Weighted ABS (Acrylonitrile Butadiene Styrene) resin composition and preparation method and application thereof
By adding high-density inorganic fillers and reactive organic compounds to ABS resin and optimizing the ratio, the problems of density and mechanical properties of ABS resin materials are solved, and the balance of high density, fluidity and mechanical properties is achieved, and it is suitable for high-end products.
Patent Information
- Application Number
- CN202411057253.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
AI Technical Summary
Existing ABS resin materials cannot have both high filling and fluidity, as well as high rigidity and high toughness, and the density is not enough to meet the texture requirements of high-end cosmetics.
By adding a large amount of high-density inorganic fillers to the ABS resin and adding reactive organic substances such as epoxy resin to enhance interface binding and compatibility, combining elastomers and antioxidants, the ratio is optimized to achieve high density and fluidity and balance of mechanical properties.
The density of the ABS resin composition is achieved by greater than 2g/cm3, and has good fluidity and mechanical properties, such as melt index, tensile strength and bending modulus, and is suitable for high-end products such as cosmetic packaging containers.
Smart Images

Figure BDA0004976800250000041 
Figure BDA0004976800250000042 
Figure BDA0004976800250000051
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a weighted ABS resin composition and a preparation method and application thereof. Background Art
[0002] ABS resin (acrylonitrile-butadiene-styrene terpolymer) has the common properties of the three components. It is a material with easy-to-obtain raw materials, good comprehensive properties, low price, and wide applications. It has many advantages such as good impact resistance, processability, dimensional stability, wear resistance, and chemical corrosion resistance. Its operating temperature range can vary between -40 and 100°C. At present, ABS resin has been widely used in manufacturing industries such as machinery, electrical, textile, automobile, aircraft, and shipbuilding, as well as chemical industry.
[0003] Products made of ABS resin have low density and light weight. They feel light and plastic, and cannot meet the texture requirements of high-end cosmetics. At present, ABS resin is used as the base material, and high-density inorganic powder materials are added as fillers. Through different weight ratios and material combinations, ABS resin materials with high specific gravity, unique performance and applicability are obtained.
[0004] Patent application CN111040367A discloses a method for preparing a high-filling, low-density ABS masterbatch, wherein hollow spherical calcium carbonate particles and ABS resin are mixed, and under vacuum negative pressure conditions, the air contained in the hollow spherical calcium carbonate is exhausted during the vacuum process, and the ABS resin is then filled into the hollow spherical calcium carbonate. After the vacuum state of the sealed container ends, during the process of restoring normal pressure, the pressure generated by the entry of external air further makes the ABS resin in the inner cavity of the calcium carbonate and the inner wall of the hollow spherical calcium carbonate fit more tightly. However, the density of the ABS masterbatch obtained is not high, about 1.3-1.4 g / cm 3 .
[0005] Patent application CN113698726A discloses a highly filled, high-performance flame-retardant ABS material, which is composed of the following raw materials in parts by weight: 60-62 parts of ABS resin, 10-13.5 parts of bromine flame retardant, 2-5 parts of antimony trioxide, 20 parts of filler, 0.2-1 parts of lubricant, 0.1-1 parts of antioxidant and 5 parts of dendritic macromolecular fusion agent. The dendritic macromolecular fusion agent is added to the ABS resin to achieve uniform dispersion of the filler in the ABS resin. However, in order to ensure the fluidity of the obtained ABS material for subsequent processing, the amount of filler added in the system is limited (the amount of filler added is 20%), and the density of the obtained ABS material is not high. Summary of the invention
[0006] The object of the present invention is to provide a weighted ABS resin composition and a preparation method and application thereof, which solves the problem that the existing ABS resin material cannot have high filling and fluidity, high rigidity and high toughness at the same time.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The first aspect of the present invention provides a weighted ABS resin composition, which is composed of the following raw materials in parts by weight:
[0009] 10-50 parts of ABS resin, 0-20 parts of AS resin, 0-25 parts of high-rubber powder, 50-90 parts of inorganic filler, 0.1-10 parts of reactive organic matter, 0-10 parts of elastomer, 0-5 parts of titanium dioxide, and 0-1 part of antioxidant.
[0010] Using the above technical solution:
[0011] In the present application, a large amount of high-density inorganic filler is added to the ABS resin to ensure that the density of the final ABS resin composition is greater than 2g / cm 3 However, if the filling amount of the inorganic filler is too high, the processing performance of the ABS resin composition will deteriorate (fluidity will deteriorate) and the basic mechanical properties of the material cannot be maintained.
[0012] In order to solve the above problems, in the present application, a reactive organic substance is added to the reaction system. The reactive organic substance can react with the interface of the ABS resin and the inorganic filler particles. Through the chelation effect, the interfacial bonding force of the two phases is enhanced, which has the effect of improving the toughness of the material. At the same time, the reactive organic substance and the inorganic filler act synergistically to improve the matrix strength and improve the compatibility of the inorganic filler particles with the organic ABS matrix. While maintaining a balance between high filling and fluidity of the improved composition, and in combination with the addition of other additives (such as elastomers, antioxidants, etc.), the goal of high stiffness and high toughness of the material properties is achieved.
[0013] In order to obtain better performance, the amount of components of the weighted ABS resin composition is optimized, and the composition is composed of the following raw materials in parts by weight:
[0014] 15-40 parts of ABS resin, 5-15 parts of AS resin, 3-10 parts of high-rubber powder, 55-70 parts of inorganic filler, 0.5-3 parts of reactive organic matter, 1-5 parts of elastomer, 0-5 parts of titanium dioxide, and 0.2-2 parts of antioxidant.
[0015] The controlled variable method was used to conduct the test, and it was finally determined that the optimal ratio of the weighted ABS resin composition system was composed of the following raw materials in parts by weight:
[0016] 30 parts of ABS resin, 10 parts of AS resin, 5 parts of high-rubber powder, 65 parts of inorganic filler, 2 parts of reactive organic matter, 1 part of elastomer, 1 part of titanium dioxide, and 1 part of antioxidant.
[0017] Furthermore, the reactive organic matter is an epoxy resin or an isocyanate. Preferably, the reactive organic matter is an epoxy resin with an epoxy equivalent of 25 to 3000, and more preferably, an epoxy resin with an epoxy equivalent of 3000 is selected, at which time the comprehensive performance of the ABS resin composition is the best, especially the fluidity is relatively better.
[0018] Further, the inorganic filler is calcium carbonate, barium sulfate, zinc oxide, talc, wollastonite, mica or kaolin. Preferably, the inorganic filler is calcium carbonate, barium sulfate or zinc oxide. More preferably, zinc oxide is selected, in which case the comprehensive performance of the ABS resin composition is the best, and the balance of various physical properties can be maintained while ensuring that the ABS resin composition has good molding fluidity.
[0019] Furthermore, the antioxidant is a mixture of antioxidant 1010 and antioxidant 168.
[0020] Furthermore, the density of the weighted ABS resin composition is ≥2g / cm 3 , melt index ≥12g / 10min at 230℃ and 2.16KG, tensile strength ≥16MPa, flexural modulus ≥2400MPa, unnotched impact strength ≥8kJ / m 2 .
[0021] The second aspect of the present invention provides a method for preparing the above-mentioned weighted ABS resin composition, comprising the following steps:
[0022] S1. Weigh ABS resin, AS resin, high-rubber powder, inorganic filler, reactive organic matter, elastomer, titanium dioxide and antioxidant according to weight ratio, and stir and mix the above raw materials evenly;
[0023] S2. Add the mixed materials into a twin-screw extruder with a melting temperature of 200-240°C and a screw speed of 300-500rpm. After sufficient melting, compounding, extrusion, drawing, cooling, pelletizing and drying, the finished product is obtained.
[0024] The third aspect of the present invention provides an application of the above-mentioned weighted ABS resin composition, wherein the weighted ABS resin composition has a high specific gravity and good fluidity, while achieving the best effect of the toughness and rigidity of the material, and is used for processing and producing cosmetic packaging containers, household electronic products, and office supplies.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] In the present invention, a large amount of high-density inorganic filler is added to the ABS resin to ensure that the density of the final ABS resin composition is greater than 2g / cm 3 , and adding reactive organic matter into the reaction system, the reactive organic matter can react with the interface of ABS resin and inorganic filler particles, and through chelation, the interfacial bonding force of the two phases is enhanced, which has the effect of improving the toughness of the material. At the same time, the reactive organic matter and the inorganic filler work synergistically, and the purpose of improving the strength of the matrix and improving the compatibility of the inorganic filler particles with the organic ABS matrix is achieved. While maintaining the balance of high filling and fluidity of the improved composition, and in combination with the addition of other additives (such as elastomers, antioxidants, etc.), the goal of high stiffness and high toughness of the material properties is achieved. DETAILED DESCRIPTION
[0027] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In each embodiment, the experimental methods used are conventional methods unless otherwise specified; the various reagents and raw materials used are commercially available products or products that can be prepared by known methods unless otherwise specified.
[0029] The epoxy equivalent weight of epoxy resin 1 is 250; the epoxy equivalent weight of epoxy resin 2 is 3000;
[0030] High-glue powder is a core-shell polymer, which contains glue components inside. Its glue content is 55%-70%. In each embodiment, high-glue powder adopts Kumho HR181;
[0031] The elastomer is added to the ABS resin system to play a toughening role. The elastomer in the embodiment is Sumitomo Chemical BF-7M.
[0032] Examples 1-12
[0033] A weighted ABS resin composition, the weight parts of its components are as shown in Table 1, wherein:
[0034] The weighted ABS resin composition is prepared by the following steps:
[0035] S1. Weigh ABS resin, AS resin, high-rubber powder, inorganic filler, reactive organic matter, elastomer, titanium dioxide and antioxidant according to weight ratio, add the above raw materials into a high-speed mixer, stir for 1-2 minutes at a speed of 100 rpm, stir for 2-5 minutes at a speed of 300 rpm, and stir and mix evenly;
[0036] S2. Add the mixed materials into a twin-screw extruder with a melting temperature of 200-240°C and a screw speed of 300-500rpm. After sufficient melting, compounding, extrusion, drawing, cooling, pelletizing and drying, the finished product is obtained.
[0037] Table 1 Composition by weight of each component in Examples 1-12
[0038]
[0039] Comparative Examples 1-4
[0040] The only difference between Comparative Examples 1-4 and Example 6 in the present invention is that the contents of the inorganic filler-zinc oxide and the reactive organic matter-epoxy resin 2 in the raw material components are adjusted, as shown in Table 2 for details.
[0041] Table 2 Composition by weight of each component in Comparative Examples 1-4
[0042]
[0043] After the extruded materials in Examples 1-12 and Comparative Examples 1-4 were dried, the injection molded specimens were subjected to corresponding performance tests according to the following standards (the test standard for the flexural strength of the finished product is ISO 527, the test standard for the flexural modulus and tensile strength of the finished product is ISO 178, the test standard for the impact strength (unnotched) of the finished product is ISO 180, the test standard for the melt index of the finished product is ISO 1133, and the test standard for the density of the finished product is ISO 1183). The specific test results are shown in Table 3.
[0044] Table 3 Test results of various properties of finished products
[0045]
[0046] From the test results in Table 3, it can be seen that the density of the weighted ABS resin composition prepared by the preferred formula ratio of the present invention is ≥2g / cm 3 , melt index ≥12g / 10min at 230℃ and 2.16KG, tensile strength ≥16MPa, flexural modulus ≥2400MPa, unnotched impact strength ≥8kJ / m 2, with high specific gravity, good processing fluidity, and at the same time achieving the best effect of material toughness and rigidity. Among them, the weighted ABS resin composition prepared by the formula ratio in Example 6 has the best performance.
[0047] The test results of the finished product performance of Example 2, Example 5 and Example 12 are compared. In Example 12, the reactive organic matter is isocyanate, in Example 2, the reactive organic matter is epoxy resin 1 with an epoxy equivalent of 250, and in Example 5, the reactive organic matter is epoxy resin 2 with an epoxy equivalent of 3000, to illustrate the effect of the type of reactive organic matter on the performance of the finished product. When the reactive organic matter is epoxy resin 2 with an epoxy equivalent of 3000, the comprehensive performance of the finished product is better than that of isocyanate or epoxy resin 1 with an epoxy equivalent of 250, especially, the fluidity (melt index) of the finished product is relatively better.
[0048] The test results of the finished product performance of Examples 3, 4 and 5 are compared. In Example 3, the inorganic filler is calcium carbonate, in Example 4, the inorganic filler is barium sulfate, and in Example 5, the inorganic filler is zinc oxide, to illustrate the influence of the type of inorganic filler on the performance of the finished product. When zinc oxide is selected as the inorganic filler, which is equivalent to calcium carbonate and barium sulfate, the performance of the finished product is the best, and the balance of various physical properties can be maintained while ensuring the molding fluidity.
[0049] The finished product performance test results of Examples 5, 6, 7 and Comparative Examples 1 and 2 are compared. In Example 5, the amount of reactive organic matter-epoxy resin 2 added is 1 part by weight, in Example 6, the amount of reactive organic matter-epoxy resin 2 added is 2 parts by weight, in Example 7, the amount of reactive organic matter-epoxy resin 2 added is 3 parts by weight, no reactive organic matter is added in Comparative Example 1, and the amount of reactive organic matter-epoxy resin 2 added in Comparative Example 2 is 4 parts by weight, to illustrate the influence of the content of reactive organic matter-epoxy resin 2 on the performance of the finished product. When the amount of reactive organic matter-epoxy resin 2 added is too high, the viscosity of the finished product is too large and cannot be formed. When the amount of reactive organic matter-epoxy resin 2 added is too low or not added, the melt fluidity and mechanical properties of the finished product are poor. Among them, when the amount of reactive organic matter-epoxy resin 2 added in Example 6 is 2 parts by weight, the various properties of the finished product are the best.
[0050] The test results of the finished product performance of Example 1 and Example 5 are compared to illustrate the influence of the ratio of AS resin to ABS resin on the performance of the finished product, and to illustrate that appropriately increasing the content of AS resin in the system is beneficial to improving various properties of the finished product.
[0051] The finished product performance test results of Example 5 are compared with those of Comparative Examples 3 and 4 to illustrate the influence of the content of inorganic filler-zinc oxide on the performance of the finished product. When the content of inorganic filler-zinc oxide is outside 50-90 parts by weight (within the range of protection of the claims), the performance of the finished product is significantly reduced. When the content of inorganic filler-zinc oxide is lower than the above lower limit, the high density requirement is not met. When the content of inorganic filler-zinc oxide is higher than the above upper limit, the impact strength of the obtained finished product is low, and the fluidity is poor and molding is difficult.
[0052] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A weighted ABS resin composition, characterized in that: It is composed of the following raw materials in parts by weight: 10-50 parts of ABS resin, 0-20 parts of AS resin, 0-25 parts of high-rubber powder, 50-90 parts of inorganic filler, 0.5-3 parts of reactive organic matter, 0-10 parts of elastomer, 0-5 parts of titanium dioxide, and 0-1 part of antioxidant.
2. The weighted ABS resin composition according to claim 1, characterized in that: It is composed of the following raw materials in parts by weight: 15-40 parts of ABS resin, 5-15 parts of AS resin, 3-10 parts of high-rubber powder, 55-70 parts of inorganic filler, 0.5-3 parts of reactive organic matter, 1-5 parts of elastomer, 0-5 parts of titanium dioxide, and 0.2-2 parts of antioxidant.
3. The weighted ABS resin composition according to claim 1 or 2, characterized in that: The reactive organic matter is epoxy resin or isocyanate.
4. The weighted ABS resin composition according to claim 3, characterized in that: The reactive organic matter is an epoxy resin with an epoxy equivalent of 25 to 3000.
5. The weighted ABS resin composition according to claim 1 or 2, characterized in that: The inorganic filler is calcium carbonate, barium sulfate, zinc oxide, talc, wollastonite, mica or kaolin.
6. The weighted ABS resin composition according to claim 5, characterized in that: The inorganic filler is zinc oxide.
7. The weighted ABS resin composition according to claim 1 or 2, characterized in that: The antioxidant is a mixture of antioxidant 1010 and antioxidant 168.
8. A method for preparing a weighted ABS resin composition as claimed in claim 1, characterized in that: The following steps are involved: S1. Weigh ABS resin, AS resin, high-rubber powder, inorganic filler, reactive organic matter, elastomer, titanium dioxide and antioxidant according to weight ratio, and stir and mix the above raw materials evenly; S2. Add the mixed materials into a twin-screw extruder with a melting temperature of 200-240°C and a screw speed of 300-500rpm. After sufficient melting, compounding, extrusion, drawing, cooling, pelletizing and drying, the finished product is obtained.
9. An application of a weighted ABS resin composition as claimed in any one of claims 1 to 7, characterized in that: The weighted ABS resin composition is used for processing and producing cosmetic packaging containers, household electronic products, and office supplies.