Recycled PC / PET reclaimed material and preparation method thereof
By using reinforcement and compatibility agents prepared by diatomaceous earth and other materials in PC/PET recycling materials, the compatibility and dispersion of the recycling materials are improved, and the problems of low mechanical strength and wear resistance of the recycling materials are solved. Achieve high-performance recycled materials suitable for electronic products.
Patent Information
- Application Number
- CN202411193259.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
The existing PC/PET mixed recycled materials have low mechanical strength and wear resistance, mainly due to poor impurity composition and compatibility, resulting in material aging and molecular segment breakage during long-term use.
Use the optimized ratio of PET recycling and PC recycling, and use reinforcement consisting of diatomaceous earth, allyl polyoxyethylene methyl terminated polyether, long-chain alkyl silane coupling agent and pentaerythritol glycidyl ether The agent is compounded and combined with compatible agents and antioxidants to improve compatibility and dispersion, improve mechanical properties and wear resistance.
The produced recycled PC/PET recycled materials have good mechanical properties and wear resistance. They are suitable for electronic product shells and other fields. The tensile strength is improved, the number of wear resistance increases, and they show good aging after weather resistance test. performance.
Smart Images

Figure BDA0005015665130000051 
Figure BDA0005015665130000061 
Figure BDA0005015665130000062
Abstract
Description
Technical Field
[0001] The present application relates to the field of recycled plastic materials, and more specifically, to a recycled PC / PET regenerated material and a preparation method thereof. Background Art
[0002] With the continuous development of the national economy and the continuous tightening of low-carbon emission policies, people's awareness of environmental protection has gradually increased, and the recycling and reuse of polymer materials has become a hot topic in current research; PC (polycarbonate) and PET (polyethylene terephthalate) are widely used engineering plastics, and their recycling and regeneration technology is of great significance to resource conservation and environmental protection.
[0003] However, the existing PC / PET mixed recycled materials have the problems of unstable performance and poor compatibility. In the prior art, some compatibilizers are added to improve the compatibility of PC and PET. However, due to the large amount of impurities in the recycled PC and PET, the amount of compatibilizer required to be added is also large, which reduces the mechanical strength and wear resistance of the obtained PC / PET mixed recycled materials. Summary of the invention
[0004] In order to solve the problem of low mechanical strength and wear resistance of existing PC / PET mixed recycled materials, the present application provides a recycled PC / PET recycled material and a preparation method thereof.
[0005] In the first aspect, the present application provides a method for recycling PC / PET recycled materials, using the following technical solution: A recycled PC / PET material is prepared from the following raw materials in parts by weight: 50-80 parts of PET recycled material 30-60 pieces of PC recycled materials Reinforcing agent 20-25 parts Compatibilizer 2-4 parts 1-3 parts of antioxidants; The reinforcing agent consists of diatomaceous earth, allyl polyoxyethylene methyl terminated polyether, long-chain alkyl silane coupling agent and pentaerythritol glycidyl ether.
[0006] By adopting the above technical scheme, the present application uses PET recycled materials and PC recycled materials as matrix materials to prepare recycled PC / PET recycled materials. Since PET recycled materials and PC recycled materials contain a large amount of impurities, such as polyolefin resins, powder fillers, etc., the compatibility of the mixed PET recycled materials and PC recycled materials is reduced, and during the long-term use of PET recycled materials and PC recycled materials, material aging will occur, and there will be molecular chain breakage, which will result in low mechanical strength and wear resistance of the recycled PC / PET recycled materials.
[0007] In the present application, PET recycled material and PC recycled material are mixed in an optimal dosage ratio, and reinforced and compatibilized with an optimal dosage to improve the compatibility and dispersibility of the PET recycled material and the PC recycled material, and then compounded with an antioxidant to improve the aging resistance. The recycled PC / PET recycled material thus prepared has good mechanical properties and wear resistance, and is suitable for use in the fields of electronic product casings.
[0008] The reinforcing agent of the present application is composed of diatomaceous earth, allyl polyoxyethylene methyl end-capped polyether, long-chain alkyl silane coupling agent and pentaerythritol glycidyl ether; the diatomaceous earth has a large specific surface area and has a large number of microporous structures, and the long-chain alkyl silane coupling agent can be adsorbed on the surface of the diatomaceous earth. Under the synergistic enhancement and infiltration effect of allyl polyoxyethylene methyl end-capped polyether and pentaerythritol glycidyl ether, a reinforcing agent with good dispersion and reinforcing properties is prepared, which can be evenly filled in the molecular gaps of PET recycled materials and PC recycled materials; the reinforcing agent and the compatibilizer produce a good synergistic effect, and the molecular chain segments are intertwined with each other, thereby improving the compatibility of PET recycled materials and PC recycled materials, thereby improving the mechanical properties and wear resistance of the prepared recycled PC / PET recycled materials.
[0009] Preferably, the weight ratio of the diatomaceous earth, the allyl polyoxyethylene methyl terminated polyether, the long-chain alkyl silane coupling agent and the pentaerythritol glycidyl ether is 4:(1-2):(1-2):(2-3).
[0010] By adopting the above technical scheme, diatomaceous earth, allyl polyoxyethylene methyl terminated polyether, long-chain alkyl silane coupling agent and pentaerythritol glycidyl ether are compounded with a better dosage ratio, and the reinforcing agent prepared in this way has good dispersibility in PET recycled materials and PC recycled materials.
[0011] Preferably, the reinforcing agent is prepared by the following steps: A long-chain alkyl silane coupling agent is added to diatomaceous earth for dispersion, and then allyl polyoxyethylene methyl terminated polyether and pentaerythritol glycidyl ether are added, and the temperature is raised to 90-110° C. for kneading and stirring for 1-2 hours to obtain a reinforcing agent.
[0012] By adopting the above technical scheme, the reinforcing agent is prepared under better kneading conditions and preparation process, and the reinforcing agent prepared in this way has better dispersibility and processing stability.
[0013] Preferably, the long-chain alkylsilane coupling agent is one or a combination of n-octyltrimethoxysilane, n-octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane and octadecyltrimethoxysilane.
[0014] By adopting the above technical scheme, the above long-chain alkyl silane coupling agent has a hydrophilic group and a hydrophobic soft long chain, which can modify the surface of diatomite, improve the dispersion and wettability of diatomite in allyl polyoxyethylene methyl end-capped polyether and pentaerythritol glycidyl ether, and at the same time can be interwoven with the molecular structure of allyl polyoxyethylene methyl end-capped polyether and pentaerythritol glycidyl ether, thereby improving the dispersion and compatibility of the prepared reinforcing agent with PET recycled materials and PC recycled materials.
[0015] Preferably, the compatibilizer is ethylene-butyl acrylate-glycidyl methacrylate copolymer and / or ethylene-1-octene copolymer grafted with glycidyl methacrylate.
[0016] By adopting the above technical solution, the above compatibilizer can produce a good synergistic effect with the reinforcing agent, thereby improving the compatibility of PET recycled materials and PC recycled materials.
[0017] Preferably, the diatomaceous earth is pretreated diatomaceous earth, which is obtained by ball-milling diatomaceous earth with a short-chain alcohol, the weight ratio of the diatomaceous earth to the short-chain alcohol is 100:(3-8), and the short-chain alcohol is any one of propylene glycol, ethylene glycol and butanediol.
[0018] By adopting the above technical scheme and using short-chain alcohol to pretreat diatomite, the adsorption stability of diatomite can be improved, and the obtained pretreated diatomite can be better dispersed with allyl polyoxyethylene methyl terminated polyether, long-chain alkyl silane coupling agent and pentaerythritol glycidyl ether, thereby improving the mechanical strength and wear resistance of the obtained recycled PC / PET recycled materials.
[0019] Preferably, the PET recycled material is obtained by crushing, washing and screening PET waste, and the longest dimension of the PET recycled material is less than 5 mm; the PC recycled material is obtained by crushing, washing and screening PC waste, and the longest dimension of the PET recycled material is less than 5 mm.
[0020] By adopting the above technical scheme, PET waste and PC waste are processed by crushing, washing and screening to prepare PET recycled materials and PC recycled materials with the longest size less than 5 mm. Some impurities can be removed during the washing process, and controlling the optimal size can enable the PET recycled material and PC waste to be melted evenly during the processing and melting process, thereby improving the mixing and melting uniformity.
[0021] Preferably, the antioxidant is antioxidant 1010 and / or antioxidant 168.
[0022] By adopting the above technical solution, the above antioxidant has good antioxidant properties, which can improve the aging resistance of the recycled PC / PET recycled materials, thereby increasing the service life.
[0023] In a second aspect, the present application provides a method for preparing recycled PC / PET recycled materials, using the following technical solution: A method for preparing recycled PC / PET recycled materials, comprising the following steps: The PET recycled material, PC recycled material, reinforcing agent, compatibilizer and antioxidant are added into a mixing device, mixed evenly, melt-extruded, cooled, dried and pelletized to obtain recycled PC / PET recycled material.
[0024] By adopting the above technical scheme, using the preparation process of mixing, melt extrusion molding, cooling, drying and pelletizing, the recycled PC / PET recycled material of the present application is prepared.
[0025] Preferably, the melting temperature is 250-280°C.
[0026] By adopting the above technical solution, the optimal melting temperature can make the various raw materials evenly mixed and melted, thereby improving the comprehensive performance of the recycled PC / PET recycled materials.
[0027] In summary, this application has the following beneficial effects: 1. The recycled PC / PET material of the present application is mixed with PET recycled material and PC recycled material in an optimal dosage ratio, and compounded with a reinforcing agent and a compatibilizer in an optimal dosage, wherein the reinforcing agent is composed of diatomaceous earth, allyl polyoxyethylene methyl terminated polyether, long-chain alkyl silane coupling agent and pentaerythritol glycidyl ether, and can be evenly filled in the molecular gaps of the PET recycled material and the PC recycled material; the reinforcing agent and the compatibilizer produce a good synergistic effect, and the molecular chain segments are intertwined with each other, thereby improving the compatibility of the PET recycled material and the PC recycled material, thereby improving the mechanical properties and wear resistance of the obtained recycled PC / PET recycled material, and then compounding with an antioxidant to improve the aging resistance. The recycled PC / PET recycled material obtained in this way has good mechanical properties and wear resistance, and is suitable for use in the fields of electronic product casings.
[0028] 2. By using ethylene-butyl acrylate-glycidyl methacrylate copolymer and / or ethylene-1-octene copolymer grafted with glycidyl methacrylate as a compatibilizer, it has a good synergistic effect with the reinforcing agent and improves the compatibility of PET recycled materials and PC recycled materials.
[0029] 3. By using short-chain alcohol to pre-treat diatomite by ball milling, the adsorption stability of diatomite can be improved, and the obtained pre-treated diatomite can be well dispersed with allyl polyoxyethylene methyl-terminated polyether, long-chain alkyl silane coupling agent and pentaerythritol glycidyl ether, thereby improving the mechanical strength and wear resistance of the obtained recycled PC / PET recycled materials. DETAILED DESCRIPTION
[0030] The present application is further described in detail below in conjunction with embodiments.
[0031] The following are the sources and specifications of some raw materials of this application. The raw materials used in the preparation examples and embodiments of this application can be obtained from the market, including but not limited to the raw materials of the following models and manufacturers. Raw materials with equivalent performance can be used: 1. PET recycled material: plastic recycling plant, tensile strength 25-27MPa, density 1.25g / cm 3 ; 2. PC recycled material: plastic recycling plant, tensile strength 20-23MPa, density 1.23g / cm 3 ; 3. Diatomaceous earth: 400-800 mesh; 4. Allyl polyoxyethylene methyl terminated polyether: CAS No. 27252-80-8, content 98% g / kg; 5. Pentaerythritol glycidyl ether: CAS#3126-63-4, content 95%, gm; 6. Ethylene-butyl acrylate-glycidyl methacrylate copolymer: DuPont, USA, PTW-1; 7. Ethylene-1-octene copolymer grafted with glycidyl methacrylate: Jiayirong, SOG-03.
[0032] Preparation example of pretreated diatomaceous earth Preparation Example 1 Preparation Example 1 discloses a pretreated diatomaceous earth prepared by the following steps: 0.3 kg of propylene glycol as a short-chain alcohol was added to 10 kg of commercially available diatomaceous earth, and the mixture was ball-milled for 20 minutes at a rotation speed of 500 r / min to obtain pretreated diatomaceous earth.
[0033] Preparation Example 2 The difference between Preparation Example 2 and Preparation Example 1 is that 0.5 kg of ethylene glycol as a short-chain alcohol is added to 10 kg of commercially available diatomaceous earth, and the mixture is ball-milled for 30 minutes at a rotation speed of 750 r / min to obtain pretreated diatomaceous earth.
[0034] Preparation Example 3 The difference between Preparation Example 3 and Preparation Example 1 is that 0.8 kg of butanediol as a short-chain alcohol is added to 10 kg of commercially available diatomaceous earth, and the mixture is ball-milled at a rotation speed of 1000 r / min for 40 min to obtain pretreated diatomaceous earth.
[0035] Preparation example of reinforcing agent Preparation Example 4 Preparation Example 4 discloses a reinforcing agent prepared by the following steps: 1 kg of n-octyltrimethoxysilane was added to 6 kg of commercially available diatomaceous earth as a long-chain alkylsilane coupling agent for dispersion, and then 0.5 kg of allyl polyoxyethylene methyl terminated polyether and 2 kg of pentaerythritol glycidyl ether were added, and the temperature was raised to 90-110° C. for kneading and stirring for 1-2 hours to obtain a reinforcing agent.
[0036] Preparation Example 5-7 The difference between Preparation Examples 5-7 and Preparation Example 4 is that the amounts of raw materials used and the preparation conditions are different, see Table 1 below for details.
[0037] Table 1 Raw material dosage and preparation conditions of Preparation Examples 4-7 Preparation Examples 8-10 The difference between Preparation Examples 8-10 and Preparation Example 5 is that the sources of diatomaceous earth are different, see Table 2 below for details.
[0038] Table 2 Sources of diatomaceous earth in Preparation Examples 8-10 Preparation Example Source of Diatomaceous Earth Preparation Example 8 Preparation Example 1 Preparation Example 9 Preparation Example 2 Preparation Example 10 Preparation Example 3 Preparation Comparative Example 1 The difference between Preparation Comparative Example 1 and Preparation Example 4 is that an equal amount of allyl polyoxyethylene methyl terminated polyether is replaced with pentaerythritol glycidyl ether, and the rest is the same as Preparation Example 4.
[0039] Preparation Comparative Example 2 The difference between Preparation Comparative Example 2 and Preparation Example 4 is that the long-chain alkyl silane coupling agent is replaced with vinyl trimethoxy silane, and the other steps are the same as Preparation Example 4.
[0040] Preparation Comparative Example 3 The difference between Preparation Comparative Example 3 and Preparation Example 4 is that an equal amount of pentaerythritol glycidyl ether is replaced by glycidyl methacrylate, and the rest is the same as Preparation Example 4. Example
[0041] Example 1 Example 1 discloses a recycled PC / PET regrind, which is prepared by the following steps: 5kg PET recycled material, 3kg PC recycled material, 2kg of the reinforcing agent prepared in Preparation Example 4, 0.2kg ethylene-butyl acrylate-glycidyl methacrylate copolymer as a compatibilizer and 0.1lg antioxidant 1010 are added to a mixer, and after mixing evenly, the processing temperature in the screw extruder is controlled to 250°C in zone 1, 260°C in zone 2, 265°C in zone 3, 275°C in zone 4, 260°C in zone 5, and 255°C at the die head, and melt extrusion molding is performed, water cooling, hot air drying, and pelletizing are performed to obtain recycled PC / PET recycled material.
[0042] Embodiment 2-4 The difference between Example 2-4 and Example 1 is that the amount of raw materials used and the source of the reinforcing agent are different, see Table 3 below for details.
[0043] Table 3 The amount of raw materials and the source of reinforcing agent in Examples 1-4 Embodiment 5-7 The difference between Examples 5-7 and Example 1 is that the sources of the reinforcing agent are different, see Table 4 below for details.
[0044] Table 4 Sources of reinforcing agents for Examples 5-7 Example Sources of reinforcing agents Example 5 Preparation Example 8 Example 6 Preparation Example 9 Example 7 Preparation Example 10 Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the reinforcing agent is derived from the preparation of Comparative Example 1, and the rest is the same as Example 1.
[0045] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the reinforcing agent is derived from the preparation of Comparative Example 2, and the rest is the same as Example 1.
[0046] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the reinforcing agent is derived from the preparation of Comparative Example 3, and the rest is the same as Example 1.
[0047] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that the amount of the reinforcing agent is 1.5 kg, the amount of the compatibilizer is 0.7 kg, and the others are the same as Example 1.
[0048] Comparative Example 5 The difference between Comparative Example 5 and Example 1 is that the reinforcing agent consists of 1.5 kg of commercially available diatomaceous earth and 0.5 kg of n-octyltrimethoxysilane coupling agent, and the rest is the same as Example 1.
[0049] Performance Test The following performance tests were conducted on the PC / PET recycled materials obtained in Examples 1-7 and Comparative Examples 1-5: The recycled PC / PET material prepared above was placed in an oven at 75°C for 90 minutes and then injection molded at 275°C using an injection molding machine. The test strip thickness was 1 mm and was cut according to the test standard for testing.
[0050] 1. Tensile strength test: According to the test method in GB / T 1040-2006, test the tensile strength (unit: MPa) of recycled PC / PET materials, test and record the test results; 2. Weather resistance test: Place the test strip in a constant temperature and humidity chamber at 85°C and 85% humidity for 7 days, then wipe it dry and return it to room temperature (25°C). Test the tensile strength (unit: MPa) according to the test method in GB / T 1040-2006, and record the test results. 3. Wear resistance: Use TABER abrasion tester, load 500g, set the number of test laps, adjust the speed to 60r / min for testing, observe every 25 laps, record the number of frictions when the test strip shows wear, scratches or discoloration, test and record the test results; The following are the performance test data of the recycled PC / PET materials obtained in Examples 1-7 and Comparative Examples 1-5, see Table 5 below for details.
[0051] Table 5 Performance data of recycled PC / PET recycled materials of Examples 1-7 and Comparative Examples 1-5 Combining Examples 1-4 and Comparative Examples 1-3, 5 and Table 5, it can be concluded that the use of diatomaceous earth, long-chain alkyl silane coupling agent, allyl polyoxyethylene methyl end-capped polyether and pentaerythritol glycidyl ether in a preferred dosage ratio as a reinforcing agent, the obtained recycled PC / PET recycled material has good mechanical properties and wear resistance, the tensile strength can reach 40.5MPa, the wear resistance number can reach 1375 times, and after the weather resistance test, the tensile strength only decreases by 1MPa; while the tensile strength and wear resistance of the recycled PC / PET recycled materials obtained in Comparative Examples 1-3 and Comparative Example 5 are significantly reduced, indicating that there is no synergistic effect of diatomaceous earth, long-chain alkyl silane coupling agent, allyl polyoxyethylene methyl end-capped polyether and pentaerythritol glycidyl ether in Comparative Examples 1-3 and Comparative Example 5, which reduces the dispersion and filling performance of the reinforcing agent in the PC recycled material and the PET recycled material, thereby reducing the mechanical properties and wear resistance of the obtained recycled PC / PET recycled material.
[0052] Combining Examples 2-4 and Examples 5-7 with Table 5, it can be seen that before preparing the reinforcing agent, the diatomaceous earth is pretreated with a short carbon chain alcohol, and the pretreated diatomaceous earth obtained is applied to the reinforcing agent. The recycled PC / PET recycled material has good mechanical properties and wear resistance, the tensile strength can reach 42.3 MPa, the wear resistance can reach 1500 times, and after the weather resistance test, the tensile strength only decreases by 0.5 MPa.
[0053] Furthermore, in combination with Example 1 and Comparative Example 4 and Table 5, it can be seen that the use of a better dosage ratio of reinforcing agent and compatibilizer for compounding can improve the mechanical properties and wear resistance of the recycled PC / PET recycled material. In Comparative Example 4, the compatibilizer is increased and the reinforcing agent is reduced, and the tensile strength and wear resistance of the recycled PC / PET recycled material are reduced.
[0054] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for recycling PC / PET recycled materials, characterized in that: Made from the following raw materials in parts by weight: 50-80 parts of PET recycled material 30-60 PC recycled materials Reinforcing agent 20-25 parts 2-4 parts of compatibilizer 1-3 parts of antioxidants; The reinforcing agent consists of diatomaceous earth, allyl polyoxyethylene methyl terminated polyether, long-chain alkyl silane coupling agent and pentaerythritol glycidyl ether.
2. The PC / PET recycled material according to claim 1, characterized in that: The weight ratio of the diatomaceous earth, the allyl polyoxyethylene methyl terminated polyether, the long-chain alkyl silane coupling agent and the pentaerythritol glycidyl ether is 4:(1-2):(1-2):(2-3).
3. The PC / PET recycled material according to claim 1, characterized in that: The reinforcing agent is prepared by the following steps: A long-chain alkyl silane coupling agent is added to diatomaceous earth for dispersion, and then allyl polyoxyethylene methyl terminated polyether and pentaerythritol glycidyl ether are added, and the temperature is raised to 90-110° C. for kneading and stirring for 1-2 hours to obtain a reinforcing agent.
4. The PC / PET recycled material according to claim 1, characterized in that: The long-chain alkylsilane coupling agent is one or a combination of n-octyltrimethoxysilane, n-octyltriethoxysilane, dodecyltrimethoxysilane, dodecyltriethoxysilane, hexadecyltrimethoxysilane and octadecyltrimethoxysilane.
5. The PC / PET recycled material according to claim 1, characterized in that: The compatibilizer is ethylene-butyl acrylate-glycidyl methacrylate copolymer and / or ethylene-1-octene copolymer grafted with glycidyl methacrylate.
6. The PC / PET recycled material according to claim 1, characterized in that: The diatomaceous earth is pretreated diatomaceous earth, which is obtained by ball-milling diatomaceous earth with a short-chain alcohol. The weight ratio of the diatomaceous earth to the short-chain alcohol is 100:(3-8), and the short-chain alcohol is any one of propylene glycol, ethylene glycol and butanediol.
7. The PC / PET recycled material according to claim 1, characterized in that: The PC recycled material is obtained by crushing, washing and screening PC waste, and the longest dimension of the PET recycled material is less than 5 mm; the PET recycled material is obtained by crushing, washing and screening PET waste, and the longest dimension of the PET recycled material is less than 5 mm.
8. The PC / PET recycled material according to claim 1, characterized in that: The antioxidant is antioxidant 1010 and / or antioxidant 168.
9. A method for preparing recycled PC / PET regenerated material according to any one of claims 1 to 8, characterized in that: The PET recycled material, PC recycled material, reinforcing agent, compatibilizer and antioxidant are added into a mixing device, mixed evenly, melt-extruded, cooled, dried and pelletized to obtain recycled PC / PET recycled material.
10. The method for preparing recycled PC / PET materials according to claim 9, characterized in that: The melting temperature is 250-280°C.
Citation Information
Cited By
PC material based on waste PC car lamp and preparation method of PC material
CN119978757A