10min, test conditions are: 10kg, 220℃), after being evenly mixed in a high-speed stirrer, melt-extruded in a twin-screw extruder, the extrusion temperature is 220℃, the screw speed is 130rpm, the material residence time is 1.5min, and after melt-extrusion, antistatic modified nylon is obtained.

[0050] Comparative Example 1

[0051] Take 1000g nylon 6 (model BASF B3WG5 BK00564, melt flow rate 50cm 3 / 10min, test conditions: 10kg, 220℃), after being evenly mixed in a high-speed stirrer, melt-extruded in a twin-screw extruder, the extrusion temperature is 220℃, the screw speed is 130rpm, the material residence time is 1.5min, and after melt-extrusion, a nylon sample is obtained.

[0052] Comparative Example 2

[0053] Take 50g antistatic agent AG700 and 950g nylon 6 (model BASF B3WG5 BK00564, melt flow rate 50cm 3 / 10min, test conditions are: 10kg, 220℃), after being evenly mixed in a high-speed stirrer, melt-extruded in a twin-screw extruder, the extrusion temperature is 220℃, the screw speed is 130rpm, the material residence time is 1.5min, and after melt-extrusion, antistatic modified nylon is obtained.

[0054] Comparative Example 3

[0055] Take 50g of tributyl hexadecylphosphonium bromide and 950g of nylon 6 (model BASF B3WG5 BK00564, melt flow rate 50cm 3 / 10min, test conditions are: 10kg, 220℃), after being evenly mixed in a high-speed stirrer, melt-extruded in a twin-screw extruder, the extrusion temperature is 220℃, the screw speed is 130rpm, the material residence time is 1.5min, and after melt-extrusion, antistatic modified nylon is obtained.

[0056] Performance Testing

[0057] Table 1 Antistatic test results of the obtained nylon products

[0058]

[0059] In order to evaluate the durability of the antistatic agent, the above nylon product test sample was placed in a constant temperature and humidity chamber at a temperature of 60±2°C and a humidity of 95±2% for 96 hours, and the resistance data was tested again.

[0060] Table 2 Antistatic durability test results of the obtained nylon products

[0061]

[0062] It can be seen from the test results in Tables 1 and 2 that the antistatic modified nylon provided by the present invention has excellent antistatic performance, and the antistatic modified nylon provided by the present invention has excellent antistatic durability.

[0063] Comparative Example 2: The antistatic modified nylon material was prepared according to the preparation process of Example 4, except that the antistatic agent AG700 was added. As a result, the antistatic effect and durability of the material were not as good as those of the present invention.

[0064] Comparative Example 3: An antistatic modified nylon material was prepared according to the preparation process of Example 4, except that tributyl hexadecylphosphonium bromide was added. As a result, the antistatic effect and durability of the material were not as good as those of the present invention.

[0065] It can be seen that only when the sodium polystyrene sulfonate provided by the present invention is combined with tributyl hexadecylphosphonium bromide to form a composite can the antistatic effect of the nylon material be significantly improved, and the antistatic durability is excellent.

[0066] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An antistatic modifier, characterized in that It is a sodium polystyrene sulfonate-surfactant complex formed by combining sodium polystyrene sulfonate with a cationic surfactant.

2. The antistatic modifier according to claim 1, characterized in that The number average molecular weight of the sodium polystyrene sulfonate is 2,000 to 200,000.

3. The antistatic modifier according to claim 1, characterized in that The cationic surfactant is selected from one or more of quaternary ammonium salt type, quaternary phosphonium salt type and guanidine type.

4. The antistatic modifier according to claim 1, characterized in that The molecular weight of the cationic surfactant is 50-3000.

5. The antistatic modifier according to claim 1, characterized in that The mass ratio of the sodium polystyrene sulfonate to the cationic surfactant is 1:(0.1-2).

6. A method for preparing the antistatic modifier according to any one of claims 1 to 5, characterized in that: The following steps are involved: The sodium polystyrene sulfonate aqueous solution is mixed with the cationic surfactant aqueous solution to form a water-insoluble sodium polystyrene sulfonate-surfactant complex.

7. The preparation method according to claim 6, characterized in that: The mass percentage concentration of the sodium polystyrene sulfonate aqueous solution is 0.1-5%; The mass percentage concentration of the cationic surfactant aqueous solution is 0.1-5%.

8. An antistatic modified nylon, characterized in that: The components of the antistatic modified nylon include: an antistatic modifier and nylon; The antistatic modifier is the antistatic modifier according to any one of claims 1 to 6 or the antistatic modifier prepared by the preparation method according to any one of claims 6 to 7; The mass percentage of the antistatic modifier in the antistatic modified nylon is 1-10%.

9. The antistatic modified nylon according to claim 8, characterized in that: The nylon includes one or more of nylon 6, nylon 6 elastomer, nylon 66, nylon 66 elastomer, nylon 11, nylon 11 elastomer, nylon 12, nylon 12 elastomer, nylon 610, nylon 610 elastomer, nylon 612 and nylon 612 elastomer.

10. A method for preparing the antistatic modified nylon according to claim 8 or 9, characterized in that: The following steps are involved: The antistatic modifier is mixed with nylon and melt-extruded to obtain antistatic modified nylon.

Citation Information

Patent Citations

  • Oil agent for textile fibers, and preparation method thereof

    CN111411517A

  • Double-antibody material and preparation method thereof

    CN114806155A

  • Preparation method of nylon 6 / polyelectrolyte anti electrostatic composite material and anti electrostatic mother particle

    CN1752142A

  • Synthetic fiber with improved antistaticity

    JP1999081132A

Cited By

  • Flame-retardant antistatic nylon and preparation method thereof

    CN121950035A