Elastomer of light foaming wire rod and preparation method of elastomer
By using specific raw materials composition and preparation methods, the problem of low floating rate of cables in water is solved, the thermal stability and UV resistance are improved, and the use cycle is extended and the cost is reduced.
Patent Information
- Application Number
- CN202411054605.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing cable wires have low floating rate and are unstable in water environments, mainly due to the unstable foaming of the elastomer during the wire making process.
A lightweight consisting of homopolymer polypropylene, hydrogenated styrene butadiene styrene block copolymer, softening plasticizer, ethylene methyl acrylate copolymer, anti-copper resistant and polymer silicone masterbatch Magnetic foam wire elastomer is prepared by melt mixing, molding and cooling and solidification steps to ensure the purity and mixing uniformity of the raw materials.
It significantly improves the thermal stability, weather resistance and UV resistance of the finished product, enhances the floating rate and compressive resistance in water, reduces the cost of use and extends the service cycle.
Smart Images

Figure CN118931092A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of foaming materials, and in particular to an elastomer of a lightweight foaming wire material and a preparation method thereof. Background Art
[0002] Nowadays, cables are used more and more widely in underwater environments, but the existing materials have low floating rates and unstable floating rates when used in underwater environments. The reason for the unstable floating rate is that the elastomer raw materials have unstable foaming during the wire making process, which leads to instability in later use.
[0003] In order to solve the above problems, the present application proposes an elastomer of a lightweight foamed wire and a preparation method thereof. Summary of the invention
[0004] (I) Purpose of the invention
[0005] In order to solve the technical problems existing in the background technology, the present invention proposes an elastomer of a lightweight foam wire and a preparation method thereof. The present invention significantly improves the thermal stability, weather resistance and UV resistance of the finished product, effectively reduces the cost of use and increases the service life.
[0006] (II) Technical solution
[0007] In order to solve the above problems, the present invention provides a lightweight foamed wire elastic body, which is composed of the following raw materials in percentage by weight:
[0008]
[0009] Preferably, it is composed of the following raw materials in weight percentage:
[0010]
[0011] Preferably, it is composed of the following raw materials in weight percentage:
[0012]
[0013] A method for preparing an elastic body of a lightweight foamed wire material, the specific steps are as follows:
[0014] S1. Raw material preparation:
[0015] Prepare homopolymer polypropylene, hydrogenated styrene butadiene styrene block copolymer, softening plasticizer, ethylene methyl acrylate copolymer, copper resistance agent and high molecular silicone masterbatch according to the proportion;
[0016] S2. Melt mixing:
[0017] S3, mold or extrusion head settings:
[0018] Select the appropriate die or extrusion head according to the shape and size of the required product.
[0019] Adjust and install the die or extrusion head according to product requirements and ensure its proper position and temperature.
[0020] S4, molding process:
[0021] The mixed raw materials are injected into a mold or extruder.
[0022] Control the temperature, pressure and speed parameters of the injection molding machine or extruder to keep the raw materials in the required state.
[0023] S5. Cooling and solidification:
[0024] The formed product enters the cooling area and is cooled in the cooler to solidify the product quickly.
[0025] Control cooling rate and time to ensure good development and solidification of physical properties of the product.
[0026] If necessary, cooling water or other cooling media can be used to assist cooling.
[0027] Preferably, in S1, the purity and quality stability of the raw materials are ensured.
[0028] Preferably, in S2,
[0029] Place the prepared raw materials into the hopper of the injection molding machine or extruder;
[0030] Start the machine and allow it to reach melting temperature;
[0031] Set the melting temperature and mixing time to ensure that the raw materials are fully melted and mixed evenly;
[0032] Adjust the stirring device or screw speed in the machine to ensure uniform mixing of the raw materials.
[0033] Preferably, post-processing is also included:
[0034] The formed products undergo possible post-processing operations, such as removing burrs, trimming edges, and repairing surface defects.
[0035] Carry out necessary cleaning and inspection to ensure product quality meets requirements.
[0036] Preferably, inspection and quality control are also included:
[0037] Inspect the finished products in terms of appearance, size and mechanical properties.
[0038] Conduct random inspections or full inspections according to quality control standards, and record and analyze the results.
[0039] If necessary, functional tests and durability tests can be carried out on the product to ensure that the product performance meets the requirements.
[0040] The above technical solution of the present invention has the following beneficial technical effects:
[0041] The softness, compression resistance and wear resistance of the finished wire are greatly improved compared with before; the floating rate of the foamed wire used in water and underwater is greatly improved, and the problems of low floating rate, hardness and instability of the wire in water in the past are solved; the thermal stability, weather resistance and UV resistance of the finished product are significantly improved, which effectively reduces the cost of use and increases the service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 The present invention provides a flow chart of a method for preparing an elastic body of a lightweight foamed wire material. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0044] Example 1
[0045] A lightweight foamed wire elastomer is composed of the following raw materials in percentage by weight:
[0046]
[0047] A method for preparing an elastic body of a lightweight foamed wire material, the specific steps are as follows:
[0048] S1. Raw material preparation:
[0049] Prepare homopolymer polypropylene, hydrogenated styrene butadiene styrene block copolymer, softening plasticizer, ethylene methyl acrylate copolymer, copper resistance agent and high molecular silicone masterbatch according to the proportion;
[0050] S2. Melt mixing:
[0051] S3, mold or extrusion head settings:
[0052] Select the appropriate die or extrusion head according to the shape and size of the required product.
[0053] Adjust and install the die or extrusion head according to product requirements and ensure its proper position and temperature.
[0054] S4, molding process:
[0055] The mixed raw materials are injected into a mold or extruder.
[0056] Control the temperature, pressure and speed parameters of the injection molding machine or extruder to keep the raw materials in the required state.
[0057] S5. Cooling and solidification:
[0058] The formed product enters the cooling area and is cooled in the cooler to solidify the product quickly.
[0059] Control cooling rate and time to ensure good development and solidification of physical properties of the product.
[0060] If necessary, cooling water or other cooling media can be used to assist cooling.
[0061] Preferably, in S1, the purity and quality stability of the raw materials are ensured.
[0062] Place the prepared raw materials into the hopper of the injection molding machine or extruder;
[0063] Start the machine and allow it to reach melting temperature;
[0064] Set the melting temperature and mixing time to ensure that the raw materials are fully melted and mixed evenly;
[0065] Adjust the stirring device or screw speed in the machine to ensure uniform mixing of the raw materials.
[0066] Preferably, post-processing is also included:
[0067] The formed products undergo possible post-processing operations, such as removing burrs, trimming edges, and repairing surface defects.
[0068] Carry out necessary cleaning and inspection to ensure product quality meets requirements.
[0069] Also includes inspection and quality control:
[0070] Inspect the appearance, dimensions and mechanical properties of finished products;
[0071] Conduct random inspections or full inspections according to quality control standards, and record and analyze the results.
[0072] If necessary, functional tests and durability tests can be carried out on the product to ensure that the product performance meets the requirements.
[0073] Example 2
[0074] The difference from Example 1 is that:
[0075] Preferably, it is composed of the following raw materials in weight percentage:
[0076] Homopolymer polypropylene 16 parts;
[0077] 30 parts of hydrogenated styrene butadiene styrene block copolymer;
[0078] 20 parts of softening plasticizer;
[0079] 17.5 parts of ethylene methyl acrylate copolymer;
[0080] 2.5 parts of copper resistance agent;
[0081] 3.5 parts of polymer silicone masterbatch.
[0082] Example 3
[0083] The difference from Example 1 is that:
[0084]
[0085] experiment:
[0086] The products of Example 1, Example 2 and Example 3 were selected for testing and compared with the previous products, and the average value of the three was taken. The specific test results are shown in the following table:
[0087] Embodiments of the present invention Previous Products proportion 0.90g / cm3 0.95g / cm3 Tensile 12Mpa 8Mpa Elongation 700% 580% Floating rate 94% 75% Copper Oxygen Damage No yellowing, no greening Yellow, green
[0088] It can be seen from the above table that the floating rate, compression resistance and wear resistance of the finished product have been greatly improved compared with before.
[0089] The floating rate of plastic products used in water and underwater is greatly improved, solving the problem that the products in the past floated unstably in water and were prone to yellowing, greening and aging.
[0090] The thermal stability, weather resistance and UV resistance of the finished product are significantly improved. When used in swimming pools, the water quality will not cause the surface of the product to turn green or yellow. The aging resistance is also greatly improved, thereby effectively reducing the cost of use and increasing the service life.
[0091] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A lightweight foamed wire elastic body, characterized in that: It is composed of the following raw materials in percentage by weight:
2. The lightweight foamed wire elastic body according to claim 1, characterized in that: It is composed of the following raw materials in percentage by weight:
3. The lightweight foamed wire elastic body according to claim 1, characterized in that: It is composed of the following raw materials in percentage by weight:
4. A method for preparing an elastic body of a lightweight foamed wire, characterized in that: The specific steps are as follows: S1. Raw material preparation: Prepare homopolymer polypropylene, hydrogenated styrene butadiene styrene block copolymer, softening plasticizer, ethylene methyl acrylate copolymer, copper resistance agent and high molecular silicone masterbatch according to the proportion; S2, melt mixing; S3, mold or extrusion head settings: Choose the appropriate die or extrusion head according to the shape and size of the required product; Adjust and install the die or extrusion head according to product requirements and ensure its proper position and temperature; S4, molding process: Inject the mixed raw materials into a mold or extruder; Control the temperature, pressure and speed parameters of the injection molding machine or extruder to keep the raw materials in the required state; S5. Cooling and solidification: The formed product enters the cooling area and is cooled in the cooler to solidify the product quickly; Control cooling rate and time to ensure good development and solidification of physical properties of the product; If necessary, cooling water or other cooling media can be used to assist cooling.
5. The method for preparing an elastic body of a lightweight foamed wire material according to claim 4, characterized in that: In S1, the purity and quality of raw materials are ensured to be stable.
6. The method for preparing an elastic body of a lightweight foamed wire material according to claim 5, characterized in that: In S2, Place the prepared raw materials into the hopper of the injection molding machine or extruder; Start the machine and allow it to reach melting temperature; Set the melting temperature and mixing time to ensure that the raw materials are fully melted and mixed evenly; Adjust the stirring device or screw speed in the machine to ensure uniform mixing of the raw materials.
7. The method for preparing an elastic body of a lightweight foamed wire material according to claim 6, characterized in that: Post-processing is also included: The formed product undergoes possible post-processing operations, such as removing burrs, trimming edges, and repairing surface defects; Carry out necessary cleaning and inspection to ensure product quality meets requirements.
8. The method for preparing an elastic body of a lightweight foamed wire material according to claim 7, characterized in that: Also includes inspection and quality control: Inspect the appearance, dimensions and mechanical properties of finished products; Conduct random inspections or full inspections according to quality control standards, and record and analyze the results; If necessary, functional tests and durability tests can be carried out on the product to ensure that the product performance meets the requirements.
9. The method for preparing an elastic body of a lightweight foamed wire material according to claim 8, characterized in that: It is made by twin-screw extruder, and the specific setting parameters are as follows: Zone 1: 185℃~190; Zone 2: 190℃~195℃; Zone 3: 200℃~205℃; Zone 4: 205℃~210℃; Zone 5: 210℃~215℃; Zone 6: 210℃~215℃; Zone 7: 215℃~210℃; Zone 8: 210℃~205℃; Zone 9: 210℃~205℃; Zone 10: 205℃~200℃; Zone 11: 200℃; Zone 12: 200℃~205℃.