Method for preparing high-strength damping sound insulation material by recycling waste fan blades

By recycling waste fan blades and preparing high-strength damping sound insulation materials, the problems of insufficient damping performance of rubber damping materials and agglomeration of inorganic powders are solved, the combination of high-strength, excellent damping performance and mechanical properties is achieved, and the resource circulation is realized. use.

CN118931085AInactive Publication Date: 2024-11-12ANHUI ZHONGXIAN NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411184550.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing rubber damping materials have a small number of monomer side chains and polar functional groups, resulting in insufficient damping performance, and inorganic powders are prone to agglomeration in organic damping materials, reducing mechanical properties.

Method used

By removing and cutting the waste fan blades, sieving them after pyrolysis to obtain inorganic powder material, and using copolymer rubber, supramolecular materials, epoxy resin, etc., high-strength damping sound insulation materials are prepared through mixing and sulfurization processes to increase the materials damping and mechanical properties.

Benefits of technology

The prepared high-strength damping sound insulation material has excellent mechanical properties and damping properties, which can effectively improve the waterproof performance and sound insulation effect of rubber, reduce the self-aggregation effect of glass fibers, and realize the recycling of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013150230000031
    Figure BDA0005013150230000031
  • Figure BDA0005013150230000041
    Figure BDA0005013150230000041
  • Figure BDA0005013150230000042
    Figure BDA0005013150230000042
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-strength damping sound insulation material by recycling waste fan blades, and aims to solve the technical problems that in monomers of synthetic rubber damping materials in the prior art, the number of side chains and polar functional groups is small, damping performance cannot be improved easily, and organic damping materials are poor in mechanical performance. The method comprises the following steps: processing the waste fan blade to obtain an inorganic powder material; the high-strength damping sound insulation material is prepared by mixing copolymer rubber, a supramolecular material, an inorganic powder material, epoxy resin and the like and performing mixing and vulcanization processes, vinyl acetate is used as a soft segment chain, styrene is used as a hard segment chain, tetrafluoroethylene is added, and the copolymer rubber with water resistance, high temperature resistance, good mechanical performance and good damping performance is obtained. The supramolecular material has more chain segments and polar functional groups, not only has strong damping and sound insulation properties, but also can be used as a buffer intermediate to improve the uniform distribution of an inorganic powder material in matrix resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of damping materials, and in particular to a method for preparing high-strength damping sound insulation materials by recycling waste fan blades. Background Art

[0002] Vibration and noise are often linked together. Vibration can cause noise, and noise can be converted into vibration. The hazards of vibration and noise are mainly manifested in: damage to human hearing and nervous system. Wide-band random vibration can cause multi-level resonance of the structure, making it difficult for equipment, instruments and meters to work normally.

[0003] Polymer materials represented by rubber have the advantages of outstanding elasticity, large internal friction and strong damping effect, and are most suitable for making damping materials. However, rubber damping materials synthesized from monomers such as styrene and butadiene have poor waterproof and corrosion resistance, and the number of side chains and polar functional groups is small, which is not conducive to improving their own damping performance. In addition, how to further improve the mechanical properties of rubber damping materials is also a technical problem that needs to be solved urgently.

[0004] As a solid waste from an emerging industry, fan blades were initially treated by incineration. The incineration process produces a large amount of smoke and a large amount of pollutants. The main material of fan blades is usually a glass fiber composite material. After retirement, the glass fiber still has excellent mechanical properties. If the glass fiber in the fan blades is treated and added to the preparation of damping and sound insulation materials, the strength of the damping and sound insulation materials can be effectively improved, and the recycling of resources can be achieved. However, inorganic powders are prone to agglomeration in rubber base materials, which reduces their mechanical properties such as tensile strength and elongation at break.

[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for recycling waste fan blades to prepare high-strength damping sound insulation materials, which is used to solve the technical problems that the synthetic rubber damping materials in the prior art have a small number of monomer side chains and polar functional groups, which is not conducive to improving their own damping performance; as well as the poor mechanical properties of organic damping materials and the easy agglomeration of inorganic materials in organic damping materials.

[0007] The object of the present invention can be achieved by the following technical solution: A method for recycling waste fan blades to prepare high-strength damping sound insulation materials comprises the following steps:

[0008] S1. Dismantle and cut the waste fan blades, collect the skin, interlayer and blade root respectively; feed the skin into a pyrolysis reactor, perform micro-negative pressure pyrolysis, and collect the solid product; grind the solid product and then sieve it with a vibrating screen machine, and the particle size range of the standard sieve is 0.3-2.36mm to obtain an inorganic powder material;

[0009] The fan blades include skin, interlayer and blade root. The interlayer is PVC, PET or balsa wood, the blade root is a metal part, the skin includes glass fiber, carbon fiber and resin, and the main material of the fan blade is generally a composite material of glass fiber and epoxy resin. Both of the above main materials are difficult to degrade;

[0010] The present invention comprises the steps of dismantling and cutting waste fan blades, collecting the components respectively, pyrolyzing the skin, removing the coating material and resin components on the surface, grinding the solid product, and then sieving to obtain inorganic powder material with a certain particle size.

[0011] S2, according to parts by weight, the copolymer rubber, supramolecular material, inorganic powder material, epoxy resin, sulfur, ZnO, stearic acid and accelerator NS are mixed, and added into a rubber mixer for mixing to obtain a rubber material;

[0012] S3. The rubber material is added into a flat vulcanizer for vulcanization at a vulcanization temperature of 170-180° C., a vulcanization pressure of 4-5 MPa, and a vulcanization time of 10-20 min to obtain a high-strength damping sound insulation material.

[0013] The high-strength damping sound insulation material prepared by the invention uses copolymer rubber as a base material, and the copolymer rubber, supramolecular material, inorganic powder material and epoxy resin are all solid. The production method of rubber products is adopted, and the high-strength damping sound insulation material is obtained through mixing and vulcanization processes.

[0014] Furthermore, in step S2, the method for preparing the copolymer rubber comprises the following steps:

[0015] A1, adding 0.5 parts of initiator, 1 part of accelerator, 1-2 parts of composite emulsifier, 0.5-1 parts of polymerization catalyst and 100 parts of solvent into a polymerization reactor, replacing the air so that the reactor is placed under a nitrogen atmosphere; then adding vinyl acetate tetrafluoroethylene and styrene into the reactor to obtain a reaction system;

[0016] A2, setting the temperature of the polymerization reactor to 25-30°C and the pressure to 0-2MPa, adding 8-10 parts of a reducing agent to the polymerization reactor, reacting for 1 hour, then adding 10-20 parts of tetrafluoroethylene, maintaining the temperature and pressure of the polymerization reactor unchanged, and continuing the reaction; when the conversion rate of the above polymerization reaction reaches more than 80%, continue stirring for 1 hour, then stop the reaction, discharge the material, and obtain a copolymer emulsion;

[0017] A3. The copolymer emulsion is diluted with water to 1.5 times of the original volume, and then 0.1 mol / L hydrochloric acid is added dropwise to adjust the pH value to 3-4, and 0.1 parts of CaCl2 solution is added dropwise to break the emulsion to obtain a polymer; the polymer is washed with deionized water until the conductivity of the washing liquid is <10 μs / cm to obtain a raw rubber; the raw rubber is vacuum dried at 100°C to a constant weight to obtain a copolymer rubber.

[0018] The invention adopts a multi-step feeding method to prepare copolymer rubber, vinyl acetate is used as a soft segment chain, styrene is used as a hard segment chain to form a block copolymer, and a certain amount of tetrafluoroethylene is introduced into the block copolymer to prepare the copolymer rubber.

[0019] The reaction principle of the addition polymerization of vinyl acetate, styrene and tetrafluoroethylene is as follows:

[0020]

[0021] Furthermore, in step A1, the initiator is ammonium persulfate, the accelerator is accelerator CZ, the composite emulsifier is a mixture of sodium dodecylbenzene sulfonate and potassium oleate in a mass ratio of 1:1, and the polymerization catalyst is triisobutylaluminum; in step A2, the reducing agent is sodium pyrophosphate.

[0022] Furthermore, in step S2, the method for preparing the supramolecular material comprises the following steps:

[0023] B1, lignin and acetone are mixed evenly to obtain a mixed solid-liquid; methacrylic acid is added to the mixed solid-liquid, condensed and refluxed at 60-70° C., and reacted for 2-3 hours to obtain a product; the product is filtered, and the solid is collected, and the solid is washed with deionized water and vacuum dried to constant weight to obtain modified lignin;

[0024] Acetone is used as solvent, and the reaction equation of lignin and methacrylic acid is as follows:

[0025]

[0026] B2. The chain transfer agent is dissolved in deionized water to obtain a chain transfer agent solution; acrylamide, modified lignin and deionized water are heated and stirred until the acrylamide is completely dissolved to obtain a mixture; sodium methyl methacrylate sulfonate and an initiator are added to the mixture, mixed and stirred, and then the temperature is raised to 60° C. and the temperature is kept for reaction for 2-3 hours to obtain a product; the product is cooled to room temperature, and then a NaOH solution is added dropwise to adjust the pH value to 6-8 to obtain a copolymer; the copolymer is dried at 50-60° C. to constant weight to obtain a solid supramolecular material.

[0027] Under the action of an initiator and the regulation of a chain transfer agent, acrylamide and modified lignin undergo addition polymerization to prepare a solid supramolecular material.

[0028] The reaction equation for the addition polymerization of modified lignin and acrylamide is as follows:

[0029]

[0030] Furthermore, in step B1, the usage ratio of lignin, acetone and methacrylic acid is 50-60g:200g:15-20g, and the vacuum drying temperature is 70-80°C.

[0031] Furthermore, in step B2, the chain transfer agent is thioglycolic acid, and the ratio of the chain transfer agent to deionized water is 0.2-0.3 g:50 mL; the ratio of acrylamide, modified lignin and deionized water is 10-20 g:40-50 g:100 mL; the initiator is a mixture of sodium sulfate and potassium persulfate in a mass ratio of 1:1, and the ratio of sodium methyl methacrylate sulfonate to the initiator is 10-20 g:1-3 g.

[0032] Furthermore, in step S2, the amount ratio of copolymer rubber, supramolecular material, inorganic powder material, epoxy resin, sulfur, ZnO, stearic acid and accelerator NS is 100g:10-20g:10-20g:5-10g:1.5-2g:4-5g:1-2g:0.6-1g; the mixing temperature is 160-170°C and the mixing time is 20-30min.

[0033] The present invention has the following beneficial effects:

[0034] 1. The present invention uses copolymer rubber as the base material for the high-strength damping sound insulation material, and the copolymer rubber uses vinyl acetate, styrene and tetrafluoroethylene monomers as polymerization monomers; vinyl acetate is used as a high damping material, and its glass transition temperature is about 30°C, and the maximum loss factor can be 2.6; however, the water resistance of vinyl acetate is poor, which limits the application scope of the prepared damping sound insulation material. In the copolymer rubber, the grafted tetrafluoroethylene monomer contains fluorine atoms on its molecular side chain, which can improve its own waterproof performance; however, if the copolymer rubber contains excessive fluorine elements, it will lead to greater polarity and prone to surface cracking under alkaline conditions. The present invention adopts a multi-step feeding method to prepare the copolymer rubber, using vinyl acetate as the soft segment chain and styrene as the hard segment chain to form a block copolymer; the addition of styrene introduces a benzene ring with steric hindrance on the side group of the prepared damping sound insulation material, so the hysteresis loss is large, thereby improving its own damping performance. A certain amount of tetrafluoroethylene is introduced into the above block copolymer to improve its waterproof performance and prepare a copolymer rubber with excellent mechanical properties and damping properties.

[0035] 2. The present invention designs supramolecular materials with high damping and sound insulation properties. After lignin and rubber base materials are mixed, a large number of hydrogen bonds can be formed; when many hydrogen bonds are formed in the polymer molecular chain, the opening and closing of the hydrogen bonds will consume a large part of the energy, which can enhance the damping performance of the copolymer rubber. Lignin and methacrylic acid react to obtain modified lignin; acrylamide and modified lignin undergo addition polymerization, which can increase the chain length of lignin, increase the number of side chains, further enhance the polarity of the side chains, and the entanglement between chain segments tends to intensify, thereby showing a higher damping value; in addition, the polar functional groups of supramolecular materials strengthen the affinity between rubber and glass fibers in waste fan blades, reduce the self-aggregation effect of glass fibers in rubber base materials, and improve the hysteresis loss of rubber. The amino groups in the supramolecular materials can react with epoxy resins, thereby improving the compatibility of supramolecular materials with other organic components.

[0036] 3. The present invention recycles waste fan blades, pyrolyzes the skin of the waste fan blades, removes the polyester coating and resin components, and thus recovers the glass fiber. After grinding and screening the glass fiber, the inorganic powder material obtained can be used as a reinforcing material for damping and sound insulation materials, and is used to improve its own mechanical properties and realize the recycling of waste resources. The base copolymer rubber and epoxy resin are removed, and the inorganic powder material of the reinforcing material is added. The additives also include vulcanizing agent sulfur, vulcanization activator zinc oxide, and plasticizer stearic acid. The appropriate vulcanization system can give the mixed rubber stable, good physical and mechanical properties and process performance. The high-strength damping and sound insulation material prepared by the present invention is the same as the production method of general rubber products, and needs to go through processes such as mixing and vulcanization. The finished product has the advantages of high strength, excellent mechanical properties, and good damping and sound insulation effects. DETAILED DESCRIPTION

[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] This embodiment provides a method for preparing a copolymer rubber for a high-strength damping sound insulation material, comprising the following steps:

[0040] A1, sodium dodecylbenzene sulfonate and potassium oleate are mixed in a mass ratio of 1:1 to obtain a composite emulsifier; 0.5 parts of initiator ammonium persulfate, 1 part of accelerator CZ, 1 part of composite emulsifier, 0.5 parts of polymerization catalyst triisobutylaluminum and 100 parts of solvent ethanol are added to a polymerization reactor in sequence according to weight parts, the polymerization reactor is closed, and the air in the polymerization reactor is replaced with nitrogen so that the reactor is in a nitrogen atmosphere; and 50 parts of vinyl acetate and 20 parts of styrene are added to the polymerization reactor through a rear buffer tank to obtain a reaction system.

[0041] A2. Set the temperature of the polymerization reactor to 25°C and the pressure of the polymerization reactor to 0MPa; then add 8 parts of reducing agent sodium pyrophosphate to the reaction system through a metering pump, react for 1 hour, then add 10 parts of tetrafluoroethylene, and continue to react in the polymerization reactor at this temperature and pressure, take samples every 30 minutes, and measure the conversion rate until the conversion rate of the above polymerization reaction reaches more than 80%, continue stirring for 1 hour, then stop the reaction, discharge the material, and obtain a copolymer emulsion. The water vapor generated during the above polymerization reaction is removed by vacuuming.

[0042] A3. The copolymer emulsion is diluted with water to 1.5 times of the original volume, and then 0.1 mol / L hydrochloric acid is added dropwise to adjust the pH value to 3, and then a CaCl2 solution is added to break the emulsion to obtain a polymer; the polymer is washed with deionized water until the conductivity of the washing liquid is <10 μs / cm to obtain a raw rubber; the raw rubber is vacuum dried at 100° C. to a constant weight to obtain a copolymer rubber.

[0043] Example 2

[0044] This embodiment provides a method for preparing a copolymer rubber for a high-strength damping sound insulation material, comprising the following steps:

[0045] A1, sodium dodecylbenzene sulfonate and potassium oleate are mixed in a mass ratio of 1:1 to obtain a composite emulsifier; 0.5 parts of initiator ammonium persulfate, 1 part of accelerator CZ, 2 parts of composite emulsifier, 0.8 parts of polymerization catalyst triisobutylaluminum and 100 parts of solvent ethanol are added to a polymerization reactor in sequence according to weight parts, the polymerization reactor is closed, and the air in the polymerization reactor is replaced with nitrogen so that the reactor is under a nitrogen atmosphere; and 50 parts of vinyl acetate and 25 parts of styrene are added to the polymerization reactor through a rear buffer tank to obtain a reaction system.

[0046] A2. Set the temperature of the polymerization reactor to 26°C and the pressure of the polymerization reactor to 1MPa; then add 9 parts of reducing agent sodium pyrophosphate to the reaction system through a metering pump, react for 1.3 hours, then add 15 parts of tetrafluoroethylene, and continue to react in the polymerization reactor at this temperature and pressure, sample every 30 minutes, and measure the conversion rate until the conversion rate of the above polymerization reaction reaches more than 80%, continue stirring for 1 hour, then stop the reaction, discharge the material, and obtain a copolymer emulsion. The water vapor generated during the above polymerization reaction is removed by vacuuming.

[0047] A3. The copolymer emulsion is diluted with water to 1.5 times of the original volume, and then 0.1 mol / L hydrochloric acid is added dropwise to adjust the pH value to 3.5, and then a CaCl2 solution is added to break the emulsion to obtain a polymer; the polymer is washed with deionized water until the conductivity of the washing liquid is <10 μs / cm to obtain a raw rubber; the raw rubber is vacuum dried at 100° C. to a constant weight to obtain a copolymer rubber.

[0048] Example 3

[0049] This embodiment provides a method for preparing a copolymer rubber for a high-strength damping sound insulation material, comprising the following steps:

[0050] A1, sodium dodecylbenzene sulfonate and potassium oleate are mixed in a mass ratio of 1:1 to obtain a composite emulsifier; 0.5 parts of initiator ammonium persulfate, 1 part of accelerator CZ, 2 parts of composite emulsifier, 1 part of polymerization catalyst triisobutylaluminum and 100 parts of solvent ethanol are added to a polymerization reactor in sequence according to weight parts, the polymerization reactor is closed, and the air in the polymerization reactor is replaced with nitrogen so that the reactor is under a nitrogen atmosphere; and 50 parts of vinyl acetate and 30 parts of styrene are added to the polymerization reactor through a rear buffer tank to obtain a reaction system.

[0051] A2. Control the temperature of the polymerization reactor to 30°C and the pressure of the polymerization reactor to 2MPa; then add 10 parts of reducing agent sodium pyrophosphate to the reaction system through a metering pump, react for 2 hours, then add 20 parts of tetrafluoroethylene, and continue to react in the polymerization reactor at this temperature and pressure, sample every 30 minutes, and measure the conversion rate until the conversion rate of the above polymerization reaction reaches more than 80%, continue stirring for 1 hour, then stop the reaction, discharge the material, and obtain a copolymer emulsion. The water vapor generated during the above polymerization reaction is removed by vacuuming.

[0052] A3. The copolymer emulsion is diluted with water to 1.5 times of the original volume, and then 0.1 mol / L hydrochloric acid is added dropwise to adjust the pH value to 4, and then a CaCl2 solution is added to break the emulsion to obtain a polymer; the polymer is washed with deionized water until the conductivity of the washing liquid is <10 μs / cm to obtain a raw rubber; the raw rubber is vacuum dried at 100°C to a constant weight to obtain a copolymer rubber.

[0053] Example 4

[0054] This embodiment provides a method for preparing a supramolecular material for a high-strength damping sound insulation material, comprising the following steps:

[0055] B1, 50g of lignin and 200g of acetone are added to a 500mL three-necked flask, and the mixture is stirred at 100r / min for 30min to obtain a mixed solid-liquid mixture; then 15g of methacrylic acid is added to the three-necked flask, the three-necked flask is connected to a reflux tube, a stirring device, and an electric heating jacket is arranged on the outside, and the other port is capped, and then the temperature of the electric heating jacket is adjusted to 60°C, and the reaction is carried out for 2h to obtain a product; the product is filtered and the solid is collected; the solid is washed with deionized water, and then the solid is placed in a vacuum oven at 50°C and dried to constant weight to obtain modified lignin.

[0056] B2, sodium sulfate and potassium persulfate are mixed in a mass ratio of 1:1 to obtain an initiator; 0.2g of chain transfer agent thioglycolic acid is dissolved in 50mL of deionized water and stirred evenly to prepare a chain transfer agent solution. 10g of acrylamide, 40g of modified lignin and 100mL of deionized water are put into a 500mL reactor, heated to 30°C, and stirred until the acrylamide is completely dissolved to obtain a mixture. Then 10g of sodium methyl propylene sulfonate and 1g of initiator are added to the reactor, mixed and stirred at 100r / min for 30min, and then the reactor is heated to 60°C, and then all the chain transfer agent solution is added dropwise at a uniform rate. After the addition is completed, the reaction is continued at 60°C for 2h to obtain a product. After the reaction is completed, the reactor is cooled to room temperature, and then 0.1mol / L NaOH solution is added dropwise to adjust the pH value of the product to 6 to obtain a copolymer; the copolymer is dried at 50°C to constant weight to obtain a solid supramolecular material.

[0057] Example 5

[0058] This embodiment provides a method for preparing a supramolecular material for a high-strength damping sound insulation material, comprising the following steps:

[0059] B1, 55g of lignin and 200g of acetone were added to a 500mL three-necked flask, and the mixture was stirred at 160r / min for 50min to obtain a mixed solid-liquid mixture; then 18g of methacrylic acid was added to the three-necked flask, and the three-necked flask was connected to a reflux tube, a stirring device, and an electric heating jacket was set on the outside, and the other port was capped, and then the temperature of the electric heating jacket was adjusted to 65°C, and the reaction was carried out for 2.3h to obtain a product; the product was filtered and the solid was collected; the solid was washed with deionized water, and then the solid was placed in a vacuum oven at 55°C and dried to constant weight to obtain modified lignin.

[0060] B2, sodium sulfate and potassium persulfate are mixed in a mass ratio of 1:1 to obtain an initiator; 0.25g of chain transfer agent thioglycolic acid is dissolved in 50mL of deionized water and stirred evenly to prepare a chain transfer agent solution. 15g of acrylamide, 45g of modified lignin and 100mL of deionized water are put into a 500mL reactor, heated to 33°C, and stirred until the acrylamide is completely dissolved to obtain a mixture. Then 15g of sodium methyl propylene sulfonate and 2g of initiator are added to the reactor, mixed and stirred at 150r / min for 50min, and then the reactor is heated to 60°C, and then all the chain transfer agent solution is added dropwise at a uniform rate. After the addition is completed, the reaction is continued at 60°C for 2.6h to obtain a product. After the reaction is completed, the reactor is cooled to room temperature, and then 0.1mol / L NaOH solution is added dropwise to adjust the pH value of the product to 7 to obtain a copolymer; the copolymer is dried at 55°C to constant weight to obtain a solid supramolecular material.

[0061] Example 6

[0062] This embodiment provides a method for preparing a supramolecular material for a high-strength damping sound insulation material, comprising the following steps:

[0063] B1, 60g of lignin and 200g of acetone are added to a 500mL three-necked flask, and the mixture is stirred at 200r / min for 60min to obtain a mixed solid-liquid mixture; then 20g of methacrylic acid is added to the three-necked flask, the three-necked flask is connected to a reflux tube, a stirring device, and an electric heating jacket is arranged on the outside, and the other port is capped, and then the temperature of the electric heating jacket is adjusted to 70°C, and the reaction is carried out for 3h to obtain a product; the product is filtered and the solid is collected; the solid is washed with deionized water, and then the solid is placed in a vacuum oven at 60°C and dried to constant weight to obtain modified lignin.

[0064] B2, sodium sulfate and potassium persulfate are mixed in a mass ratio of 1:1 to obtain an initiator; 0.3g of chain transfer agent thioglycolic acid is dissolved in 50mL of deionized water and stirred evenly to prepare a chain transfer agent solution. 20g of acrylamide, 50g of modified lignin and 100mL of deionized water are put into a 500mL reactor, heated to 40°C, and stirred until the acrylamide is completely dissolved to obtain a mixture. Then 20g of sodium methyl propylene sulfonate and 3g of initiator are added to the reactor, mixed and stirred at 200r / min for 60min, and then the reactor is heated to 60°C, and then all the chain transfer agent solution is added dropwise at a uniform rate. After the addition is completed, the reaction is continued at 60°C for 3h to obtain a product. After the reaction is completed, the reactor is cooled to room temperature, and then 0.1mol / L NaOH solution is added dropwise to adjust the pH value of the product to 8 to obtain a copolymer; the copolymer is dried at 60°C to constant weight to obtain a solid supramolecular material.

[0065] Example 7

[0066] This embodiment provides a method for recycling waste fan blades to prepare high-strength damping sound insulation materials, comprising the following steps:

[0067] S1. Dismantle and cut the waste fan blades, and collect the skin, interlayer and blade root respectively; feed the skin into the pyrolysis reactor, and the pyrolysis reactor adopts micro-negative pressure pyrolysis technology to collect pyrolysis gas, fuel oil and solid products in turn; sieve the solid product using a top-impact standard vibrating screen machine, and the particle size range of the standard screen is 0.3-2.36mm. The weight of the crushed waste fan blade material weighed each time is 500g, and the vibrating screen time is 10-20min, so as to obtain the recycled inorganic powder material.

[0068] S2. According to parts by weight, 100 g of the copolymer rubber prepared in Example 1, 10 g of the supramolecular material prepared in Example 4, 10 g of the inorganic powder material, 5 g of epoxy resin, 1.5 g of sulfur, 4 g of ZnO, 1 g of stearic acid and 0.6 g of accelerator NS were mixed and added to a rubber mixer for mixing to obtain a rubber compound. The roller spacing was 4 mm, the front roller temperature was 45 ° C, the rear roller temperature was 55 ° C, and the roller speed was 16 r / min. The mixing temperature of the rubber mixer was 160 ° C and the mixing time was 20 min.

[0069] S3. Add the rubber material into a flat vulcanizer for vulcanization at a vulcanization temperature of 170°C, a vulcanization pressure of 4MPa, and a vulcanization time of 10min to obtain a high-strength damping sound insulation material.

[0070] Example 8

[0071] This embodiment provides a method for recycling waste fan blades to prepare high-strength damping sound insulation materials, comprising the following steps:

[0072] S1. Dismantle and cut the waste fan blades, and collect the skin, interlayer and blade root respectively; feed the skin into the pyrolysis reactor, and the pyrolysis reactor adopts micro-negative pressure pyrolysis technology to collect pyrolysis gas, fuel oil and solid products in turn; sieve the solid product using a top-impact standard vibrating screen machine, and the particle size range of the standard screen is 0.3-2.36mm. The weight of the crushed waste fan blade material weighed each time is 500g, and the vibrating screen time is 15min, so as to obtain the recycled inorganic powder material.

[0073] S2. According to parts by weight, 100 g of the copolymer rubber prepared in Example 2, 15 g of the supramolecular material prepared in Example 5, 15 g of the inorganic powder material, 8 g of epoxy resin, 1.8 g of sulfur, 4.5 g of ZnO, 1.5 g of stearic acid and 0.8 g of accelerator NS were mixed and added to a rubber mixer for mixing to obtain a rubber compound. The roller spacing was 6 mm, the front roller temperature was 46 ° C, the rear roller temperature was 58 ° C, and the roller speed was 17 r / min. The mixing temperature of the rubber mixer was 165 ° C and the mixing time was 25 min.

[0074] S3. Add the rubber material into a flat vulcanizer for vulcanization at a vulcanization temperature of 172°C, a vulcanization pressure of 4.5MPa, and a vulcanization time of 15min to obtain a high-strength damping sound insulation material.

[0075] Example 9

[0076] This embodiment provides a method for recycling waste fan blades to prepare high-strength damping sound insulation materials, comprising the following steps:

[0077] S1. Dismantle and cut the waste fan blades, and collect the skin, interlayer and blade root respectively; feed the skin into the pyrolysis reactor, and the pyrolysis reactor adopts micro-negative pressure pyrolysis technology to collect pyrolysis gas, fuel oil and solid products in turn; sieve the solid product using a top-impact standard vibrating screen machine, and the particle size range of the standard screen is 0.3-2.36mm. The weight of the crushed waste fan blade material weighed each time is 500g, and the vibrating screen time is 20min, so as to obtain the recycled inorganic powder material.

[0078] S2. According to parts by weight, 100 g of the copolymer rubber prepared in Example 3, 20 g of the supramolecular material prepared in Example 6, 20 g of the inorganic powder material, 10 g of epoxy resin, 2 g of sulfur, 5 g of ZnO, 2 g of stearic acid and 1 g of accelerator NS were mixed and added to a rubber mixer for mixing to obtain a rubber compound. The roller spacing was 8 mm, the front roller temperature was 50 ° C, the rear roller temperature was 60 ° C, and the roller speed was 18 r / min. The mixing temperature of the rubber mixer was 170 ° C and the mixing time was 30 min.

[0079] S3. Add the rubber material into a flat vulcanizer for vulcanization at a vulcanization temperature of 180°C, a vulcanization pressure of 5MPa, and a vulcanization time of 20min to obtain a high-strength damping sound insulation material.

[0080] Comparative Example 1

[0081] The difference between this comparative example and Example 9 is that in step 2, when preparing the copolymer rubber, no styrene is added, and the copolymer rubber is prepared by copolymerization of vinyl acetate and tetrafluoroethylene.

[0082] Comparative Example 2

[0083] The difference between this comparative example and Example 9 is that in step 2, the modified lignin does not react with acrylamide, and the modified lignin is used instead of the supramolecular material.

[0084] Comparative Example 3

[0085] The difference between this comparative example and Example 9 is that no inorganic powder material is added when preparing the rubber material in step 2.

[0086] Performance Testing:

[0087] 1. According to GB / T531.1-2008 "Test method for indentation hardness of vulcanized rubber or thermoplastic rubber Part 1: Shore durometer method", the high-strength damping sound insulation materials prepared in Examples 7-9 and Comparative Examples 1-3 were tested for hardness using a Shore A durometer.

[0088] 2. According to GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", the high-strength damping sound insulation materials prepared in Examples 7-9 and Comparative Examples 1-3 were tested for tensile strength and elongation at break at room temperature using a WDL-10 microcomputer-controlled electronic universal testing machine, and the tensile rate was maintained at 500 mm / min.

[0089] 3. The damping temperature range of the high-strength damping sound insulation materials prepared in Examples 7-9 and Comparative Examples 1-3 was tested.

[0090] 4. According to GB / T18696.2-2002 "Determination of sound absorption coefficient and acoustic impedance in acoustic impedance tubes Part 2: Transfer function method", the sound insulation value within the frequency range of 1000Hz and 2000Hz is collected. The specific test results are shown in Table 1.

[0091] Table 1-Performance test data of the sample

[0092]

[0093]

[0094] Data Analysis:

[0095] A comparative analysis of the data in Table 1 above shows that the high-strength damping sound insulation materials prepared in Examples 7-9 of the present invention have excellent mechanical properties, as shown by relatively high Shore hardness values, tensile strength values, and elongation at break values; however, in Comparative Example 1, when preparing the copolymer rubber, the rigid segment monomer styrene was not added, which reduced the mechanical properties of the prepared material. In Comparative Example 3, when preparing the copolymer rubber, the inorganic powder material was not added, which significantly reduced the mechanical properties of the prepared material, as shown by significantly reduced Shore hardness values, tensile strength values, and elongation at break values.

[0096] The high-strength damping sound insulation materials prepared in Examples 7-9 of the present invention have excellent sound insulation effects, which are manifested in a wide damping temperature range and high sound insulation at 1000 Hz and 2000 Hz; however, in Comparative Example 2, the modified lignin did not react with acrylamide, and the modified lignin was used to replace the supramolecular material, which reduced the number of its own side chains and hydrogen bonds, thereby reducing the damping and sound insulation properties of the supramolecular material.

[0097] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0098] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0099] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for recycling waste fan blades to prepare high-strength damping sound insulation materials, characterized in that: The following steps are involved: S1. Dismantle and cut the waste fan blades, collect the skin, interlayer and blade root respectively; feed the skin into a pyrolysis reactor, perform micro-negative pressure pyrolysis, and collect the solid product; grind the solid product and sieve it with a vibrating screen, and the particle size range of the standard sieve is 0.3-2.36mm to obtain an inorganic powder material; S2, according to parts by weight, the copolymer rubber, supramolecular material, inorganic powder material, epoxy resin, sulfur, ZnO, stearic acid and accelerator NS are mixed, and added into a rubber mixer for mixing to obtain a rubber material; S3. The rubber material is added into a flat vulcanizer for vulcanization at a vulcanization temperature of 170-180° C., a vulcanization pressure of 4-5 MPa, and a vulcanization time of 10-20 min to obtain a high-strength damping sound insulation material.

2. The method for recycling waste fan blades to prepare high-strength damping sound insulation materials according to claim 1 is characterized in that: In step S2, the method for preparing the copolymer rubber comprises the following steps: A1. According to parts by weight, 0.5 parts of initiator, 1 part of promoter, 1-2 parts of composite emulsifier, 0.5-1 parts of polymerization catalyst and 100 parts of solvent are added to a polymerization reactor, and the air is replaced so that the reactor is placed under a nitrogen atmosphere; vinyl acetate tetrafluoroethylene and styrene are then added to the reactor to obtain a reaction system; A2, setting the temperature of the polymerization reactor to 25-30°C and the pressure to 0-2MPa, adding 8-10 parts of a reducing agent to the polymerization reactor, reacting for 1 hour, then adding 10-20 parts of tetrafluoroethylene, maintaining the temperature and pressure of the polymerization reactor unchanged, and continuing the reaction; when the conversion rate of the above polymerization reaction reaches more than 80%, continue stirring for 1 hour, then stop the reaction, discharge the material, and obtain a copolymer emulsion; A3. The copolymer emulsion is diluted with water to 1.5 times of the original volume, and then 0.1 mol / L hydrochloric acid is added dropwise to adjust the pH value to 3-4, and 0.1 parts of CaCl2 solution is added dropwise to break the emulsion to obtain a polymer; the polymer is washed with deionized water until the conductivity of the washing liquid is <10 μs / cm to obtain a raw rubber; the raw rubber is vacuum dried at 100°C to a constant weight to obtain a copolymer rubber.

3. The method for recycling waste fan blades to prepare high-strength damping sound insulation materials according to claim 2 is characterized in that: In step A1, the initiator is ammonium persulfate, the accelerator is accelerator CZ, the composite emulsifier is a mixture of sodium dodecylbenzene sulfonate and potassium oleate in a mass ratio of 1:1, and the polymerization catalyst is triisobutylaluminum; in step A2, the reducing agent is sodium pyrophosphate.

4. The method for recycling waste fan blades to prepare high-strength damping sound insulation materials according to claim 1 is characterized in that: In step S2, the method for preparing the supramolecular material comprises the following steps: B1, lignin and acetone are mixed evenly to obtain a mixed solid-liquid; methacrylic acid is added to the mixed solid-liquid, condensed and refluxed at 60-70° C., and reacted for 2-3 hours to obtain a product; the product is filtered, and the solid is collected, and the solid is washed with deionized water and vacuum dried to constant weight to obtain modified lignin; B2. The chain transfer agent is dissolved in deionized water to obtain a chain transfer agent solution; acrylamide, modified lignin and deionized water are heated and stirred until the acrylamide is completely dissolved to obtain a mixture; sodium methyl methacrylate sulfonate and an initiator are added to the mixture, mixed and stirred, and then the temperature is raised to 60° C. and the temperature is kept for reaction for 2-3 hours to obtain a product; the product is cooled to room temperature, and then a NaOH solution is added dropwise to adjust the pH value to 6-8 to obtain a copolymer; the copolymer is dried at 50-60° C. to constant weight to obtain a solid supramolecular material.

5. The method for recycling waste fan blades to prepare high-strength damping sound insulation materials according to claim 4 is characterized in that: In step B1, the usage ratio of lignin, acetone and methacrylic acid is 50-60g:200g:15-20g, and the vacuum drying temperature is 70-80°C.

6. The method for recycling waste fan blades to prepare high-strength damping sound insulation materials according to claim 5 is characterized in that: In step B2, the chain transfer agent is thioglycolic acid, and the ratio of the chain transfer agent to deionized water is 0.2-0.3 g:50 mL; the ratio of acrylamide, modified lignin and deionized water is 10-20 g:40-50 g:100 mL; the initiator is a mixture of sodium sulfate and potassium persulfate in a mass ratio of 1:1, and the ratio of sodium methyl methacrylate sulfonate to the initiator is 10-20 g:1-3 g.

7. The method for recycling waste fan blades to prepare high-strength damping sound insulation materials according to claim 1, characterized in that: In step S2, the amount ratio of copolymer rubber, supramolecular material, inorganic powder material, epoxy resin, sulfur, ZnO, stearic acid and accelerator NS is 100g:10-20g:10-20g:5-10g:1.5-2g:4-5g:1-2g:0.6-1g; the mixing temperature is 160-170°C and the mixing time is 20-30min.

Citation Information

Cited By

  • EPDM (Ethylene-Propylene-Diene Monomer) regenerated rubber containing waste wind power blade cracking product and preparation method of EPDM regenerated rubber

    CN121736415A