Carbon fiber reinforced weather-resistant ASA composite material and preparation method thereof
By combining modified carbon fiber with ASA resin, the problem of insufficient mechanical performance in automotive accessories is solved, which significantly improves mechanical properties and toughness, and reduces smoke generation during combustion.
Patent Information
- Application Number
- CN202411233146.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
AI Technical Summary
ASA resin has insufficient mechanical properties in automotive accessories applications and needs to be improved by adding fillers to meet the needs of use.
Using modified carbon fibers through aqueous suspension and ultrasonic treatment, combined with end-group modified silane coupling agent and nanohydroxide, a multi-dimensional composite material with hyperbranched polysiloxane load is prepared for mechanical enhancement of ASA composite materials. Performance and carbon fiber reinforced ASA composite material is prepared through twin screw extrusion mechanism.
It significantly improves the mechanical properties and toughness of ASA composites, improves the interface performance between carbon fiber and ASA resin, and reduces cracking problems after molding and smoke generation during combustion.
Smart Images

Figure BDA0005026890310000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ASA composite material preparation, and specifically relates to a carbon fiber reinforced weather-resistant ASA composite material and a preparation method thereof. Background Art
[0002] ASA resin is a ternary graft copolymer composed of acrylonitrile (A), styrene (S) and acrylate (A). ASA resin is similar to ABS resin, and has good mechanical properties, processing properties, electrical insulation and chemical resistance. In addition, because the raw material of ASA resin replaces butadiene rubber with acrylate rubber, its weather resistance is stronger than that of ABS. Its excellent weather resistance makes it widely used in outdoor products and automotive fields. However, when ASA resin is directly used in automotive accessories, its mechanical properties are insufficient, and fillers need to be added to improve the mechanical properties of ASA composite materials to meet the use requirements of automotive accessories.
[0003] Based on this, the present invention provides a carbon fiber reinforced weather-resistant ASA composite material and a preparation method thereof. Summary of the invention
[0004] The object of the present invention is to provide a carbon fiber reinforced weather-resistant ASA composite material and a preparation method thereof, so as to improve the mechanical properties of the ASA composite material.
[0005] One object of the present invention can be achieved by the following technical solutions:
[0006] A carbon fiber reinforced weather-resistant ASA composite material comprises the following raw materials in parts by weight: 100 parts of ASA resin, 15-30 parts of modified carbon fiber, and 0.1-5 parts of auxiliary agent;
[0007] The modified carbon fiber is prepared by mixing and thermally reacting a water suspension of carbon fiber, ethanol containing a terminal-modified silane coupling agent, and a water suspension of nano hydroxide;
[0008] The terminal group-modified silane coupling agent is produced by a ring-opening reaction of a terminal hydroxyl acrylate derivative and an epoxy silane coupling agent;
[0009] The terminal hydroxyl acrylate derivatives are prepared by the addition reaction of diamine and acrylate.
[0010] Furthermore, the reaction for obtaining the modified carbon fiber includes:
[0011] Add ethanol containing terminal modified silane coupling agent to the water suspension of carbon fiber, then add the water suspension of nano hydroxide dropwise at pH 5-6, 50-60°C and stirring. After the addition is completed, continue stirring and reacting for 2-6 hours, stop the reaction, filter, wash and dry to obtain modified carbon fiber.
[0012] In the above reaction, the self-hyperbranching reaction of siloxane at the end of the terminal-modified silane coupling agent under acidic conditions is utilized, and a uniformly dispersed aqueous hydroxide suspension is added during the self-hyperbranching reaction of siloxane, so that the hydroxide is dispersed in the dispersion and captured by the cavity in the hyperbranched polysilane generated by the reaction. At the same time, the highly active silanol bonds under acidic conditions can be coupled with the hydroxyl groups on the surface of carbon fibers and / or hydroxides, so that the carbon fibers and nano-hydroxides are loaded by hyperbranched polysilane to obtain modified carbon fibers. It can be seen that the modified carbon fibers are multi-dimensional composite materials composed of rods and particles.
[0013] Furthermore, the carbon fiber water suspension is prepared by ultrasonicating the carbon fiber and water under 30-40 kHz ultrasound for 20-30 minutes.
[0014] Furthermore, the water suspension of the nano hydroxide is prepared by ultrasonicating the nano hydroxide and water under 30-40 kHz ultrasound for 20-30 minutes.
[0015] Furthermore, the mass ratio of the carbon fiber water suspension, the ethanol containing the terminal-modified silane coupling agent, and the nano hydroxide water suspension is 50:20-30:50.
[0016] Furthermore, the mass concentration of the carbon fiber water suspension is 10-20%.
[0017] Furthermore, the length of the carbon fiber is 5-10 microns.
[0018] Furthermore, the mass ratio of the terminal-modified silane coupling agent to the ethanol in the ethanol containing the terminal-modified silane coupling agent is 2-5:15-25.
[0019] Furthermore, the mass concentration of the nano hydroxide water suspension is 3-8%, the nano hydroxide is magnesium hydroxide and / or aluminum hydroxide, and the particle size of the nano hydroxide is 100-200 nm.
[0020] Furthermore, the terminal hydroxyl acrylate derivative and the epoxy silane coupling agent undergo a ring-opening reaction in the presence of a first organic solvent, and the ring-opening reaction conditions are: pH 9-10, reaction temperature 60-75° C., and reaction time 2-6 hours.
[0021] Furthermore, the molar ratio of the terminal hydroxyl acrylate derivative to the epoxy silane coupling agent is 1.1-1.3:1.
[0022] Furthermore, the first organic solvent is one of benzene, toluene, tetrahydrofuran, and N,N-dimethylformamide.
[0023] Preferably, the first organic solvent is tetrahydrofuran.
[0024] Preferably, the ring-opening reaction of the terminal hydroxyl acrylate derivative and the epoxy silane coupling agent comprises:
[0025] After the terminal hydroxyl acrylate derivative, epoxy silane coupling agent and the first organic solvent are mixed, the pH is adjusted to 9-10, and the mixture is heated to 60-75° C., and the reaction is continued with stirring for 2-6 hours. The reaction is stopped, rotary evaporated, washed and dried to obtain a terminal modified silane coupling agent.
[0026] Furthermore, the diamine and the acrylate undergo an addition reaction in the presence of a second organic solvent, and the addition reaction conditions are: pH 9-10, reaction temperature 20-90° C., and reaction time 2-4 hours.
[0027] Furthermore, the diamine is one of 1,4-butanediamine, 1,6-diaminohexane, and 2-methyl-1,5-pentanediamine.
[0028] Furthermore, the molar ratio of the diamine to the acrylate is 1:1.1-1.4.
[0029] Furthermore, the acrylic acid ester is one of methyl acrylate, methyl acrylate and butyl acrylate.
[0030] Furthermore, the second solvent is one of tetrahydrofuran and N,N-dimethylformamide.
[0031] Preferably, the addition reaction of the diamine and acrylate comprises:
[0032] After the diamine, acrylate and the second organic solvent are uniformly mixed, the pH is adjusted to 9-10, and the mixture is heated to 20-90°C. The mixture is stirred and reacted for 2-4 hours. The reaction is stopped, and the mixture is rotary evaporated, washed and dried to obtain a terminal hydroxy acrylate derivative.
[0033] Furthermore, the auxiliary agent is one or more of an antioxidant, a weathering agent, and a lubricant.
[0034] Another object of the present invention can be achieved by the following technical solutions:
[0035] A method for preparing a carbon fiber reinforced weather-resistant ASA composite material, comprising:
[0036] The ASA resin, modified carbon fiber and auxiliary agent are mixed, extruded and granulated through a twin-screw extruder to obtain an ASA composite material.
[0037] Beneficial effects of the present invention:
[0038] The invention discloses a carbon fiber reinforced weather-resistant ASA composite material and a preparation method thereof. The mechanical properties of the obtained ASA composite material are improved by introducing modified carbon fiber and utilizing the excellent mechanical reinforcement characteristics of the carbon fiber. Remarkably, the modified carbon fiber of the invention is a multi-dimensional composite material with a surface coated with hyperbranched polysiloxane and nano hydroxide, which not only improves the interface performance between the carbon fiber and the ASA resin, but also makes the carbon fiber uniformly dispersed in the ASA resin. In particular, the end group of the hyperbranched polysiloxane contains a long-chain acrylate chain, which gives the carbon fiber and the ASA resin molecular chain better blending and processing performance, improves the toughness of the obtained ASA composite material, and overcomes the disadvantage that the ASA resin is easy to crack after molding. Finally, the hydroxide loaded on the surface of the carbon fiber can greatly reduce the smoke generated when the ASA resin is burned. DETAILED DESCRIPTION
[0039] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] Terminal modified silane coupling agent:
[0042] Step 1: After 0.11 mol 1,6-diaminohexane, 0.1 mol methyl acrylate and 100 mL tetrahydrofuran are mixed evenly, the pH is adjusted to 9-10, heated to reflux under condensation conditions, and stirred for reaction for 2 hours, the reaction is stopped, rotary evaporated, washed, and dried to obtain a terminal hydroxy acrylate derivative;
[0043] The second step: after mixing 0.11 mol of terminal hydroxyl acrylate derivative (the amount of substance is based on the amount of added methyl acrylate), 0.1 mol of epoxy silane coupling agent (KH560) and 150 mL of tetrahydrofuran, adjust the pH to 9-10, and heat to 60°C, continue stirring the reaction for 6 hours, stop the reaction, rotary evaporate, wash, and dry to obtain a terminal modified silane coupling agent.
[0044] Example 2
[0045] Terminal modified silane coupling agent:
[0046] Step 1: After 0.14 mol 1,6-diaminohexane, 0.1 mol methyl acrylate and 100 mL tetrahydrofuran are mixed evenly, the pH is adjusted to 9-10, heated to reflux under condensation conditions, and stirred to react for 4 hours, the reaction is stopped, rotary evaporated, washed, and dried to obtain a terminal hydroxy acrylate derivative;
[0047] The second step: after mixing 0.13 mol of terminal hydroxyl acrylate derivative (the amount of substance is based on the amount of added methyl acrylate), 0.1 mol of epoxy silane coupling agent (KH560) and 150 mL of tetrahydrofuran, adjust the pH to 9-10, and heat to 65°C, continue stirring and reacting for 2 hours, stop the reaction, rotary evaporate, wash, and dry to obtain a terminal modified silane coupling agent.
[0048] Example 3
[0049] Modified carbon fiber:
[0050] Preparation of carbon fiber aqueous suspension: 10 g of carbon fiber with a length of 5-10 μm and 90 g of water were ultrasonicated at 30 kHz for 30 min.
[0051] Preparation of nano hydroxide aqueous suspension: 3 g of nano magnesium hydroxide with a particle size of 100-150 nm and 97 g of water were ultrasonicated at 30 kHz for 30 min.
[0052] Modification step: add 20g of ethanol containing the end-group modified silane coupling agent prepared in Example 1 to an aqueous suspension of 50g of carbon fiber, then add 50g of an aqueous suspension of nano hydroxide dropwise at pH 5-6, 50°C and stirring, after the addition is completed, continue stirring and reacting for 6h, ageing, separating and taking the precipitate, washing with water and immersing alternately, and finally drying to obtain modified carbon fiber, wherein the mass ratio of the end-group modified silane coupling agent to ethanol in the ethanol containing the end-group modified silane coupling agent is 2:18.
[0053] Example 4
[0054] Modified carbon fiber:
[0055] Preparation of carbon fiber aqueous suspension: 20 g of carbon fiber with a length of 5-10 μm and 80 g of water were ultrasonicated at 40 kHz for 20 min.
[0056] Preparation of nano hydroxide aqueous suspension: 8 g of nano magnesium hydroxide with a particle size of 150-200 nm and 92 g of water were ultrasonicated at 40 kHz for 20 min.
[0057] Modification step: add 30g of ethanol containing the end-group modified silane coupling agent prepared in Example 1 to an aqueous suspension of 50g of carbon fiber, then add 50g of an aqueous suspension of nano hydroxide dropwise at pH 5-6, 60°C and stirring, after the addition is completed, continue stirring and reacting for 2h, ageing, separating and taking the precipitate, washing with water and immersing alternately, and finally drying to obtain modified carbon fiber, wherein the mass ratio of the end-group modified silane coupling agent to the ethanol containing the end-group modified silane coupling agent is 5:25.
[0058] Example 5
[0059] Composite Materials:
[0060] The first step is to prepare the following raw materials in parts by weight: 100 parts of ASA resin, 15 parts of modified carbon fiber prepared in Example 3, and 0.1 parts of an auxiliary agent, wherein the auxiliary agent is a lubricant (zinc stearate);
[0061] In the second step, the ASA resin, modified carbon fiber and auxiliary agent are mixed, extruded and granulated by a twin-screw extruder to obtain an ASA composite material. The extrusion temperature is 200-250°C and the rotation speed is 200-500r / min.
[0062] Example 6
[0063] Composite Materials:
[0064] The first step is to prepare the following raw materials in parts by weight: 100 parts of ASA resin, 20 parts of modified carbon fiber prepared in Example 3, and 1 part of an auxiliary agent, wherein the auxiliary agent is a lubricant (zinc stearate);
[0065] In the second step, the ASA resin, modified carbon fiber and auxiliary agent are mixed, extruded and granulated by a twin-screw extruder to obtain an ASA composite material. The extrusion temperature is 200-250°C and the rotation speed is 200-500r / min.
[0066] Example 7
[0067] Composite Materials:
[0068] The first step is to prepare the following raw materials in parts by weight: 100 parts of ASA resin, 30 parts of modified carbon fiber prepared in Example 3, and 2 parts of auxiliary agent, wherein the auxiliary agent is a lubricant (zinc stearate);
[0069] In the second step, the ASA resin, modified carbon fiber and auxiliary agent are mixed, extruded and granulated by a twin-screw extruder to obtain an ASA composite material. The extrusion temperature is 200-250°C and the rotation speed is 200-500r / min.
[0070] Comparative Example 1
[0071] Composite material: Compared with Example 5, an equal amount of modified carbon fiber is replaced by carbon fiber, and the rest is the same.
[0072] Comparative Example 2
[0073] Composite material: Compared with Example 5, the modified carbon fiber is deleted, and the rest is the same.
[0074] Comparative Example 3
[0075] Composite material: Compared with Example 5, the modified carbon fiber is replaced with carbon fiber prepared by the following steps, and the rest is the same:
[0076] Preparation of carbon fiber aqueous suspension: 10 g of carbon fiber with a length of 5-10 μm and 90 g of water were ultrasonicated at 30 kHz for 30 min.
[0077] Modification step: add 20g of ethanol containing the end-group modified silane coupling agent prepared in Example 1 to an aqueous suspension of 50g of carbon fiber, then react at pH 5-6, 50°C, and stirring for 6h, age, separate and take the precipitate, rinse with water and soak alternately, and finally dry to obtain modified carbon fiber, wherein the mass ratio of the end-group modified silane coupling agent to ethanol in the ethanol containing the end-group modified silane coupling agent is 2:18.
[0078] Comparative Example 4
[0079] Composite material: Compared with Example 5, the modified carbon fiber is replaced with carbon fiber prepared by the following steps, and the rest is the same:
[0080] Preparation of carbon fiber aqueous suspension: 10 g of carbon fiber with a length of 5-10 μm and 90 g of water were ultrasonicated at 30 kHz for 30 min.
[0081] Preparation of nano hydroxide aqueous suspension: 3 g of nano magnesium hydroxide with a particle size of 100-150 nm and 97 g of water were ultrasonicated at 30 kHz for 30 min.
[0082] Modification steps: add 50g of nanohydroxide suspension to 50g of carbon fiber suspension under stirring at pH 5-6 and 50℃. After the addition is completed, continue to stir and react for 6h, age, separate and take the precipitate, rinse and soak alternately with water, and finally dry to obtain modified carbon fiber.
[0083] The composite materials obtained in Examples 5-7 and Comparative Examples 1-4 were tested for physical properties, and the test results are shown in Table 1. The tensile strength was tested according to GB / T 1040.2, the flexural strength was tested according to GB / T 9341, the notched impact strength was tested according to GB / T 1043.1, and the smoke density was tested according to GB / T8323.2, using a flameless combustion mode, a test radiation intensity of 25 kW / m, and a test time of 20 min;
[0084] Table 1
[0085]
[0086] It can be seen from the data in Table 1 that the composite materials obtained in Examples 5-7 have excellent mechanical strength and toughness.
[0087] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0088] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A carbon fiber reinforced weather-resistant ASA composite material, characterized in that: The method comprises the following raw materials in parts by weight: 100 parts of ASA resin, 15-30 parts of modified carbon fiber, and 0.1-5 parts of auxiliary agent; The modified carbon fiber is prepared by mixing and thermally reacting a water suspension of carbon fiber, ethanol containing a terminal-modified silane coupling agent, and a water suspension of nano hydroxide; The terminal group modified silane coupling agent is produced by a ring-opening reaction of a terminal hydroxyl acrylate derivative and an epoxy silane coupling agent; The terminal hydroxyl acrylate derivatives are prepared by the addition reaction of diamine and acrylate.
2. A carbon fiber reinforced weather-resistant ASA composite material according to claim 1, characterized in that: The reaction for obtaining the modified carbon fiber comprises: Add ethanol containing terminal modified silane coupling agent to the water suspension of carbon fiber, then add the water suspension of nano hydroxide dropwise at pH 5-6, 50-60°C and stirring. After the addition is completed, continue stirring and reacting for 2-6 hours, stop the reaction, filter, wash and dry to obtain modified carbon fiber.
3. A carbon fiber reinforced weather-resistant ASA composite material according to claim 2, characterized in that: The mass ratio of the carbon fiber water suspension, the ethanol containing the terminal-modified silane coupling agent, and the nano hydroxide water suspension is 50:20-30:
50.
4. The carbon fiber reinforced weather-resistant ASA composite material according to claim 1, characterized in that: The mass concentration of the carbon fiber water suspension is 10-20%.
5. The carbon fiber reinforced weather-resistant ASA composite material according to claim 1, characterized in that: The length of the carbon fiber is 5-10 microns.
6. The carbon fiber reinforced weather-resistant ASA composite material according to claim 1, characterized in that: The mass ratio of the terminal-modified silane coupling agent to the ethanol in the ethanol containing the terminal-modified silane coupling agent is 2-5:15-25.
7. The carbon fiber reinforced weather-resistant ASA composite material according to claim 1, characterized in that: The mass concentration of the nano hydroxide water suspension is 3-8%, the nano hydroxide is magnesium hydroxide and / or aluminum hydroxide, and the particle size of the nano hydroxide is 100-200 nm.
8. The carbon fiber reinforced weather-resistant ASA composite material according to claim 1, characterized in that: The terminal hydroxyl acrylate derivative and the epoxy silane coupling agent undergo a ring-opening reaction in the presence of a first organic solvent, and the ring-opening reaction conditions are: pH 9-10, reaction temperature 60-75° C., and reaction time 2-6 hours; the first organic solvent is one of benzene, toluene, tetrahydrofuran, and N,N-dimethylformamide; the molar ratio of the terminal hydroxyl acrylate derivative and the epoxy silane coupling agent is 1.1-1.3:
1.
9. The carbon fiber reinforced weather-resistant ASA composite material according to claim 1, characterized in that: The diamine and the acrylate undergo an addition reaction in the presence of a second organic solvent, and the addition reaction conditions are: pH 9-10, reaction temperature 20-90°C, and reaction time 2-4h; the diamine is one of 1,4-butanediamine, 1,6-diaminohexane, and 2-methyl-1,5-pentanediamine; the acrylate is one of methyl acrylate, methyl acrylate, and butyl acrylate; the second solvent is one of tetrahydrofuran and N,N-dimethylformamide; and the molar ratio of the diamine to the acrylate is 1:1.1-1.
4.
10. A method for preparing a carbon fiber reinforced weather-resistant ASA composite material according to any one of claims 1 to 9, characterized in that: include: The ASA resin, modified carbon fiber and auxiliary agent are mixed, extruded and granulated by a twin-screw extruder to obtain an ASA composite material.