Fireproof fluororubber for sealing and preparation method thereof
By wrapping carbon nanotubes with layered double hydroxides of thiophosphonate intercalation in fluoroelastomer and adding in synergistically with sphere-like zirconium phosphate, the poor dispersion and binding of carbon nanotubes in sealing materials are solved. The problem of low force significantly improves fire and waterproof performance and achieves better sealing effect.
Patent Information
- Application Number
- CN202411004236.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When using carbon nanotubes, existing sealing materials have problems such as poor dispersion and low interface bonding with polymer matrix, resulting in insufficient fire and smoke resistance.
The carbon nanotubes are wrapped with layered double hydroxides of thiophosphonate intercalation and are added to the fluoroelastomer in concert with the homemade sphere-like zirconium phosphate to form a network structure to improve flame retardant performance.
It significantly improves the fire and waterproof performance of the material, enhances the dispersion and flame retardancy of carbon nanotubes, and achieves better fire resistance and sealing performance.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fluororubber, in particular to fireproof fluororubber for sealing and a preparation method thereof. Background Art
[0002] At present, sealing materials are often needed in the construction industry and the machinery industry to improve the sound insulation, dustproof, antifreeze, warmth retention and waterproof performance of the structure. For some special fields, such as fire doors, fire windows, fire dampers and fire shutters, it is necessary to use sealing materials with fire retardant effects, and such sealing materials need to have fire and smoke retardant effects both at normal temperature and in fire environment.
[0003] Carbon nanotubes are one-dimensional nanomaterials formed by curling a single or multi-layer graphite sheet around a central axis at a certain spiral angle. Due to their unique structure and excellent physical and chemical properties, they are widely used in the fields of polymer composites, catalysis and adsorption carriers, electrode materials, etc. When carbon nanotubes are dispersed in a polymer matrix as fillers, they can form a network structure, significantly improving the mechanical, thermal stability and flame retardant properties of the material. However, due to their high surface energy, they are prone to agglomeration, and when they are applied to polymer materials, they have problems such as poor dispersibility and low interfacial bonding with the polymer matrix. Therefore, the present invention is based on carbon nanotubes, and phosphorus-based organic matter is used to modify them, and a hybrid filler with a network structure is prepared in coordination with metal hydroxides and added to fluororubber for fireproof modification. Summary of the invention
[0004] The object of the present invention is to provide a fireproof fluororubber for sealing and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a fire-resistant fluororubber for sealing, wherein the fire-resistant fluororubber is prepared by modifying fluororubber with homemade hybrid filler and homemade spherical α-zirconium phosphate as additives.
[0006] Furthermore, the self-made hybrid filler is prepared by wrapping carbon nanotubes with layered double hydroxides intercalated with thiophosphonate.
[0007] Furthermore, the spherical α-zirconium phosphate is synthesized by a reflux method to form a layered α-zirconium phosphate powder, and then the layered α-zirconium phosphate raw powder is ground by ball milling mechanical modification to obtain a micron-level single-layer α-zirconium phosphate powder, which is finally formed using a rotary spray dryer.
[0008] Furthermore, a method for preparing fire-resistant fluororubber for sealing includes the following preparation steps:
[0009] (1) Multi-walled carbon nanotubes with an average diameter of 120 nm were first heated to reflux at 100° C. for 2 h with a mixture of analytically pure concentrated sulfuric acid and concentrated nitric acid, and the filtered precipitate was then refluxed at 100° C. for 2 h with 2 mol / L analytically pure hydrochloric acid, and finally rinsed with deionized water to make the pH value of the filtrate neutral, and then dried at 50° C. for 2 h for standby use; the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1, the concentration of concentrated sulfuric acid was 98%, and the concentration of concentrated nitric acid was 67%; 0.2- 0.214 parts of N-phenylthiophthalimide and 0.2-0.204 parts of diphenylphosphine oxide are added to 2 parts of deionized water, stirred at 40°C and 150 rpm for 3 hours, filtered and filtered, washed twice with deionized water, and air-dried for 2 hours to obtain diphenylthiophosphinate; 4-7 parts of zinc nitrate hydrate and 1-3 parts of aluminum nitrate hydrate are weighed and dissolved in 100 parts of deionized water to prepare a mixed salt solution; 1-2 parts of sodium bicarbonate and 2 1. Dissolve 20 parts of sodium hydroxide in 20 parts of deionized water to prepare a mixed alkali solution; weigh 0.4-0.6 parts of diphenylthiophosphinate, dissolve it in a mixed solution of 50 parts of deionized water and 50 parts of anhydrous ethanol, stir at 60rpm for 30min, add 0.03-0.04 parts of acid-treated multi-walled carbon nanotubes, and ultrasonically disperse for 1-3h to prepare a dispersion of carbon nanotubes; transfer the dispersion to a three-necked flask equipped with a mechanical stirring device and a condensing device, add the mixed alkali solution and stir evenly, slowly add the mixed salt solution dropwise through a constant pressure dropping funnel for 30min, adjust the pH of the system to 10 with hydrochloric acid solution, control the reaction temperature to 70℃ through an oil bath, react for 24h, cool the solution and wash it by centrifugation with deionized water, the centrifugal speed is 3500r / min, the centrifugal time is 6-10min, and the obtained product is dried in an oven at 60℃ for 24h to obtain intercalated layered double hydroxide-wrapped carbon nanotubes;
[0010] (2) dissolving 5-9 parts of ZrOCl2·8H2O in 125 parts of hydrochloric acid solution with a concentration of 1.5-3.0 mol / L to prepare a ZrOCl2 hydrochloric acid solution; mixing 15-35 parts of phosphoric acid with a molar concentration of 4 mol / L with 25 parts of hydrochloric acid with a molar concentration of 2 mol / L to prepare a mixed acid solution; slowly dropping the ZrOCl2 hydrochloric acid solution into the mixed acid solution to obtain a zirconium phosphate gel, wherein the volume ratio of the ZrOCl2 hydrochloric acid solution to the mixed acid is 4:1-4:3; then adding the zirconium phosphate gel to a phosphoric acid solution with a mass percentage of 85% and mixing evenly, and controlling the volume ratio of the gel to the phosphoric acid solution to be 4:1-4:5; stirring and refluxing at a temperature of 50-100° C. for 1-8 days for reaction, centrifuging at a speed of 3500 r / min for 10 minutes, and then drying at room temperature for 2 hours, The α-zirconium phosphate raw powder is obtained; the dried α-zirconium phosphate raw powder is dissolved in deionized water to make its mass percentage content of 1-10%, and then the α-zirconium phosphate raw powder is wet-milled and activated by a high-energy ball mill, a 40mm steel ball is added as a ball milling medium, the ball-to-material ratio is 10-20:1, the ball mill voltage is set to 80-110V, the ball milling tank speed is 400-700r / min, and the ball milling is performed for 30-360min; then a delaminating agent in an amount of 0.1-0.6% deionized water volume ratio is added dropwise to the delaminating agent with a concentration of 4-6g / L, and then the formed gel is ultrasonicated for 1-4 hours with an ultrasonic power of 35kHz, and then placed at room temperature for 1-4d to obtain a delaminated α-zirconium phosphate colloid; and then a rotary spray dryer is used for granulation and drying to obtain micron-level spherical α-zirconium phosphate;
[0011] (3) 100 parts of fluororubber raw rubber, 4-5 parts of triethylene glycol diethylhexanoate, 1-2 parts of alumina, 1-5 parts of modified carbon nanotubes, 0.5-2.5 parts of quasi-spherical α-zirconium phosphate, 2-3 parts of stearic acid monoglyceride, 1.5-2 parts of vulcanizing agent, and 0.3-0.6 parts of vulcanizing aid. Put the raw rubber into an internal mixer according to the proportion and plasticize it for 15-20 minutes at a plasticizing temperature of 70-90°C. After the plasticizing, a fire-resistant fluororubber for sealing is obtained.
[0012] Furthermore, in step (1), the ultrasonic power is 30 kHz.
[0013] Furthermore, the concentration of the hydrochloric acid solution in step (1) is 1.0 mol / L.
[0014] Furthermore, in step (2), the stripping agent is one of methylamine, ethylamine and ethylenediamine.
[0015] Furthermore, during the rotary spray drying in step (2), the feed rate is 50 ml / min and the air inlet temperature is 160°C.
[0016] Furthermore, in step (3), the fluororubber raw rubber is a terpolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene; the fluorine content of the fluororubber raw rubber is 67-70.5%, the Mooney viscosity ML121°C (1+10) is 10-50, the average molecular weight (GPC test) is Mw50,000-600,000, and the broad molecular weight distribution or bimodal distribution (GPC test) is Mw / Mn≧2.0.
[0017] Furthermore, in step (3), the vulcanizing agent is bisphenol AF and the vulcanizing aid is benzyltriphenylphosphonium chloride.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] The present invention uses thiophosphonate intercalated layered double hydroxide wrapped carbon nanotubes as hybrid fillers, and adds self-made spheroidal α-zirconium phosphate into fluororubber in coordination to achieve waterproof and fireproof effects.
[0020] Firstly, thiophosphite is prepared from N-phenylthiophthalimide and diphenylphosphine oxide as raw materials, and then intercalated on a layered double hydroxide. The phosphite and the layered double hydroxide can be mixed evenly at the molecular level, which is helpful to improve the synergistic flame retardant efficiency; the intercalated layered double hydroxide and the carbon nanotubes with negative charge after acid treatment are subjected to electrostatic self-assembly precipitation, so that the surface of the carbon nanotubes is coated; the organic molecular phosphate is hybridized with the inorganic carbon nanotubes by combining the highly delocalized π electrons of the carbon nanotubes with the thiophosphite organic molecules with phenyl groups through the π-π conjugated effect and coordination effect, and the hybrid filler with a network structure is prepared; the filler can form a network structure when dispersed in a polymer matrix, and the layered double hydroxide coated on the surface thereof can improve the dispersibility of the carbon nanotubes while preserving its layered structure, so that the flame retardancy of the filler as a whole works synergistically, and a better fireproof effect is achieved.
[0021] Secondly, a layered α-zirconium phosphate powder is synthesized by a reflux method, and then the layered α-zirconium phosphate raw powder is ground by ball mill mechanical modification to obtain a single-layer α-zirconium phosphate powder at the micron level, and finally a rotary spray dryer is used for molding to form the α-zirconium phosphate into a spherical shape; the layered structure of the spherical α-zirconium phosphate is stable and has a large specific surface area; and the H protons between the α-zirconium phosphate layers can be directly exchanged with metal ions, and the α-zirconium phosphate spheres are added to the fluororubber, and they exchange and adsorb with the hydroxide metal on the surface of the nano-scale filler to form a micro-nano rough structure, which gives the rubber a certain waterproof property, thereby improving the sealing effect; the fluororubber filler of the present invention has a high proportion of organic phosphorus flame retardants, phosphoric acid prevents CO from being oxidized to CO2, and the reaction absorbs heat to reduce the heating process. At the same time, the condensed phase forms a thin glassy or liquid protective layer, thereby reducing oxygen diffusion and heat and mass transfer between the gas phase and the solid phase. The high proportion of phosphorus flame retardants cooperates with the hydroxide metal to make the overall fireproof effect of the rubber obvious. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of a fire-resistant fluororubber for sealing prepared in the following examples are as follows:
[0024] Flame retardancy: The prepared fluororubber material is placed into a mold in a vulcanization device for vulcanization treatment at a temperature of 200°C, a pressure of 180Kgf / cm2, and a vulcanization time of 5 minutes. A flame retardancy test is performed on the sample rubbers of the embodiment and the comparative example: the fluororubber material obtained in this embodiment is burned with a flame of 1100°C for 1 minute to check the burning condition of the fluororubber.
[0025] Mechanical properties: The prepared fluororubber material was placed into a mold in a vulcanization device for vulcanization treatment at a temperature of 200°C, a pressure of 180Kgf / cm2, and a vulcanization time of 5 minutes. The mechanical properties of the fluororubber samples of the embodiment and the comparative example were tested in accordance with the tensile stress-strain properties of fluororubber materials in accordance with GB / T 528-2009.
[0026] Example 1
[0027] (1) Multi-walled carbon nanotubes with an average diameter of 120 nm were first heated to reflux at 100° C. for 2 h with a mixture of analytically pure concentrated sulfuric acid and concentrated nitric acid, and the filtered precipitate was then refluxed at 100° C. for 2 h with 2 mol / L analytically pure hydrochloric acid, and finally rinsed with deionized water to make the pH value of the filtrate neutral, and then dried at 50° C. for 2 h for standby use; the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1, the concentration of concentrated sulfuric acid was 98%, and the concentration of concentrated nitric acid was 67%; 0.2 parts of N-phenylthiophthalimide and 0.2 parts of diphenylphosphine oxide were added to 2 parts of deionized water, stirred at 40°C and 150 rpm for 3 hours, filtered and filtered, washed twice with deionized water, and air-dried for 2 hours to obtain diphenylthiophosphinate; 4 parts of zinc nitrate hydrate and 1 part of aluminum nitrate hydrate were weighed and dissolved in 100 parts of deionized water to prepare a mixed salt solution; 1 part of sodium bicarbonate and 2 parts of sodium hydroxide were dissolved in 20 parts of Prepare a mixed alkali solution in deionized water; weigh 0.4 parts of diphenylthiophosphinate, dissolve it in a mixed solution of 50 parts of deionized water and 50 parts of anhydrous ethanol, stir at 60rpm for 30min, add 0.03 parts of acid-treated multi-walled carbon nanotubes, and ultrasonically disperse at a power of 30kHz for 1h to prepare a dispersion of carbon nanotubes; transfer the dispersion to a three-necked flask equipped with a mechanical stirring device and a condensing device, add the mixed alkali solution and stir evenly, slowly add the mixed salt solution through a constant pressure dropping funnel for 30min, adjust the pH of the system to 10 with 1.0mol / L hydrochloric acid solution, control the reaction temperature to 70℃ through an oil bath, react for 24h, cool the solution and wash it with deionized water by centrifugation, the centrifugal speed is 3500r / min, the centrifugal time is 6min, and the obtained product is dried in an oven at 60℃ for 24h to obtain intercalated layered double hydroxide-wrapped carbon nanotubes;
[0028] (2) dissolving 5 parts of ZrOCl2·8H2O in 125 parts of 1.5 mol / L hydrochloric acid solution to prepare a ZrOCl2 hydrochloric acid solution; mixing 15 parts of 4 mol / L phosphoric acid with 25 parts of 2 mol / L hydrochloric acid to prepare a mixed acid solution; slowly dropping the ZrOCl2 hydrochloric acid solution into the mixed acid solution to obtain a zirconium phosphate gel, wherein the volume ratio of the ZrOCl2 hydrochloric acid solution to the mixed acid is 4:1; then adding the zirconium phosphate gel to a phosphoric acid solution having a mass percentage of 85% and mixing them evenly, wherein the volume ratio of the gel to the phosphoric acid solution is controlled to be 4:1; stirring and refluxing at 50°C for 1 day for reaction, centrifuging at 3500 r / min for 10 minutes, and then drying at room temperature for 2 hours to obtain α-zirconium phosphate raw powder; The dried α-zirconium phosphate raw powder is dissolved in deionized water to make its mass percentage content of 1%, and then the α-zirconium phosphate raw powder is wet-milled and activated using a high-energy ball mill, and a 40mm steel ball is added as a ball milling medium, the ball-to-material ratio is 10:1, the ball mill voltage is set to 80V, the ball milling jar speed is 400r / min, and the ball milling is performed for 30min; then a methylamine delamination agent in an amount of 0.1% deionized water volume ratio is added dropwise to the delamination agent with a concentration of 4g / L, and then the formed gel is ultrasonicated for 1 hour with an ultrasonic power of 35kHz, and then placed at room temperature for 1d to obtain a delaminated α-zirconium phosphate colloid; then a rotary spray dryer is used for granulation and drying, the feed rate is 50ml / min, and the air inlet temperature is 160°C to obtain micron-sized spherical α-zirconium phosphate;
[0029] (3) Fluorine rubber raw rubber is a ternary copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene; the fluorine content of the fluorine rubber raw rubber is 67%, the Mooney viscosity ML121℃(1+10) is 10-50, the average molecular weight (GPC test) is Mw50,000-600,000, and the broad molecular weight distribution or bimodal distribution (GPC test) is Mw / Mn≧2.0; 100 parts of fluorine rubber raw rubber, 4 parts of triethylene glycol diisooctanoate, 1 part of alumina, 1 part of modified carbon nanotubes, 0.5 parts of spherical α-zirconium phosphate, 2 parts of stearic acid monoglyceride, 1.5 parts of bisphenol AF, 0.3 parts of benzyl triphenylphosphonium chloride, according to the proportion, put the raw rubber into an internal mixer for plasticization for 15 minutes, the plasticization temperature is 70℃, and after the end, a fireproof fluorine rubber for sealing is obtained.
[0030] Example 2
[0031] (1) Multi-walled carbon nanotubes with an average diameter of 120 nm were first heated to reflux at 100°C for 2 h with a mixture of analytically pure concentrated sulfuric acid and concentrated nitric acid. The filtered precipitate was then refluxed at 100°C for 2 h with 2 mol / L analytically pure hydrochloric acid. Finally, it was rinsed with deionized water to make the pH value of the filtrate neutral. The filtrate was dried at 50°C for 2 h and then used. The volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1, the concentration of concentrated sulfuric acid was 98%, and the concentration of concentrated nitric acid was 67%. 0. 207 parts of N-phenylthiophthalimide and 0.202 parts of diphenylphosphine oxide were added to 2 parts of deionized water, stirred at 40°C and 150 rpm for 3 hours, filtered and the filtrate was washed twice with deionized water, and air-dried for 2 hours to obtain diphenylthiophosphinate; 5.5 parts of zinc nitrate hydrate and 2 parts of aluminum nitrate hydrate were weighed and dissolved in 100 parts of deionized water to prepare a mixed salt solution; 1.5 parts of sodium bicarbonate and 2 parts of sodium hydroxide were dissolved in 100 parts of deionized water to prepare a mixed salt solution; Prepare a mixed alkali solution in 20 parts of deionized water; weigh 0.5 parts of diphenylthiophosphinate, dissolve it in a mixed solution of 50 parts of deionized water and 50 parts of anhydrous ethanol, stir at 60rpm for 30min, add 0.035 parts of acid-treated multi-walled carbon nanotubes, and ultrasonically disperse at a power of 30kHz for 2h to prepare a dispersion of carbon nanotubes; transfer the dispersion to a three-necked flask equipped with a mechanical stirring device and a condensing device, add the mixed alkali solution and stir evenly, slowly add the mixed salt solution through a constant pressure dropping funnel for 30min, adjust the pH of the system to 10 with 1.0mol / L hydrochloric acid solution, control the reaction temperature to 70℃ through an oil bath, react for 24h, cool the solution and wash it with deionized water by centrifugation, the centrifugal speed is 3500r / min, the centrifugal time is 8min, and the obtained product is dried in an oven at 60℃ for 24h to obtain intercalated layered double hydroxide-wrapped carbon nanotubes;
[0032] (2) Dissolving 7 parts of ZrOCl2·8H2O in 125 parts of 2.75 mol / L hydrochloric acid solution to prepare a ZrOCl2 hydrochloric acid solution; mixing 25 parts of 4 mol / L phosphoric acid with 25 parts of 2 mol / L hydrochloric acid to prepare a mixed acid solution; slowly dropping the ZrOCl2 hydrochloric acid solution into the mixed acid solution to obtain a zirconium phosphate gel, wherein the volume ratio of the ZrOCl2 hydrochloric acid solution to the mixed acid is 4:2; then adding the zirconium phosphate gel to a phosphoric acid solution having a mass percentage of 85% and mixing them uniformly, wherein the volume ratio of the gel to the phosphoric acid solution is controlled to be 4:4; stirring and refluxing at 75°C for 4.5 days to react, centrifuging at 3500 r / min for 10 minutes, and then drying at room temperature for 2 hours to obtain α-zirconium phosphate raw powder; The dried α-zirconium phosphate raw powder is dissolved in deionized water to make its mass percentage content of 5%, and then the α-zirconium phosphate raw powder is wet-milled and activated using a high-energy ball mill, and a 40mm steel ball is added as a ball milling medium, the ball-to-material ratio is 15:1, the ball mill voltage is set to 95V, the ball milling jar speed is 550r / min, and the ball milling is performed for 190min; then, 0.35% deionized water volume ratio of ethylamine delamination agent is added dropwise to the delamination agent with a concentration of 5g / L, and then the formed gel is ultrasonicated for 2.5 hours at an ultrasonic power of 35kHz, and then placed at room temperature for 2.5d to obtain a delaminated α-zirconium phosphate colloid; then a rotary spray dryer is used for granulation and drying, the feed rate is 50ml / min, and the air inlet temperature is 160°C to obtain micron-sized spherical α-zirconium phosphate;
[0033] (3) Fluorine rubber raw rubber is a terpolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene; the fluorine content of the fluorine rubber raw rubber is 69%, the Mooney viscosity ML121℃(1+10) is 10-50, the average molecular weight (GPC test) is Mw50,000-600,000, and the broad molecular weight distribution or bimodal distribution (GPC test) is Mw / Mn≧2.0; 100 parts of fluorine rubber raw rubber, 4.5 parts of triethylene glycol diisooctanoate, 1.5 parts of alumina, 3 parts of modified carbon nanotubes, 1.5 parts of spherical α-zirconium phosphate, 2.5 parts of stearic acid monoglyceride, 1.75 parts of bisphenol AF, 0.45 parts of benzyl triphenylphosphonium chloride, according to the proportion, the raw rubber is put into an internal mixer for plasticization for 17.5 minutes, the plasticization temperature is 80℃, and after the end, a fireproof fluorine rubber for sealing is obtained.
[0034] Example 3
[0035] (1) Multi-walled carbon nanotubes with an average diameter of 120 nm were first heated to reflux at 100° C. for 2 h with a mixture of analytically pure concentrated sulfuric acid and concentrated nitric acid, and the filtered precipitate was then refluxed at 100° C. for 2 h with 2 mol / L analytically pure hydrochloric acid, and finally rinsed with deionized water to make the pH value of the filtrate neutral, and then dried at 50° C. for 2 h for standby use; the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1, the concentration of concentrated sulfuric acid was 98%, and the concentration of concentrated nitric acid was 67%; 0 .214 parts of N-phenylthiophthalimide and 0.204 parts of diphenylphosphine oxide were added to 2 parts of deionized water, stirred at 40°C and 150rpm for 3 hours, filtered and the filtrate was washed twice with deionized water, and air-dried for 2 hours to obtain diphenylthiophosphinate; 7 parts of zinc nitrate hydrate and 3 parts of aluminum nitrate hydrate were weighed and dissolved in 100 parts of deionized water to prepare a mixed salt solution; 2 parts of sodium bicarbonate and 2 parts of sodium hydroxide were dissolved in 2 0.6 parts of diphenylthiophosphinate were weighed and dissolved in a mixed solution of 50 parts of deionized water and 50 parts of anhydrous ethanol, and after stirring at 60 rpm for 30 min, 0.04 parts of acid-treated multi-walled carbon nanotubes were added thereto, and ultrasonic dispersion was performed at a power of 30 kHz for 3 h to prepare a dispersion of carbon nanotubes; the dispersion was transferred to a three-necked flask equipped with a mechanical stirring device and a condensing device, the mixed alkali solution was added and stirred evenly, and the mixed salt solution was slowly added dropwise through a constant pressure dropping funnel for 30 min, the pH of the system was adjusted to 10 with a 1.0 mol / L hydrochloric acid solution, the reaction temperature was controlled to 70°C by an oil bath, the reaction was carried out for 24 h, the solution was cooled and washed by centrifugation with deionized water, the centrifugal speed was 3500 r / min, the centrifugal time was 10 min, and the obtained product was dried in an oven at 60°C for 24 h to obtain intercalated layered double hydroxide-wrapped carbon nanotubes;
[0036] (2) dissolving 9 parts of ZrOCl2·8H2O in 125 parts of 3.0 mol / L hydrochloric acid solution to prepare a ZrOCl2 hydrochloric acid solution; mixing 35 parts of 4 mol / L phosphoric acid with 25 parts of 2 mol / L hydrochloric acid to prepare a mixed acid solution; slowly dropping the ZrOCl2 hydrochloric acid solution into the mixed acid solution to obtain a zirconium phosphate gel, wherein the volume ratio of the ZrOCl2 hydrochloric acid solution to the mixed acid is 4:3; then adding the zirconium phosphate gel to a phosphoric acid solution having a mass percentage of 85% and mixing them evenly, wherein the volume ratio of the gel to the phosphoric acid solution is controlled to be 4:5; stirring and refluxing at 100°C for 8 days to react, centrifuging at 3500 r / min for 10 minutes, and then drying at room temperature for 2 hours to obtain α-zirconium phosphate raw powder; The dried α-zirconium phosphate raw powder is dissolved in deionized water to make its mass percentage content of 10%, and then the α-zirconium phosphate raw powder is wet-milled and activated using a high-energy ball mill, and a 40mm steel ball is added as a ball milling medium, the ball-to-material ratio is 20:1, the ball mill voltage is set to 110V, the ball milling jar speed is 700r / min, and the ball milling is performed for 360min; then, 0.6% deionized water volume ratio of ethylenediamine stripping agent is added dropwise to the stripping agent with a concentration of 6g / L, and then the formed gel is ultrasonicated for 4 hours with an ultrasonic power of 35kHz, and then placed at room temperature for 4d to obtain a stripped α-zirconium phosphate colloid; then a rotary spray dryer is used for granulation and drying, the feed rate is 50ml / min, and the air inlet temperature is 160°C to obtain micron-sized spherical α-zirconium phosphate;
[0037] (3) Fluorine rubber raw rubber is a ternary copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene; the fluorine content of the fluorine rubber raw rubber is 70.5%, the Mooney viscosity ML121℃(1+10) is 10-50, the average molecular weight (GPC test) is Mw50,000-600,000, and the broad molecular weight distribution or bimodal distribution (GPC test) is Mw / Mn≧2.0; 100 parts of fluorine rubber raw rubber, 5 parts of triethylene glycol diisooctanoate, 2 parts of aluminum oxide, 5 parts of modified carbon nanotubes, 2.5 parts of spherical α-zirconium phosphate, 3 parts of stearic acid monoglyceride, 2 parts of bisphenol AF, 0.6 parts of benzyl triphenylphosphonium chloride, according to the proportion, put the raw rubber into an internal mixer and plasticize for 20 minutes, the plasticizing temperature is 90℃, and after the plasticizing, a fireproof fluorine rubber for sealing is obtained.
[0038] Comparative Example 1
[0039] The difference between Comparative Example 1 and Example 2 lies in the difference in step (1), where step (1) is modified as follows: multi-walled carbon nanotubes with an average diameter of 120 nm are first heated to reflux at 100° C. for 2 h with a mixture of analytically pure concentrated sulfuric acid and concentrated nitric acid, the filtered precipitate is then refluxed at 100° C. for 2 h with 2 mol / L analytically pure hydrochloric acid, and finally rinsed with deionized water to make the pH value of the filtrate neutral, and then dried at 50° C. for 2 h for standby use; the volume ratio of concentrated sulfuric acid to concentrated nitric acid is 3:1, the concentration of concentrated sulfuric acid is 98%, and the concentration of concentrated nitric acid is 67%; 5.5 parts of zinc nitrate hydrate and 2 parts of aluminum nitrate hydrate are weighed and dissolved in 100 parts of deionized water to prepare a mixed salt solution; 1.5 parts of sodium bicarbonate and 2 parts of sodium hydroxide are dissolved in 20 parts of deionized water to prepare a mixed alkali solution; 50 parts of deionized water and 50 parts of anhydrous In the mixed solution of ethanol, after stirring at 60rpm for 30min, 0.035 parts of acid-treated multi-walled carbon nanotubes were added thereto, and ultrasonic dispersion was carried out at a power of 30kHz for 2h to prepare a dispersion of carbon nanotubes; the dispersion was transferred to a three-necked flask equipped with a mechanical stirring device and a condensing device, a mixed alkali solution was added and stirred evenly, and a mixed salt solution was slowly added dropwise through a constant pressure dropping funnel for 30min, and the pH of the system was adjusted to 10 with a 1.0mol / L hydrochloric acid solution, and the reaction temperature was controlled to 70°C by an oil bath, and the reaction was carried out for 24h. After the solution was cooled, it was centrifuged and washed with deionized water at a centrifugal speed of 3500r / min and a centrifugal time of 8min. The obtained product was dried in an oven at 60°C for 24h to obtain carbon nanotubes wrapped with layered double hydroxides; the remaining steps were the same as those in Example 2.
[0040] Comparative Example 2
[0041] The difference between Comparative Example 2 and Example 2 lies in the difference in step (1), whereby step (1) is modified as follows: multi-walled carbon nanotubes having an average diameter of 120 nm are first heated to reflux at 100° C. for 2 h with a mixture of analytically pure concentrated sulfuric acid and concentrated nitric acid, the filtered precipitate is then refluxed at 100° C. for 2 h with 2 mol / L analytically pure hydrochloric acid, and finally rinsed with deionized water to adjust the pH value of the filtrate to neutral, and then dried at 50° C. for 2 h for standby use; the volume ratio of concentrated sulfuric acid to concentrated nitric acid is 3:1, the concentration of concentrated sulfuric acid is 98%, and the concentration of concentrated nitric acid is 67%; 0.207 parts of N-phenylthiophthalimide and 0.202 parts of diphenyl oxide are added. The phosphine was added into 2 parts of deionized water, stirred at 150 rpm for 3 hours at 40°C, the filtrate was filtered, washed twice with deionized water, and dried with air for 2 hours to obtain diphenyl thiophosphinate; 0.5 parts of diphenyl thiophosphinate were weighed and dissolved in a mixed solution of 50 parts of deionized water and 50 parts of anhydrous ethanol, stirred at 60 rpm for 30 minutes, 0.035 parts of acid-treated multi-walled carbon nanotubes were added thereto, and ultrasonic dispersion was carried out at a power of 30 kHz for 2 hours to prepare a dispersion of carbon nanotubes, and the obtained product was dried in an oven at 60°C for 24 hours to obtain modified carbon nanotubes; the remaining steps were the same as those in Example 2.
[0042] Comparative Example 3
[0043] The difference between Comparative Example 3 and Example 2 is that there is no step (1), and step (3) is changed to: the fluororubber raw rubber is a terpolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene; the fluorine content of the fluororubber raw rubber is 69%, the Mooney viscosity ML121°C (1+10) is 10-50, the average molecular weight (GPC test) is Mw5-600,000, and the broad molecular weight distribution or bimodal distribution (GPC test) is Mw / Mn≧2.0; 100 parts of fluororubber raw rubber, 4.5 parts of triethylene glycol diisooctanoate, 1.5 parts of alumina, 1.5 parts of spherical α-zirconium phosphate, 2.5 parts of stearic acid monoglyceride, 1.75 parts of bisphenol AF, and 0.45 parts of benzyltriphenylphosphonium chloride are placed in an internal mixer according to the ratio and plasticized for 17.5 minutes at a plasticizing temperature of 80°C. After the plasticizing, a fireproof fluororubber for sealing is obtained; the remaining steps are the same as those in Example 2.
[0044] Comparative Example 4
[0045] The difference between Comparative Example 4 and Example 2 is that there is no step (1), and step (3) is changed to: the fluororubber raw rubber is a terpolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene; the fluorine content of the fluororubber raw rubber is 69%, the Mooney viscosity ML121°C (1+10) is 10-50, the average molecular weight (GPC test) is Mw5-600,000, and the broad molecular weight distribution or bimodal distribution (GPC test) is Mw / Mn≧2.0; 100 parts of fluororubber raw rubber, 4.5 parts of triethylene glycol diethylhexanoate, 1.5 parts of alumina, 3 parts of modified carbon nanotubes, 2.5 parts of stearic acid monoglyceride, 1.75 parts of bisphenol AF, and 0.45 parts of benzyltriphenylphosphonium chloride are placed in an internal mixer according to the ratio and plasticized for 17.5 minutes at a plasticizing temperature of 80°C. After the plasticizing, a fire-resistant fluororubber for sealing is obtained; the remaining steps are the same as those in Example 2.
[0046] Comparative Example 5
[0047] The difference between Comparative Example 5 and Example 2 lies in the difference in steps (2) and (3). Steps (2) and (3) are modified as follows: (2) 7 parts of ZrOCl2·8H2O are dissolved in 125 parts of a hydrochloric acid solution having a concentration of 2.75 mol / L to prepare a ZrOCl2 hydrochloric acid solution; 25 parts of phosphoric acid having a molar concentration of 4 mol / L and 25 parts of hydrochloric acid having a molar concentration of 2 mol / L are mixed to prepare a mixed acid solution; the ZrOCl2 hydrochloric acid solution is slowly added dropwise to the mixed acid solution to obtain a zirconium phosphate gel, wherein the volume ratio of the ZrOCl2 hydrochloric acid solution to the mixed acid is 4:2; the zirconium phosphate gel is then added to a phosphoric acid solution having a mass percentage of 85% and mixed uniformly, wherein the volume ratio of the gel to the phosphoric acid solution is controlled to be 4:4; the reaction is stirred and refluxed at 75°C for 4.5 days, and then 350 0r / min speed centrifugation for 10min, and then drying at room temperature for 2h to obtain α-zirconium phosphate raw powder; the dried α-zirconium phosphate raw powder is dissolved in deionized water to make its mass percentage content of 5%, and then the α-zirconium phosphate raw powder is wet ball-milled and activated using a high-energy ball mill, 40mm steel balls are added as ball-milling media, the ball-to-material ratio is 15:1, the ball mill voltage is set to 95V, the ball mill speed is 550r / min, and the ball milling is carried out for 190min; then 0.35% deionized water volume ratio of ethylamine stripping agent is added dropwise thereto with a concentration of 5g / L stripping agent, and then the formed gel is ultrasonicated for 2.5 hours with an ultrasonic power of 35kHz, and then placed at room temperature for 2.5d to obtain a stripped α-zirconium phosphate colloid, and dried at 50°C for 2h to obtain micron-sized α-zirconium phosphate;
[0048] (3) The fluororubber raw rubber is a terpolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene; the fluorine content of the fluororubber raw rubber is 69%, the Mooney viscosity ML121°C (1+10) is 10-50, the average molecular weight (GPC test) is Mw5-600,000, and the broad molecular weight distribution or bimodal distribution (GPC test) is Mw / Mn≧2.0; 100 parts of fluororubber raw rubber, 4.5 parts of triethylene glycol diisooctanoate, 1.5 parts of alumina, 3 parts of modified carbon nanotubes, 1.5 parts of α-zirconium phosphate, 2.5 parts of stearic acid monoglyceride, 1.75 parts of bisphenol AF, and 0.45 parts of benzyl triphenylphosphonium chloride are put into an internal mixer according to the proportion and plasticized for 17.5 minutes at a plasticizing temperature of 80°C. After the plasticization, a fireproof fluororubber for sealing is obtained; the remaining steps are the same as those in Example 2.
[0049] Effect example
[0050] Table 1 below shows the performance analysis results of a fire-resistant fluororubber for sealing using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.
[0051] Table 1
[0052] Burning effect Tensile strength MPa Elongation at break % Withstand water pressure MPa Example 1 No burning 22.7 395 0.8 Example 2 No burning 23.5 398 0.9 Example 3 No burning 22.8 394 0.9 Comparative Example 1 No burning 21.2 372 0.8 Comparative Example 2 Slight burning effect 21.8 386 0.6 Comparative Example 3 Slight burning effect 21.9 378 0.7 Comparative Example 4 Slight burning effect 22.4 365 0.7 Comparative Example 5 No burning 21.0 350 0.5
[0053] From the comparison of the experimental data of the burning effect of the embodiment and the comparative example, it can be found that the present invention prepares thiophosphite from N-phenylthiophthalimide and diphenylphosphine oxide raw materials, and intercalates on the layered double hydroxide. The phosphite and the layered double hydroxide can be mixed at the molecular level, which is helpful to improve the synergistic flame retardant efficiency; the intercalated layered double hydroxide and the carbon nanotubes with negative charge after acid treatment are subjected to electrostatic self-assembly precipitation, so that the surface of the carbon nanotubes is coated; the highly delocalized π electrons of the carbon nanotubes are combined with the thiophosphite organic molecules with phenyl groups through the π-π conjugated effect and coordination effect, and the organic molecular phosphate is hybridized with the inorganic carbon nanotubes to prepare a hybrid filler with a network structure; the filler can form a network structure when dispersed in the polymer matrix, and the layered double hydroxide coated on the surface thereof can improve the dispersibility of the carbon nanotubes while preserving its layered structure, so that the flame retardancy of the filler as a whole is synergistic, and a better fireproof effect is achieved. Secondly, the present invention synthesizes layered α-zirconium phosphate powder by a reflux method, and then grinds the layered α-zirconium phosphate raw powder by ball mill mechanical modification to obtain micron-level single-layer α-zirconium phosphate powder, and finally uses a rotary spray dryer to form the α-zirconium phosphate into a spherical shape; the spherical α-zirconium phosphate has a stable layered structure and a large specific surface area; the fluororubber filler of the present invention has a high proportion of organic phosphorus flame retardants, phosphoric acid prevents CO from being oxidized to CO2, and the reaction absorbs heat to reduce the heating process. At the same time, the condensed phase forms a thin glassy or liquid protective layer, thereby reducing oxygen diffusion and heat and mass transfer between the gas phase and the solid phase. The high proportion of phosphorus flame retardants cooperates with metal hydroxide to make the overall fire retardant effect of the rubber obvious. From the comparison of the experimental data of the waterproofness of the embodiment and the comparative example, it can be found that the H protons between the α-zirconium phosphate layers added by the present invention can be directly exchanged with metal ions. When the α-zirconium phosphate spheres are added to the fluororubber, they exchange and adsorb with the hydroxide metal on the surface of the nano-scale filler, forming a micro-nano rough structure, which gives the rubber a certain waterproof property, thereby improving the sealing effect. From the comparison of the experimental data of the mechanical properties of the embodiment and the comparative example, it can be found that in the preparation process of the present invention, the filler particles added have high fineness and good dispersibility, which ensures the tensile strength and elongation of the fluororubber, making it have good sealing performance.
[0054] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A fireproof fluororubber for sealing, characterized in that: The fireproof fluororubber is prepared by using homemade hybrid filler and homemade spherical alpha-zirconium phosphate as additives to modify the fluororubber.
2. The fireproof fluororubber for sealing according to claim 1, characterized in that: The self-made hybrid filler is prepared by wrapping carbon nanotubes with thiophosphonate intercalated layered double hydroxides.
3. The fireproof fluororubber for sealing according to claim 1, characterized in that: The spherical α-zirconium phosphate is synthesized by a reflux method into a layered α-zirconium phosphate powder, and then the layered α-zirconium phosphate raw powder is ground by ball milling mechanical modification to obtain a micron-level single-layer α-zirconium phosphate powder, which is finally formed using a rotary spray dryer.
4. A method for preparing fire-resistant fluororubber for sealing, characterized in that: The method comprises the following preparation steps: (1) Multi-walled carbon nanotubes with an average diameter of 120 nm were first heated to reflux at 100° C. for 2 h with a mixture of analytically pure concentrated sulfuric acid and concentrated nitric acid, and the filtered precipitate was then refluxed at 100° C. for 2 h with 2 mol / L analytically pure hydrochloric acid, and finally rinsed with deionized water to make the pH value of the filtrate neutral, and then dried at 50° C. for 2 h for standby use; the volume ratio of concentrated sulfuric acid to concentrated nitric acid was 3:1, the concentration of concentrated sulfuric acid was 98%, and the concentration of concentrated nitric acid was 67%; 0.2- 0.214 parts of N-phenylthiophthalimide and 0.2-0.204 parts of diphenylphosphine oxide are added to 2 parts of deionized water, stirred at 40°C and 150 rpm for 3 hours, filtered and filtered, washed twice with deionized water, and air-dried for 2 hours to obtain diphenylthiophosphinate; 4-7 parts of zinc nitrate hydrate and 1-3 parts of aluminum nitrate hydrate are weighed and dissolved in 100 parts of deionized water to prepare a mixed salt solution; 1-2 parts of sodium bicarbonate and 2 1. Dissolve 20 parts of sodium hydroxide in 20 parts of deionized water to prepare a mixed alkali solution; weigh 0.4-0.6 parts of diphenylthiophosphinate, dissolve it in a mixed solution of 50 parts of deionized water and 50 parts of anhydrous ethanol, stir at 60rpm for 30min, add 0.03-0.04 parts of acid-treated multi-walled carbon nanotubes, and ultrasonically disperse for 1-3h to prepare a dispersion of carbon nanotubes; transfer the dispersion to a three-necked flask equipped with a mechanical stirring device and a condensing device, add the mixed alkali solution and stir evenly, slowly add the mixed salt solution dropwise through a constant pressure dropping funnel for 30min, adjust the pH of the system to 10 with hydrochloric acid solution, control the reaction temperature to 70℃ through an oil bath, react for 24h, cool the solution and wash it by centrifugation with deionized water, the centrifugal speed is 3500r / min, the centrifugal time is 6-10min, and the obtained product is dried in an oven at 60℃ for 24h to obtain intercalated layered double hydroxide-wrapped carbon nanotubes; (2) dissolving 5-9 parts of ZrOCl2·8H2O in 125 parts of hydrochloric acid solution with a concentration of 1.5-3.0 mol / L to prepare a ZrOCl2 hydrochloric acid solution; mixing 15-35 parts of phosphoric acid with a molar concentration of 4 mol / L with 25 parts of hydrochloric acid with a molar concentration of 2 mol / L to prepare a mixed acid solution; slowly dropping the ZrOCl2 hydrochloric acid solution into the mixed acid solution to obtain a zirconium phosphate gel, wherein the volume ratio of the ZrOCl2 hydrochloric acid solution to the mixed acid is 4:1-4:3; then adding the zirconium phosphate gel to a phosphoric acid solution with a mass percentage of 85% and mixing evenly, and controlling the volume ratio of the gel to the phosphoric acid solution to be 4:1-4:5; stirring and refluxing at a temperature of 50-100° C. for 1-8 days for reaction, centrifuging at a speed of 3500 r / min for 10 minutes, and then drying at room temperature for 2 hours, The α-zirconium phosphate raw powder is obtained; the dried α-zirconium phosphate raw powder is dissolved in deionized water to make its mass percentage content of 1-10%, and then the α-zirconium phosphate raw powder is wet-milled and activated by a high-energy ball mill, a 40mm steel ball is added as a ball milling medium, the ball-to-material ratio is 10-20:1, the ball mill voltage is set to 80-110V, the ball milling tank speed is 400-700r / min, and the ball milling is performed for 30-360min; then a delaminating agent in an amount of 0.1-0.6% deionized water volume ratio is added dropwise to the delaminating agent with a concentration of 4-6g / L, and then the formed gel is ultrasonicated for 1-4 hours with an ultrasonic power of 35kHz, and then placed at room temperature for 1-4d to obtain a delaminated α-zirconium phosphate colloid; and then a rotary spray dryer is used for granulation and drying to obtain micron-level spherical α-zirconium phosphate; (3) 100 parts of fluororubber raw rubber, 4-5 parts of triethylene glycol diethylhexanoate, 1-2 parts of alumina, 1-5 parts of modified carbon nanotubes, 0.5-2.5 parts of quasi-spherical α-zirconium phosphate, 2-3 parts of stearic acid monoglyceride, 1.5-2 parts of vulcanizing agent, and 0.3-0.6 parts of vulcanizing aid. Put the raw rubber into an internal mixer according to the proportion and plasticize it for 15-20 minutes at a plasticizing temperature of 70-90°C. After the plasticizing, a fire-resistant fluororubber for sealing is obtained.
5. The method for preparing fireproof fluororubber for sealing according to claim 4, characterized in that: The ultrasonic power in the step (1) is 30 kHz.
6. The method for preparing fireproof fluororubber for sealing according to claim 4, characterized in that: The concentration of the hydrochloric acid solution in step (1) is 1.0 mol / L.
7. The method for preparing fireproof fluororubber for sealing according to claim 4, characterized in that: In the step (2), the stripping agent is one of methylamine, ethylamine and ethylenediamine.
8. The method for preparing fireproof fluororubber for sealing according to claim 4, characterized in that: During the rotary spray drying in step (2), the feed rate is 50 ml / min and the air inlet temperature is 160°C.
9. The method for preparing fireproof fluororubber for sealing according to claim 4, characterized in that: The fluororubber raw rubber in step (3) is a ternary copolymer of vinylidene fluoride, hexafluoropropylene and tetrafluoroethylene; the fluorine content of the fluororubber raw rubber is 67-70.5%, the Mooney viscosity ML121°C (1+10) is 10-50, the average molecular weight (GPC test) is Mw50,000-600,000, and the broad molecular weight distribution or bimodal distribution (GPC test) is Mw / Mn≧2.
0.
10. The method for preparing fireproof fluororubber for sealing according to claim 4, characterized in that: In the step (3), the vulcanizing agent is bisphenol AF, and the vulcanizing aid is benzyltriphenylphosphonium chloride.
Citation Information
Patent Citations
Sphere analogous alpha-zirconium phosphate and preparing method thereof
CN101058411A
Zinc-aluminum layered double hydroxide coated carbon nanotube composite powder and preparation method thereof
CN104610575A
Carbon nanotube / alpha-zirconium phosphate composite powder and preparation method thereof
CN104627979A
Flame-retardant smoke-suppressing carbon nano tube / nickel aluminum layered double hydroxide compound powder and preparation method and application thereof
CN105153464A
Green synthetic method of thiohypophosphate
CN110330526A
Cited By
Tear-resistant fluororubber material and preparation method thereof
CN119708731A