Anti-fogging master batch suitable for two-way stretching process and preparation method of anti-fogging master batch

Through micron-level hydrophobic anti-fog masterbatch, combined with methacrylic resin and other components, the problem of the anti-fog effect of traditional anti-fog masterbatch is not long-lasting and unprintable, and the long-lasting anti-fog and good printing adaptability is achieved, reducing the Production costs have broadened the application areas.

CN118931084AInactive Publication Date: 2024-11-12ZHONGSHAN YONGNING FILM MATERIALS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411133133.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The anti-fog masterbatch of the existing polypropylene substrate has the problem of anti-fog effect that is non-permanent and cannot be printed. The anti-fog effect of the traditional hydrophilic group masterbatch is not long-lasting and contains silicon and fluorine-based masterbatch. Not printable and increases production costs.

Method used

A micron-grade hydrophobic anti-fogging masterbatch, including methacrylic resin, acrylic acid, 1,4-butanediol dimethacrylate, 2-(dimethylamino)ethyl methacrylate and initiation The agent can achieve long-lasting anti-fog effect and excellent printability by modifying components such as fluorocarbon resin and vinyl triethoxysilane.

Benefits of technology

It achieves long-lasting anti-fog performance and good printing adaptability, reduces production costs, avoids VOC emissions and oligomer accumulation, and broadens the application fields and market prospects of the products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention is applicable to the field of antifogging, and discloses an antifogging master batch applicable to a two-way stretching process and a preparation method thereof.The antifogging master batch is prepared from, by weight, 4-5 parts of methacrylic resin, 2-4 parts of acrylic acid, 1-3 parts of 1, 2-propylene glycol, 1-3 parts of 1, 3-propylene glycol and 1-3 parts of a coupling agent. The adhesive comprises the following components in parts by weight: 1-2 parts of 1, 4-butanediol dimethacrylate, 1-2 parts of methacrylic acid 2-(dimethylamino) ethyl ester, 0.05-0.1 part of an initiator and 8-12 parts of a first solvent. The anti-fog master batch provided by the invention has hydrophobic printability and non-mobility, realizes a good long-time anti-fog effect, is low in VOC emission in the production process, is not easy to accumulate oligomers on a film die lip, and ensures the stability and environmental protection property of film processing. Meanwhile, the binding force between the ink layer and the packaging film is enhanced through the special polymerization structure and molecular chain design of the anti-fog master batch, so that the finished film is remarkable in anti-fog effect and suitable for oil-based ink printing, and the application range of the product is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of anti-fogging, and in particular to an anti-fogging masterbatch suitable for a biaxial stretching process and a preparation method thereof. Background Art

[0002] At present, the anti-fog masterbatch used in the biaxially stretched anti-fog film based on polypropylene on the market is divided into two categories. The first category is mainly based on hydrophilic groups, that is, amine and hydroxyl groups, and achieves the anti-fog effect by absorbing moisture. Once the anti-fog masterbatch group absorbs water to saturation, the anti-fog effect will drop significantly, so this anti-fog effect is not permanent; the second category is silicon- and fluorine-containing anti-fog masterbatch, which achieves the anti-fog effect through hydrophobic effect. This type of anti-fog effect is permanent, but because it contains more non-polar materials, the anti-fog film produced using this type of anti-fog masterbatch cannot be printed, and the product needs to be labeled separately, which increases the production cost. Summary of the invention

[0003] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, the present application proposes an anti-fog masterbatch suitable for a biaxial stretching process. The anti-fog masterbatch of the present application is different from the existing anti-fog masterbatch. The anti-fog mechanism of the present application is a hydrophobic effect at the micron level, which can effectively repel water without affecting the penetration of organic solvents. Therefore, the anti-fog masterbatch of the application can repel water without affecting oil-based ink printing.

[0004] The anti-fog masterbatch is calculated by weight and includes the following components:

[0005] 4-5 parts of methacrylic resin, 2-4 parts of acrylic acid, 1-2 parts of 1,4-butanediol dimethacrylate, 1-2 parts of 2-(dimethylamino)ethyl methacrylate, 0.05-0.1 parts of initiator and 8-12 parts of the first solvent.

[0006] To be more specific, in the above technical solution, the anti-fog masterbatch, calculated by weight, includes the following components: 5 parts of methacrylic resin, 2 parts of acrylic acid, 2 parts of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, 0.05 parts of initiator and 10 parts of the first solvent.

[0007] To be more specific, in the above technical solution, the anti-fog masterbatch, calculated by weight, includes the following components: 4 parts of methacrylic resin, 4 parts of acrylic acid, 1 part of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, 0.05 parts of di-tert-butyl peroxide and 10 parts of the first solvent.

[0008] More specifically, in the above technical solution, the anti-fog masterbatch comprises the following components, calculated by weight: 0.5-3 parts of modified fluorocarbon resin.

[0009] More specifically, in the above technical solution, the modified fluorocarbon resin includes, by weight percentage, 50-60% of fluorocarbon resin matrix, 18-22% of methyl methacrylate, 4-6% of glycidyl methacrylate, 0.8-1.2% of azobisisobutyronitrile and the remainder of the second solvent.

[0010] More specifically, in the above technical solution, the preparation method of the modified fluorocarbon resin includes: mixing the raw materials of the modified fluorocarbon resin uniformly in proportion, stirring at a speed of 100-200 rpm for 6-10 hours at 110-130°C, and cooling, washing and drying in sequence.

[0011] More specifically, in the above technical solution, the anti-fog masterbatch comprises the following components, calculated by weight: 0.8-2 parts of vinyl triethoxy silane.

[0012] More specifically, in the above technical solution, the initiator includes at least one of di-tert-butyl hydroperoxide, 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane, di-tert-butyl peroxide, diisopropylbenzene peroxide and benzoyl peroxide.

[0013] More specifically, in the above technical solution, the solvent is ethyl acetate.

[0014] The present application also proposes a method for preparing an anti-fog masterbatch suitable for a biaxial stretching process, comprising heating and stirring the raw material components of the anti-fog masterbatch described in any one of the above items in proportion, recovering the solvent to obtain a polymer, putting the polymer, polypropylene pellets and sodium dicyclohexyl sulfosuccinate into an extruder, extruding, water-cooling and then pelletizing to obtain the anti-fog masterbatch.

[0015] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0016] Firstly, the present application overcomes the defect that the anti-fog effect of the traditional hydrophilic group anti-fog masterbatch is non-permanent, and realizes long-lasting anti-fog performance through the hydrophobic design; secondly, the anti-fog masterbatch of the present application solves the problem that the anti-fog masterbatch containing silicon and fluorine cannot be printed. The anti-fog masterbatch of the present application has excellent printability and does not require additional labeling, thereby reducing production costs; furthermore, the anti-fog masterbatch of the present application has low VOC emissions during the production process and excellent environmental protection performance, while avoiding the accumulation of oligomers on the die lip, thereby improving the stability and quality of film processing; more importantly, the polymer structure and molecular chain designed in the present application significantly enhance the bonding force between the ink layer and the packaging film, so that the anti-fog film has good printing adaptability while maintaining excellent anti-fog effect, greatly broadening the application field and market prospects of the product. DETAILED DESCRIPTION

[0017] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0019] References to "one embodiment" or "some embodiments" etc. described in the specification of this application mean that one or more embodiments of the present application include specific features, structures or characteristics described in conjunction with the embodiment. Therefore, the phrase "in some embodiments" appearing in different places in this specification does not necessarily refer to the same embodiment, but means "one or more but not all embodiments", unless otherwise specifically emphasized in other ways. The terms "including", "comprising", "having" and their variations all mean "including but not limited to", unless otherwise specifically emphasized in other ways.

[0020] The materials and reagents in this application can be purchased from the market.

[0021] The present application proposes an anti-fog masterbatch suitable for a biaxial stretching process. The anti-fog masterbatch of the present application is suitable for PET, BOPET, CPP, BOPP, CPE or BOPE films, and can be used as a matte layer material for cast, uniaxially stretched or biaxially stretched films. The anti-fog masterbatch is calculated by weight and includes the following components: 4-5 parts of methacrylic resin, 2-4 parts of acrylic acid, 1-2 parts of 1,4-butanediol dimethacrylate, 1-2 parts of 2-(dimethylamino)ethyl methacrylate, 0.05-0.1 parts of an initiator, and 8-12 parts of a first solvent.

[0022] Firstly, the present application overcomes the defect that the anti-fog effect of the traditional hydrophilic group anti-fog masterbatch is non-permanent, and realizes long-lasting anti-fog performance through the hydrophobic design; secondly, the anti-fog masterbatch of the present application solves the problem that the anti-fog masterbatch containing silicon and fluorine cannot be printed. The anti-fog masterbatch of the present application has excellent printability and does not require additional labeling, thereby reducing production costs; furthermore, the anti-fog masterbatch of the present application has low VOC emissions during the production process and excellent environmental protection performance, while avoiding the accumulation of oligomers on the die lip, thereby improving the stability and quality of film processing; more importantly, the polymer structure and molecular chain designed in the present application significantly enhance the bonding force between the ink layer and the packaging film, so that the anti-fog film has good printing adaptability while maintaining excellent anti-fog effect, greatly broadening the application field and market prospects of the product.

[0023] On the other hand, the anti-fog masterbatch of the present application also does not contain amide polymerization monomers. In the prior art CN113088131A, due to the presence of amide polymers, the VOC emission during the extrusion process may be high. After film formation, the polymers, such as oleamide and erucamide, will migrate to the surface of the film, resulting in a decrease in the bonding force between the ink layer and the packaging film.

[0024] The anti-fog layer of the present application is formed by polymerization of monomers, and the oligomers can be reduced by extending the polymerization time or by reducing the titration rate of the polymerization process. Therefore, the VOC emission during the extrusion film forming process is low, and there are almost no migratable oligomers after film forming to affect the bonding strength between the ink layer and the packaging film. In addition, in the anti-fog masterbatch of the present application, methacrylic acid resin, acrylic acid, 1,4-butanediol dimethacrylate and 2-(dimethylamino)ethyl methacrylate can provide bonding strength with the dispersed phase in the oil-based ink (currently in the printing industry, the dispersed phase of the oil-based ink is mainly ethyl acetate and butyl acetate). The principle is the electrical effect between polar molecules. Microscopically, the compatibility between carboxyl, hydroxyl and ester groups is high, which is reflected in the improved bonding strength between the ink layer and the packaging film on a macro scale. Anti-fog principle: After the polymerization of methacrylate resin, acrylic acid, 1,4-butanediol dimethacrylate and 2-(dimethylamino)ethyl methacrylate, the methyl, ethyl and other alkane branches on the molecular side chains are water-repellent. The interaction of the four components and the control of the polymerization ratio can indirectly control the number and relative position of the methyl and ethyl groups on the side chains, thereby adjusting the spatial steric hindrance of the molecular chain to prevent water vapor from forming water mist and only forming larger water droplets that roll down.

[0025] The methacrylic acid resin and acrylic acid in this application were purchased from BASF AG of Germany; 1,4-butanediol dimethacrylate was purchased from Celanese Corporation of the United States or Shanghai MacLean Biochemical Technology Co., Ltd.; 2-(dimethylamino)ethyl methacrylate was purchased from Qingdao Reinars Polymer Materials Co., Ltd.

[0026] In some embodiments, the anti-fog masterbatch includes the following components, calculated by weight: 5 parts of methacrylic resin, 2 parts of acrylic acid, 2 parts of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, 0.05 parts of initiator and 10 parts of the first solvent.

[0027] The specific combination of methacrylate resin, acrylic acid, 1,4-butanediol dimethacrylate and 2-(dimethylamino)ethyl methacrylate is controlled to the above-mentioned polymerization ratio so that the methyl, ethyl and other alkane side chains on the molecular chain are optimally distributed, thereby realizing a hydrophobic effect at the micron level, effectively preventing water vapor from condensing into fog on the surface of the film, and only forming larger water droplets that roll down, ensuring a long-term and stable anti-fog effect.

[0028] In some embodiments, the anti-fog masterbatch includes the following components, calculated by weight: 4 parts of methacrylic resin, 4 parts of acrylic acid, 1 part of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, 0.05 parts of di-tert-butyl peroxide and 10 parts of the first solvent.

[0029] In some specifically optimized embodiments, the ratio of the anti-fog masterbatch has been carefully adjusted to show unique advantages. Specifically, the anti-fog masterbatch is based on 4 parts of methacrylic resin and supplemented with 4 parts of acrylic acid. This combination not only enhances the stability of the material, but also improves its overall performance. At the same time, the addition of 1 part of 1,4-butanediol dimethacrylate and 1 part of 2-(dimethylamino)ethyl methacrylate effectively regulates the molecular structure of the polymer, giving it better hydrophobicity and anti-fog effect. In addition, a trace amount of initiator ensures the smooth progress of the polymerization reaction, and its high efficiency reduces the generation of by-products, further improving the purity of the product.

[0030] In some embodiments, the anti-fog masterbatch comprises the following components, calculated by weight: 0.5-3 parts of modified fluorocarbon resin.

[0031] Fluorocarbon resin has extremely low surface energy and is an ideal choice for preparing water-repellent materials. The present application modifies the fluorocarbon resin so that the modified fluorocarbon resin can maintain good compatibility with oil-based inks and substrates while maintaining water-repellent properties. That is, the modified fluorocarbon resin of the present application can effectively prevent water vapor from condensing into fog on the surface of the film due to its unique chemical structure and low surface energy characteristics, thereby further improving the durability of the anti-fog effect; compared with traditional hydrophilic group anti-fog masterbatch, its anti-fog effect is more stable and less susceptible to changes in environmental humidity.

[0032] In some embodiments, the modified fluorocarbon resin comprises, by weight percentage, 50-60% fluorocarbon resin matrix, 18-22% methyl methacrylate, 4-6% glycidyl methacrylate, 0.8-1.2% azobisisobutyronitrile and the remainder a second solvent. Preferably, the fluorocarbon resin matrix is ​​polychlorotrifluoroethylene and the second solvent is isopropanol.

[0033] By introducing methyl methacrylate (MMA, 18-22%) and glycidyl methacrylate (GMA, 4-6%) as modified monomers, the modified fluorocarbon resin has extremely high compatibility with the dispersed phase in the oil-based ink. The polar groups formed by these monomers during the polymerization process enhance the binding force with the ink layer, making the anti-fog film not only have a good anti-fog effect, but also meet various printing needs, without the need for additional labeling, reducing production costs.

[0034] In some embodiments, the preparation method of the modified fluorocarbon resin includes: uniformly mixing the raw materials of the modified fluorocarbon resin according to a certain proportion, stirring at a speed of 100-200 rpm for 6-10 hours at a temperature of 110-130° C., and sequentially cooling, washing, and drying.

[0035] Specifically, a method for preparing a modified fluorocarbon resin is as follows: 55% of polytrifluorochloroethylene, 18% of methyl methacrylate (MMA), 4% of glycidyl methacrylate (GMA), 1% of azobisisobutyronitrile (AI BN) and 22% of isopropanol are added to the modified fluorocarbon resin by mass percentage, stirred at 120°C and 150 rpm for 8 hours, after the reaction is completed, the reaction solution is cooled to room temperature, and unreacted monomers and solvents are removed by filtering, washing and drying to obtain a pure modified fluorocarbon resin. The modified fluorocarbon resin in the embodiment is prepared by this method.

[0036] In some embodiments, the anti-fog masterbatch comprises the following components, calculated by weight: 0.8-2 parts of vinyl triethoxy silane.

[0037] Vinyl triethoxysilane can be used as a crosslinking agent in the anti-fog masterbatch of the present application. The crosslinking agent makes the surface of the polymer generated by the reaction denser, greatly reduces the penetration path and attachment points of water molecules, and effectively prevents the condensation of water vapor on the surface of the film, thereby significantly improving the anti-fog effect.

[0038] In addition, the generated cross-linked structure can increase the stability and durability of the anti-fog masterbatch, making the anti-fog effect more durable. When environmental factors such as temperature and humidity fluctuate, the cross-linked structure can effectively resist the adverse effects of these factors and maintain the long-term stability of the anti-fog performance.

[0039] In some embodiments, the initiator includes at least one of di-tert-butyl hydroperoxide, 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, di-tert-butyl peroxide, dicumyl peroxide and benzoyl peroxide. Preferably, the initiator is di-tert-butyl peroxide (CAS No.: 110-05-4).

[0040] As a highly efficient initiator, di-tert-butyl peroxide can accelerate the polymerization rate, effectively shorten the production cycle and improve production efficiency. Compared with other initiators, di-tert-butyl peroxide produces fewer by-products during the polymerization reaction, which helps to maintain the purity and quality stability of the product, reduce the complexity and cost of subsequent processing steps, and improve the market competitiveness of the product.

[0041] By using di-tert-butyl peroxide as an efficient initiator, the molecular structure and segment distribution of the polymer can be optimized, further improving the performance of the anti-fog masterbatch. For example, the number and position of alkane side chains such as methyl and ethyl in the polymer can be controlled to achieve better hydrophobic and anti-fog effects.

[0042] In some embodiments, the solvent is ethyl acetate.

[0043] First, as a commonly used organic solvent, ethyl acetate has relatively low volatility, which helps to reduce the emission of volatile organic compounds (VOC) during the preparation process, thus meeting the current requirements of environmentally friendly production and reducing pollution to the environment. Secondly, ethyl acetate has good solubility in raw materials such as methacrylate resin and acrylic acid, which helps to evenly disperse the raw materials in the solvent, making the subsequent polymerization reaction more sufficient and uniform, and improving the quality and stability of the product. Finally, since the dispersed phase of oil-based inks in the printing industry is mainly ester solvents such as ethyl acetate, the anti-fog masterbatch prepared by selecting ethyl acetate as the solvent can show better compatibility with the ink layer in the subsequent printing process, improve ink adhesion, and reduce printing defects.

[0044] The present application also proposes a method for preparing an anti-fog masterbatch suitable for a biaxial stretching process, comprising heating and stirring the raw material components of the anti-fog masterbatch described in any one of the above items in proportion, recovering the solvent to obtain a polymer, putting the polymer, polypropylene pellets and sodium dicyclohexyl sulfosuccinate into an extruder, extruding, water-cooling and then pelletizing to obtain the anti-fog masterbatch.

[0045] The anti-fog masterbatch prepared by the method of the present application can significantly improve the anti-fog effect, printability and environmental protection performance of the film.

[0046] The raw materials and equipment used in this application, unless otherwise specified, are all commonly used raw materials and equipment in this field; the methods used in this invention, unless otherwise specified, are all conventional methods in this field.

[0047] Unless otherwise specified, the meanings of the terms in this specification are the same as those generally understood by those skilled in the art. However, if there is any conflict, the definitions in this specification shall prevail.

[0048] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0049] Embodiment 1:

[0050] The anti-fog masterbatch is calculated by weight: 10 parts of ethyl acetate, 5 parts of methacrylic resin, 2 parts of acrylic acid, 2 parts of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, and 0.05 parts of di-tert-butyl peroxide are mixed evenly in a premixing kettle and then put into the reactor. The titration speed is 60kg / h, the reactor temperature is controlled at 85 degrees Celsius, and the titration is completed at 90℃ for 2 hours. Part of the ethyl acetate is recovered during the insulation process.

[0051] The desired anti-fogging masterbatch is obtained after the solvent ethyl acetate is recovered.

[0052] Processing stage: 4 parts of anti-fog masterbatch, 6 parts of polypropylene pellets, 0.05 parts of sodium dicyclohexyl sulfosuccinate are added to the anti-fog film anti-fog layer raw material additives by weight, and put into the extruder, the extruder feeding section is 40℃, the melting section is 220℃, the homogenization section is 220℃, and the shear rate is 130rpm. The extruded strip material is water-cooled at 20℃ and then pelletized.

[0053] The obtained pellets are used as raw material additives for the anti-fog layer of the anti-fog film, and the surface layer addition accounts for 10% of the total proportion of the film. After the conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), the conventional BOPP processing steps are common knowledge in the field and are not described in detail in this application. After processing, the anti-fog film is obtained by quenching and biaxial stretching.

[0054] Example 1 test results:

[0055] After 8 hours of continuous production, no oil droplets or condensate were found at the die lip; the maximum VOC emission in the extrusion area was 20 mg / m 3 The anti-fog effect of the finished film reaches the level 1 anti-fog effect specified in GBT 31726-2015. The film has excellent printing effect after electrode treatment, and the ink adhesion is ≥47N / 15mm.

[0056] Note: Anti-fog level 1: completely transparent, no water droplets; the clarity of the eye chart is exactly the same as before the test. Anti-fog level 2: good transparency, a small amount of uneven large water droplets, more than 50% of the clarity of the eye chart is exactly the same as before the test. Anti-fog level 3: basically transparent, with more water droplets, the font of the eye chart is deformed (the same below).

[0057] Embodiment 2:

[0058] The anti-fog masterbatch is calculated by weight: 10 parts of ethyl acetate, 4 parts of methacrylic resin, 4 parts of acrylic acid, 1 part of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, and 0.05 parts of di-tert-butyl peroxide are mixed evenly in a premixing kettle and then put into the reactor. The titration speed is 60kg / h, the reactor temperature is controlled at 85 degrees Celsius, and the titration is completed at 90℃ for 2 hours. Part of the ethyl acetate is recovered during the insulation process.

[0059] The desired anti-fogging masterbatch is obtained after the solvent ethyl acetate is recovered.

[0060] Processing stage: 4 parts of anti-fog masterbatch, 6 parts of polypropylene pellets, 0.05 parts of sodium dicyclohexyl sulfosuccinate are added to the anti-fog film anti-fog layer raw material additives by weight, and put into the extruder, the extruder feeding section is 40℃, the melting section is 220℃, the homogenization section is 220℃, and the shear rate is 130rpm. The extruded strip material is water-cooled at 20℃ and then pelletized.

[0061] The obtained pellets are used as raw material additives for the anti-fog layer of the anti-fog film. The surface layer is added to 10% of the total proportion of the film, and the anti-fog film is obtained through conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), and then quenched and biaxially stretched.

[0062] Example 2 test results:

[0063] After 8 hours of continuous production, no oil droplets or condensate were found at the die lip; the maximum VOC emission in the extrusion area was 45 mg / m 3 The anti-fog effect of the finished film reaches the second level anti-fog effect specified in GBT 31726-2015. The film has excellent printing effect after electrode treatment, and the ink adhesion is ≥47N / 15mm.

[0064] Embodiment 3:

[0065] The anti-fog masterbatch is calculated by weight: 10 parts of ethyl acetate, 5 parts of methacrylic acid resin, 2 parts of acrylic acid, 2 parts of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, 0.05 parts of di-tert-butyl peroxide and 2.5 parts of modified fluorocarbon resin are mixed evenly in a pre-mixing kettle and then put into the reactor. The titration speed is 60kg / h, the reactor temperature is controlled at 85 degrees Celsius, and the titration is completed at 90℃ for 2h. Part of the ethyl acetate is recovered during the insulation process.

[0066] The desired anti-fogging masterbatch is obtained after the solvent ethyl acetate is recovered.

[0067] Processing stage: 4 parts of anti-fog masterbatch, 6 parts of polypropylene pellets, 0.05 parts of sodium dicyclohexyl sulfosuccinate are added to the anti-fog film anti-fog layer raw material additives by weight, and put into the extruder, the extruder feeding section is 40℃, the melting section is 220℃, the homogenization section is 220℃, and the shear rate is 130rpm. The extruded strip material is water-cooled at 20℃ and then pelletized.

[0068] The obtained pellets are used as raw material additives for the anti-fog layer of the anti-fog film, and the surface layer addition accounts for 10% of the total proportion of the film. After the conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), the anti-fog film is obtained by quenching and biaxial stretching.

[0069] Example 3 test results:

[0070] After 8 hours of continuous production, no oil droplets or condensate were found at the die lip; the maximum VOC emission in the extrusion area was 15 mg / m 3The anti-fog effect of the finished film reaches the level 1 anti-fog effect specified in GBT 31726-2015. The film has excellent printing effect after electrode treatment, and the ink adhesion is ≥52N / 15mm.

[0071] Example 3 includes a modified fluorocarbon resin, the introduction of which further improves the anti-fogging effect and enhances the compatibility with oil-based inks. The polar groups formed by monomers such as methyl methacrylate (MMA) and glycidyl methacrylate (GMA) in the modified fluorocarbon resin during the polymerization process also help to enhance the bonding between the ink layer and the packaging film.

[0072] Embodiment 4:

[0073] The anti-fog masterbatch is calculated by weight: 10 parts of ethyl acetate, 4 parts of methacrylic resin, 4 parts of acrylic acid, 1 part of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, 0.05 parts of di-tert-butyl peroxide and 1.6 parts of vinyl triethoxysilane are mixed evenly in a pre-mixing kettle and then put into the reactor. The titration speed is 60kg / h, the reactor temperature is controlled at 85 degrees Celsius, and the titration is completed at 90℃ for 2h. Part of the ethyl acetate is recovered during the insulation process.

[0074] The desired anti-fogging masterbatch is obtained after the solvent ethyl acetate is recovered.

[0075] Processing stage: 4 parts of anti-fog masterbatch, 6 parts of polypropylene pellets, 0.05 parts of sodium dicyclohexyl sulfosuccinate are added to the anti-fog film anti-fog layer raw material additives by weight, and put into the extruder, the extruder feeding section is 40℃, the melting section is 220℃, the homogenization section is 220℃, and the shear rate is 130rpm. The extruded strip material is water-cooled at 20℃ and then pelletized.

[0076] The obtained pellets are used as raw material additives for the anti-fog layer of the anti-fog film. The surface layer is added to 10% of the total proportion of the film, and the anti-fog film is obtained through conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), and then quenched and biaxially stretched.

[0077] Example 4 test results:

[0078] After 8 hours of continuous production, no oil droplets or condensate were found at the die lip; the maximum VOC emission in the extrusion area was 40 mg / m 3 The anti-fog effect of the finished film reaches the level 1 anti-fog effect specified in GBT 31726-2015. The film has excellent printing effect after electrode treatment, and the ink adhesion is ≥51N / 15mm.

[0079] Vinyl triethoxysilane can be used as a crosslinking agent in the anti-fog masterbatch of the present application. The crosslinking agent makes the surface of the polymer generated by the reaction denser, greatly reduces the penetration path and attachment points of water molecules, and effectively prevents the condensation of water vapor on the surface of the film, thereby significantly improving the anti-fog effect.

[0080] In addition, the generated cross-linked structure can increase the stability and durability of the anti-fog masterbatch, making the anti-fog effect more durable. When environmental factors such as temperature and humidity fluctuate, the cross-linked structure can effectively resist the adverse effects of these factors and maintain the long-term stability of the anti-fog performance.

[0081] Comparative Example 1:

[0082] The amine and hydroxyl anti-fog masterbatch additives on the market are used. The surface layer is added to 10% of the total film ratio, and the anti-fog film is obtained after the conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), and then quenched and biaxially stretched.

[0083] Comparative Example 1 test results:

[0084] After 4 hours of continuous production, a small amount of oil droplets and condensate were found at the die lip; the maximum VOC emission in the extrusion area was 80 mg / m 3 The anti-fog effect of the finished film reaches the level 1 anti-fog effect specified in GBT 31726-2015. The film has good printing effect after electrode treatment, and the ink adhesion is ≥42N / 15mm.

[0085] Comparative Example 2:

[0086] The silicon and fluorine anti-fog masterbatch additives on the market are used. The surface layer is added to 10% of the total film ratio, and the anti-fog film is obtained after the conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), and then quenched and biaxially stretched.

[0087] Comparative Example 2 test results:

[0088] After 4 hours of continuous production, a small amount of oil droplets and condensate were found at the die lip; the maximum VOC emission in the extrusion area was 10mg / m 3 The anti-fog effect of the finished film reaches the level 1 anti-fog effect specified in GBT 31726-2015. The film has poor effect after printing after electrode treatment, and the ink adhesion is ≤18N / 15mm.

[0089] Comparative Example 3:

[0090] In the anti-fog masterbatch, calculated by weight: 10 parts of ethyl acetate, 4 parts of methacrylic resin, 3 parts of 1,4-butanediol dimethacrylate, 3 parts of 2-(dimethylamino)ethyl methacrylate, and 0.05 parts of di-tert-butyl peroxide were mixed evenly in a premixing kettle and then put into the reactor. The titration speed was 60kg / h, the reactor temperature was controlled at 85 degrees Celsius, and the temperature was kept at 90°C for 2 hours after the titration was completed. Part of the ethyl acetate was recovered during the insulation process.

[0091] The desired anti-fogging masterbatch is obtained after the solvent ethyl acetate is recovered.

[0092] Processing stage: 4 parts of polymer, 6 parts of polypropylene pellets, 0.05 parts of sodium dicyclohexyl sulfosuccinate are added to the raw material additives of the anti-fog film by weight, and put into the extruder. The feeding section of the extruder is 40°C, the melting section is 220°C, the homogenization section is 220°C, and the shear rate is 130rpm. The extruded strip material is water-cooled at 20°C and then pelletized.

[0093] The obtained pellets are used as raw material additives for the anti-fog layer of the anti-fog film. The surface layer is added to 10% of the total proportion of the film, and the anti-fog film is obtained through conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), and then quenched and biaxially stretched.

[0094] Comparative Example 3 test results:

[0095] After 8 hours of continuous production, no oil droplets or condensate were found at the die lip; the maximum VOC emission in the extrusion area was 45 mg / m 3 The anti-fog effect of the finished film reaches the second level anti-fog effect specified in GBT 31726-2015. The film has good printing effect after electrode treatment, and the ink adhesion is ≤25N / 15mm.

[0096] No acrylic acid was added to Comparative Example 3, and the test results showed that its anti-fog effect was significantly reduced. Acrylic acid not only participates in the polymerization reaction in the formula, but also interacts with other components to form a molecular structure with excellent anti-fog performance. The lack of acrylic acid weakens this synergistic effect, thereby affecting the anti-fog effect.

[0097] Comparative Example 4:

[0098] In the anti-fog masterbatch, calculated by weight: 10 parts of ethyl acetate, 4 parts of methacrylic resin, 3 parts of acrylic acid, 3 parts of 1,4-butanediol dimethacrylate, 0.05 parts of di-tert-butyl peroxide (CAS No.: 110-05-4) were mixed evenly in the pre-mixing kettle and then put into the reactor. The titration speed was 60kg / h, the reactor temperature was controlled at 85 degrees Celsius, and the temperature was kept at 90℃ for 2h after the titration was completed. Part of the ethyl acetate was recovered during the insulation process.

[0099] The desired anti-fogging masterbatch is obtained after the solvent ethyl acetate is recovered.

[0100] Processing stage: 4 parts of polymer, 6 parts of polypropylene pellets, 0.05 parts of sodium dicyclohexyl sulfosuccinate are added to the raw material additives of the anti-fog film by weight, and put into the extruder. The feeding section of the extruder is 40°C, the melting section is 220°C, the homogenization section is 220°C, and the shear rate is 130rpm. The extruded strip material is water-cooled at 20°C and then pelletized.

[0101] The obtained pellets are used as raw material additives for the anti-fog layer of the anti-fog film. The surface layer is added to 10% of the total proportion of the film, and the anti-fog film is obtained through conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), and then quenched and biaxially stretched.

[0102] Comparative Example 4 test results:

[0103] After 8 hours of continuous production, no oil droplets or condensate were found at the die lip; the maximum VOC emission in the extrusion area was 25 mg / m 3 The anti-fog effect of the finished film reaches the level 3 anti-fog effect specified in GBT 31726-2015. The film has good printing effect after electrode treatment, and the ink adhesion is ≥40N / 15mm.

[0104] In comparative example 4, 1,4-butanediol dimethacrylate was not added, and the test results showed that the hydrophobicity and anti-fog effect of the film were reduced. As an important cross-linking monomer, 1,4-butanediol dimethacrylate is crucial for regulating the molecular structure of the polymer and improving the hydrophobicity. Its absence leads to a decrease in the branching degree and steric hindrance of the molecular chain, thereby affecting the anti-fog effect.

[0105] In addition, the absence of 1,4-butanediol dimethacrylate will reduce the degree of molecular chain branching of the polymer, thereby affecting its surface morphology and the distribution of polar groups, reducing the interaction between the polymer and the polar dispersed phase in the ink, and thus weakening the bonding between the ink layer and the packaging film. Due to the contribution of 1,4-butanediol dimethacrylate to hydrophobic properties, its absence will also reduce the water contact angle on the film surface, increase the wettability of the film surface, and be detrimental to the uniform adhesion of the ink and the stable bonding during the drying process.

[0106] Comparative Example 5:

[0107] In the anti-fog masterbatch, calculated by weight: 10 parts of ethyl acetate, 4 parts of methacrylic resin, 3 parts of acrylic acid, 3 parts of 2-(dimethylamino)ethyl methacrylate, and 0.05 parts of di-tert-butyl peroxide are mixed evenly in a pre-mixing kettle and then put into the reactor. The titration speed is 60kg / h, the reactor temperature is controlled at 85 degrees Celsius, and the titration is completed at 90°C for 2 hours. Part of the ethyl acetate is recovered during the insulation process.

[0108] The desired anti-fogging masterbatch is obtained after the solvent ethyl acetate is recovered.

[0109] Processing stage: 4 parts of polymer, 6 parts of polypropylene pellets, 0.05 parts of sodium dicyclohexyl sulfosuccinate are added to the raw material additives of the anti-fog film by weight, and put into the extruder. The feeding section of the extruder is 40°C, the melting section is 220°C, the homogenization section is 220°C, and the shear rate is 130rpm. The extruded strip material is water-cooled at 20°C and then pelletized.

[0110] The obtained pellets are used as raw material additives for the anti-fog layer of the anti-fog film. The surface layer is added to 10% of the total proportion of the film, and the anti-fog film is obtained through conventional BOPP processing steps (extruder feeding section 35°C, melting section 220°C, homogenization section 220°C, shear rate 90rpm), and then quenched and biaxially stretched.

[0111] Comparative Example 5 test results:

[0112] After 8 hours of continuous production, no oil droplets or condensate were found at the die lip; the maximum VOC emission in the extrusion area was 10mg / m 3 The anti-fog effect of the finished film reaches the level 3 anti-fog effect specified in GBT 31726-2015. The film has good printing effect after electrode treatment, and the ink adhesion is ≥35N / 15mm.

[0113] In Comparative Example 5, 2-(dimethylamino)ethyl methacrylate was not added, and the test results showed that the anti-fog durability of the film was deteriorated. 2-(dimethylamino)ethyl methacrylate enhanced the interaction with other components in the formula through its unique functional groups (such as aminoethyl ester groups) and helped to form a stable hydrophobic layer. Its absence made the structure of the hydrophobic layer unstable, and the anti-fog effect was difficult to last.

[0114] On the other hand, the absence of 2-(dimethylamino)ethyl methacrylate makes it impossible to form enough cross-linking points between the molecular chains in the anti-fog masterbatch, which reduces the penetration and anchoring of ink molecules on the film surface, and the ink layer is more likely to peel or fall off, reducing the overall printing quality and durability of the product. Therefore, the presence of 2-(dimethylamino)ethyl methacrylate in the formula is crucial to ensure the long-lasting anti-fog effect and good ink adhesion of the anti-fog film.

[0115] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0116] The above-described embodiments only express several embodiments of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.

Claims

1. An anti-fog masterbatch suitable for biaxial stretching process, It is characterized in that The anti-fog masterbatch comprises the following components calculated by weight: 4-5 parts of methacrylic resin, 2-4 parts of acrylic acid, 1-2 parts of 1,4-butanediol dimethacrylate, 1-2 parts of 2-(dimethylamino)ethyl methacrylate, 0.05-0.1 parts of initiator and 8-12 parts of the first solvent.

2. The anti-fog masterbatch suitable for biaxial stretching process according to claim 1, It is characterized in that The anti-fog masterbatch includes the following components, calculated by weight: 5 parts of methacrylic resin, 2 parts of acrylic acid, 2 parts of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, 0.05 parts of initiator and 10 parts of the first solvent.

3. The anti-fog masterbatch suitable for biaxial stretching process according to claim 1, It is characterized in that The anti-fog masterbatch includes the following components, calculated by weight: 4 parts of methacrylic resin, 4 parts of acrylic acid, 1 part of 1,4-butanediol dimethacrylate, 1 part of 2-(dimethylamino)ethyl methacrylate, 0.05 parts of di-tert-butyl peroxide and 10 parts of the first solvent.

4. The anti-fog masterbatch suitable for biaxial stretching process according to claim 1, It is characterized in that The anti-fog masterbatch comprises the following components calculated by weight: 0.5-3 parts of modified fluorocarbon resin.

5. The anti-fog masterbatch suitable for biaxial stretching process according to claim 4, It is characterized in that The modified fluorocarbon resin comprises, by weight percentage, 50-60% of a fluorocarbon resin matrix, 18-22% of methyl methacrylate, 4-6% of glycidyl methacrylate, 0.8-1.2% of azobisisobutyronitrile and the remainder of a second solvent.

6. The anti-fog masterbatch suitable for biaxial stretching process according to claim 5, It is characterized in that The preparation method of the modified fluorocarbon resin comprises: uniformly mixing the raw materials of the modified fluorocarbon resin according to a certain proportion, stirring at a speed of 100-200 rpm for 6-10 hours at a temperature of 110-130° C., and cooling, washing and drying in sequence.

7. The anti-fog masterbatch suitable for biaxial stretching process according to claim 1, It is characterized in that The anti-fog masterbatch comprises the following components calculated by weight: 0.8-2 parts of vinyl triethoxy silane.

8. The anti-fog masterbatch suitable for biaxial stretching process according to any one of claims 1 to 7, It is characterized in that The initiator includes at least one of di-tert-butyl hydroperoxide, 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, di-tert-butyl peroxide, dicumyl peroxide and benzoyl peroxide.

9. The anti-fogging masterbatch suitable for biaxial stretching process according to any one of claims 1 to 7, It is characterized in that The solvent is ethyl acetate.

10. A method for preparing an anti-fogging masterbatch suitable for a biaxial stretching process, It is characterized in that The method comprises heating the raw material components of the anti-fog masterbatch according to any one of claims 1 to 9 in proportion and stirring and mixing, recovering the solvent to obtain a polymer, putting the polymer, polypropylene pellets and sodium dicyclohexyl sulfosuccinate into an extruder, extruding, water-cooling and then pelletizing to obtain the anti-fog masterbatch.

Citation Information

Patent Citations

  • Preparation method of antifogging and antireflection film coating liquid

    CN104449185A

  • Preparation method of acrylic quaternary ammonium salt film with contact antibiosis and antifogging functions

    CN112592419A

  • Anti-fogging coating composition, product coated with said composition and method for preparation of said product

    US5480917A