Resin composition
By reasonably formulating epoxy resin, allyl active ester resin and organic filler materials in the resin composition, the problem of large resin leakage is solved, and the bending resistance of the insulating layer is improved and the media performance is improved. It is suitable for Printed wiring board and semiconductor device.
Patent Information
- Application Number
- CN202410567912.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-17
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
The exudation of the resin of the conventional resin composition during the lamination process is too large, resulting in uneven thickness of the insulating layer, which is difficult to control, and affects the bending resistance of the printed wiring board.
Using a resin composition containing an epoxy resin, an allyl active ester resin and an organic filler material, the resin exudation amount is suppressed by adjusting the component ratio and adding a curing agent, an inorganic filler material, and the like, and forming curing with excellent bending resistance. Things.
The resin leakage is effectively suppressed, and the bending resistance of the insulating layer is improved, and the dielectric loss tangent is low and the dielectric constant is low. It is suitable for insulating layers for printed wiring boards and semiconductor devices.
Smart Images

Figure BDA0004829940840000021 
Figure BDA0004829940840000031 
Figure BDA0004829940840000032
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition and also to a resin sheet, a printed wiring board and a semiconductor device obtained by using the resin composition. Background Art
[0002] As a manufacturing technology for a printed wiring board, a manufacturing method based on a build-up method in which insulating layers and conductive layers are alternately stacked is known.
[0003] As an insulating material for a printed wiring board used for such an insulating layer, for example, Patent Documents 1 and 2 disclose resin compositions.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent document 1: International Publication No. 2022 / 038893;
[0007] Patent document 2: Japanese Patent Application Publication No. 2021-14577. Summary of the invention
[0008] Problems to be solved by the invention
[0009] In recent years, in order to improve the reliability of printed wiring boards, materials having high strength, particularly high bending resistance, have been required.
[0010] In addition, when the resin composition layer of the resin sheet is used to form the insulating layer, if the viscosity of the resin composition layer is low, then when the resin sheet is laminated with the inner substrate, the resin composition layer is easily enlarged by the resin exudation amount (resin flow amount) of the resin component flowing out from the support body of the resin sheet and the part between the inner substrate. If the exudation amount of the resin increases, the resin composition layer protrudes outward from the edge of the support body of the resin sheet. And, if the exudation amount of the resin increases, there is the following tendency: corresponding to the amount of the resin composition flowing out, the thickness of the resin composition layer at the end of the resin sheet is thinned. Therefore, if the exudation amount of the resin is many, the thickness of the resin composition layer becomes uneven, and it is difficult to control the thickness.
[0011] The present invention is proposed in view of the above-mentioned problems, and provides: a resin composition capable of suppressing the amount of resin bleed-out and obtaining a cured product having excellent bending resistance; a resin sheet containing the resin composition; a printed wiring board and a semiconductor device having an insulating layer formed using the resin composition.
[0012] Means for solving problems
[0013] The present inventors have conducted intensive studies on the above problems and have found that the above problems can be solved by combining (A) an epoxy resin, (B) an active ester resin having an allyl group, and a predetermined amount of (C) an organic filler, thereby completing the present invention.
[0014] That is, the present invention includes the following contents.
[0015] [1] A resin composition comprising (A) an epoxy resin, (B) an active ester resin having an allyl group, and (C) an organic filler,
[0016] However, when the non-volatile component in the resin composition is 100% by mass, the content of the component (C) is 6% by mass or less.
[0017] [2] The resin composition according to [1], further comprising (D) a curing agent.
[0018] [3] The resin composition of [2], wherein the component (D) comprises at least one selected from the group consisting of a phenol-based curing agent, a naphthol-based curing agent, a carbodiimide-based curing agent, an active ester-based curing agent (excluding a substance corresponding to the component (B)), a benzophenone-based curing agent, Oxazine-based curing agents and cyanate-based curing agents.
[0019] [4] The resin composition according to any one of [1] to [3], further comprising (E) an inorganic filler.
[0020] [5] The resin composition according to any one of [1] to [4], wherein the component (B) comprises any one of a compound represented by the general formula (B-1), a compound represented by the general formula (B-2), and a compound represented by the general formula (B-3):
[0021] [Chemical formula 1]
[0022]
[0023] In the general formula (B-1), Ar 11 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 12 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 13 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof, and n represents an integer of 0 to 10;
[0024] [Chemical formula 2]
[0025]
[0026] In the general formula (B-2), Ar 21 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 22 Each independently represents a divalent hydrocarbon group which may have a substituent, Ar 23 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, and m represents an integer of 0 to 10;
[0027] [Chemical formula 3]
[0028]
[0029] In the general formula (B-3), Ar 21 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 31 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 13 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof, and mb and nb each independently represent 0 or more.
[0030] [6] The resin composition according to any one of [1] to [7], wherein the content of the component (B) is 1% by mass or more and 25% by mass or less, when the non-volatile component in the resin composition is 100% by mass.
[0031] [7] The resin composition according to any one of [1] to [7], wherein the component (C) comprises core-shell particles.
[0032] [8] A resin sheet comprising: a support and a resin composition layer provided on the support and containing the resin composition according to any one of [1] to [7].
[0033] [9] A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to any one of [1] to [7].
[0034]
[10] A semiconductor device comprising the printed wiring board described in [9].
[0035] Effects of the Invention
[0036] According to the present invention, there can be provided: a resin composition capable of suppressing the amount of resin bleed-out and obtaining a cured product having excellent bending resistance; a resin sheet comprising the resin composition; and a printed wiring board and a semiconductor device having an insulating layer formed using the resin composition. DETAILED DESCRIPTION
[0037] Hereinafter, the present invention will be described in detail according to preferred embodiments of the present invention. However, the present invention is not limited to the following embodiments and examples, and can be implemented with any changes within the scope of the claims of the present invention and their equivalents.
[0038] [Resin composition]
[0039] Resin combination of the present invention is a resin combination containing (A) epoxy resin, (B) active ester resin with allyl group and (C) organic filler material, wherein, when the non-volatile component in the resin combination is set to 100% by mass, the content of (C) component is below 6% by mass. In the present invention, by combining (A) component, (B) component and (C) component of a prescribed amount, the exudation amount of resin can be suppressed, and a cured product with excellent bending resistance can be obtained. In addition, a cured product with a low dielectric loss tangent and a dielectric constant can also be obtained.
[0040] The resin composition can be combined with components (A) to (C) and further include optional components. As optional components, for example, (D) a curing agent (excluding a substance equivalent to component (B)), (E) an inorganic filler, (F) a curing accelerator, (G) other additives, and (H) a solvent, etc. The following describes each component contained in the resin composition in detail.
[0041] <(A) Epoxy resin>
[0042] The resin composition contains (A) epoxy resin as the (A) component. By containing (A) epoxy resin in the resin composition, a cured product having good mechanical strength and insulation reliability can be obtained. (A) Epoxy resins may be used alone or in combination of two or more.
[0043] (A) Epoxy resins include, for example, biphenylol epoxy resins, bisphenol A epoxy resins, bisphenol F epoxy resins, bisphenol S epoxy resins, bisphenol AF epoxy resins, dicyclopentadiene epoxy resins, trisphenol epoxy resins, naphthol novolac epoxy resins, phenol novolac epoxy resins, tert-butyl-catechol epoxy resins, naphthalene epoxy resins, naphthol epoxy resins, anthracene epoxy resins, glycidylamine epoxy resins, glycidylester epoxy resins. , glycidyl cyclohexane type epoxy resin, alkyl diglycidyl ether type epoxy resin, cresol novolac type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin with butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexanedimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, phenol phthalimide type epoxy resin, etc. The epoxy resin may be used alone or in combination of two or more.
[0044] The resin composition preferably contains an epoxy resin having two or more epoxy groups in one molecule as component (A). From the viewpoint of significantly obtaining the desired effect of the present invention, the proportion of the epoxy resin having two or more epoxy groups in one molecule is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more relative to 100% by mass of the epoxy resin (A).
[0045] Epoxy resins include epoxy resins that are liquid at a temperature of 20°C (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20°C (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only a liquid epoxy resin as component (A), or only a solid epoxy resin, or a combination of a liquid epoxy resin and a solid epoxy resin. Among them, from the viewpoint of significantly obtaining the effects of the present invention, it is preferred to contain a liquid epoxy resin and a solid epoxy resin in combination.
[0046] As the liquid epoxy resin, a liquid epoxy resin having two or more epoxy groups in one molecule is preferred.
[0047] As the liquid epoxy resin, preferred are bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexanedimethanol type epoxy resin, glycidyl amine type epoxy resin and epoxy resin having a butadiene structure, glycidyl cyclohexane type epoxy resin, phenol phthalimide type epoxy resin, alkyl diglycidyl ether type epoxy resin, more preferably bisphenol A type epoxy resin, bisphenol F type epoxy resin, alkyl diglycidyl ether type epoxy resin, and further preferably naphthalene type epoxy resin.
[0048] Specific examples of liquid epoxy resins include: "HP4032", "HP4032D", and "HP4032SS" (naphthalene-type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "EPIKOTE828EL" (bisphenol A-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac-type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidylamine-type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ZX1059" (a mixture of bisphenol A-type epoxy resin and bisphenol F-type epoxy resin) manufactured by Nippon Steel Chemical Materials Co., Ltd.; "EX-721" (glycidyl ester-type epoxy resin) manufactured by Nagase ChemteX; and "Celloxide "2021P" (alicyclic epoxy resin with an ester skeleton); "PB-3600" manufactured by Daicel Corporation (epoxy resin with a butadiene structure); "ZX1658" and "ZX1658GS" manufactured by Nippon Steel Chemical Materials Co., Ltd. (liquid 1,4-glycidylcyclohexane type epoxy resin); "YED216D" manufactured by Mitsubishi Chemical Corporation (alkyl diglycidyl ether type epoxy resin), etc. These can be used alone or in combination of two or more.
[0049] The solid epoxy resin is preferably a solid epoxy resin having two or more epoxy groups in one molecule, more preferably a solid epoxy resin having three or more epoxy groups in one molecule, and more preferably an aromatic solid epoxy resin having three or more epoxy groups in one molecule.
[0050] As the solid epoxy resin, preferred are biphenylol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin, and more preferred are naphthalene type epoxy resin and biphenyl type epoxy resin.
[0051] Specific examples of the solid epoxy resin include: "HP4032H" (naphthalene type epoxy resin), "HP-4700", "HP-4710" (naphthalene type tetrafunctional epoxy resin), "N-690" (cresol novolac type epoxy resin), "N-695" (cresol novolac type epoxy resin), "HP-7200", "HP-7200HH", "HP-7200H" (dicyclopentadiene type epoxy resin), "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000", "HP6000L" (naphthylene ether type epoxy resin) manufactured by DIC Corporation; "EPPN-502H" (trisphenol type epoxy resin), "NC7000L" (naphthol novolac type epoxy resin), "NC3000H", "NC3000L" (naphthylene ether type epoxy resin) manufactured by Nippon Kayaku Co., Ltd. 0", "NC3000L", "NC3100" (biphenyl type epoxy resin); "ESN475V" (naphthalene type epoxy resin), "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel Chemical Materials Co., Ltd.; "YX4000H", "YL6121" (biphenyl type epoxy resin), "YX4000HK" (biphenyl type epoxy resin), "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Corporation ; "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd.; "YL7760" (bisphenol AF type epoxy resin), "YL7800" (fluorene type epoxy resin), "jER1010" (solid bisphenol A type epoxy resin), "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "WHR-991S" (phenol phthalimide type epoxy resin) manufactured by Nippon Kayaku Co., Ltd., etc. These can be used alone or in combination of two or more.
[0052] When a liquid epoxy resin and a solid epoxy resin are used in combination as component (A), the mass ratio of the liquid epoxy resin and the solid epoxy resin is preferably 1:0.1 to 1:20, more preferably 1:0.15 to 1:10, and particularly preferably 1:0.2 to 1:5. By making the mass ratio of the liquid epoxy resin to the solid epoxy resin within the above range, the desired effect of the present invention can be significantly obtained.
[0053] The epoxy equivalent of component (A) is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., further preferably 80 g / eq. to 2000 g / eq., and further preferably 110 g / eq. to 1000 g / eq. By being within this range, a cured product of the resin composition having a sufficient crosslinking density can be obtained. The epoxy equivalent is the mass of an epoxy resin containing 1 equivalent of epoxy groups. The epoxy equivalent can be measured in accordance with JIS K7236.
[0054] From the viewpoint of significantly obtaining the desired effects of the present invention, the weight average molecular weight (Mw) of the component (A) is preferably 100 to 5000, more preferably 150 to 3000, and even more preferably 200 to 1500. The weight average molecular weight of the epoxy resin is a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).
[0055] From the viewpoint of obtaining a cured product showing good mechanical strength and insulation reliability, when the non-volatile component in the resin combination is set to 100% by mass, the content of component (A) is preferably more than 1% by mass, more preferably more than 5% by mass, and further preferably more than 8% by mass. The upper limit is preferably below 30% by mass, more preferably below 20% by mass, and particularly preferably below 15% by mass.
[0056] In the present invention, unless otherwise specified, the content of each component in the resin composition is a value when the non-volatile component in the resin composition is 100 mass %, and the non-volatile component refers to the entire non-volatile component excluding the solvent in the resin composition.
[0057] <(B) Active ester resin having an allyl group>
[0058] The resin composition contains (B) an active ester resin having an allyl group as the (B) component. The (B) component does not contain a substance equivalent to the above-mentioned (A) component. By making the resin composition contain the (B) component, a cured product with excellent bending resistance can be obtained. The (B) component can be used alone or in combination of two or more.
[0059] As the component (B), a compound having an active ester site and an allyl group that react with the component (A) can be used.
[0060] As the active ester site possessed by the (B) component, an aromatic ester skeleton is preferably used. The aromatic ester skeleton refers to a skeleton having an ester bond and an aromatic ring bonded to one or both ends of the ester bond. Among them, the aromatic ester skeleton preferably has aromatic rings at both ends of the ester bond. As a group having such a skeleton, for example, there can be mentioned: arylcarbonyloxy, aryloxycarbonyl, arylenecarbonyloxy, aryleneoxycarbonyl, arylcarbonyloxyarylene, aryloxycarbonylarylene, arylenecarbonyloxyarylene, aryleneoxycarbonylarylene, etc. In addition, the number of carbon atoms of the group having such a skeleton is preferably 7 to 20, more preferably 7 to 15, and further preferably 7 to 11. Aromatic hydrocarbon groups such as aryl and arylene may have substituents.
[0061] The aryl group is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and still more preferably an aryl group having 6 to 10 carbon atoms. Examples of such an aryl group include phenyl, furyl, pyrrolyl, thienyl, imidazolyl, pyrazolyl, Azolyl, iso The group obtained by removing one hydrogen atom from a monocyclic aromatic compound such as oxazolyl, thiazolyl, isothiazolyl, pyridyl, pyrimidinyl, pyridazinyl, pyrazinyl, triazinyl, etc.; the group obtained by removing one hydrogen atom from a condensed-ring aromatic compound such as naphthyl, anthracenyl, phenanthrenyl, quinolyl, isoquinolyl, quinazolyl, phthalazinyl, pteridinyl, coumarin, indolyl, benzimidazolyl, benzofuranyl, acridinyl, etc.
[0062] The arylene group is preferably an arylene group having 6 to 30 carbon atoms, more preferably an arylene group having 6 to 20 carbon atoms, and still more preferably an arylene group having 6 to 10 carbon atoms. Examples of such an arylene group include phenylene, naphthylene, anthrylene, biphenylene (-C6H4-C6H4-) and the like.
[0063] The terminal of the component (B) is preferably a monovalent aromatic hydrocarbon group. Examples of the monovalent aromatic hydrocarbon group include an aryl group, and the aryl group is as described above. The monovalent aromatic hydrocarbon group at the terminal of the component (B) is preferably a phenyl group.
[0064] The component (B) may have any of an aromatic hydrocarbon group, an aliphatic hydrocarbon group, an oxygen atom, a sulfur atom, and a group consisting of a combination thereof in addition to an allyl group and an aromatic ester skeleton. The term "aromatic hydrocarbon group" refers to a hydrocarbon group containing an aromatic ring, which may be a monocyclic, polycyclic, or heterocyclic ring.
[0065] As the aromatic hydrocarbon group, a divalent aromatic hydrocarbon group is preferred, an arylene group and an aralkylene group are more preferred, and an arylene group is further preferred. As the arylene group, an arylene group having 6 to 30 carbon atoms is preferred, an arylene group having 6 to 20 carbon atoms is more preferred, and an arylene group having 6 to 10 carbon atoms is further preferred. Examples of such an arylene group include phenylene, naphthylene, anthrylene, biphenylene, and the like. As the aralkylene group, an aralkylene group having 7 to 30 carbon atoms is preferred, an aralkylene group having 7 to 20 carbon atoms is more preferred, and an aralkylene group having 7 to 15 carbon atoms is further preferred. Among these, phenylene and naphthylene are preferred.
[0066] As the aliphatic hydrocarbon group, a divalent aliphatic hydrocarbon group is preferred, a divalent saturated aliphatic hydrocarbon group is more preferred, and an alkylene group and a cycloalkylene group are further preferred. As the alkylene group, an alkylene group having 1 to 10 carbon atoms is preferred, an alkylene group having 1 to 6 carbon atoms is more preferred, and an alkylene group having 1 to 3 carbon atoms is further preferred. Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a 1-methylmethylene group, a 1,1-dimethylmethylene group, a 1-methylethylene group, a 1,1-dimethylethylene group, a 1,2-dimethylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a pentylene group, a hexylene group, and the like are preferred, with a 1,1-dimethylmethylene group being preferred.
[0067] As the cycloalkylene group, a cycloalkylene group having 3 to 20 carbon atoms is preferred, a cycloalkylene group having 3 to 15 carbon atoms is more preferred, and a cycloalkylene group having 5 to 10 carbon atoms is further preferred. The cycloalkylene group may be a monocyclic structure or a polycyclic structure. Examples of the cycloalkylene group include cyclopropylene group, cyclobutylene group, cyclopentylene group, cyclohexylene group, cyclopentylene group, cycloheptylene group, and cycloalkylene groups represented by the following formulae (a) to (d). In formulae (a) to (d), "*" represents a bond.
[0068] [Chemical formula 4]
[0069]
[0070] As the group consisting of the combination thereof, a divalent group is preferred, and examples thereof include a group consisting of a combination of an aliphatic hydrocarbon group and an aromatic hydrocarbon group, a group consisting of a combination of an aromatic hydrocarbon group, an aliphatic hydrocarbon group and an aromatic hydrocarbon group, etc. As one embodiment of the group consisting of the combination thereof, a group consisting of a combination of an arylene group-an alkylene group-arylene group is preferred, and a group consisting of a combination of a phenylene group-1,1-dimethylmethylene group-phenylene group is preferred.
[0071] The component (B) has an allyl group. From the viewpoint of obtaining a cured product having excellent bending resistance, the number of allyl groups per molecule of the component (B) is preferably 1 or more, more preferably 2 or more, and preferably 10 or less, more preferably 8 or less, and even more preferably 5 or less.
[0072] The allyl group contained in the component (B) may be contained as a substituent of a terminal monovalent aromatic hydrocarbon group, or may be contained as a substituent of an aromatic hydrocarbon group or an aliphatic hydrocarbon group. When the allyl group is contained as a substituent of a terminal monovalent aromatic hydrocarbon group, it is more preferable that the allyl group is contained as a substituent of aromatic hydrocarbon groups at both terminals.
[0073] The aromatic ester skeleton, aromatic hydrocarbon group, aliphatic hydrocarbon group and unsaturated hydrocarbon group may have a substituent. Examples of the substituent include an unsaturated hydrocarbon group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, and a halogen atom. The substituent may be contained alone or in combination of two or more.
[0074] The substituent is not particularly limited, and examples thereof include a halogen atom, -OH, -OC 1-6 Alkyl, -N(C 1-10 Alkyl)2, C 1-20 Alkyl, C 2-30 Alkenyl, C 2-30 Alkynyl, C 6-10 Aryl, -NH2, -CN, -C(O)OC 1-10 Alkyl, -COOH, -C(O)H, -NO2, etc. Here, the term "C p-q ” (p and q are positive integers, and p<q) means that the number of carbon atoms in the organic group recorded immediately after the term is p~q. For example, “C 1-10 The expression "alkyl" means an alkyl group having 1 to 10 carbon atoms. These substituents may be bonded to each other to form a ring, and the ring structure may also include a spiro ring or a condensed ring.
[0075] The component (B) is preferably any one of a compound represented by the following general formula (B-1), a compound represented by the following general formula (B-2), and a compound represented by the following general formula (B-3).
[0076] [Chemical formula 5]
[0077]
[0078] In the general formula (B-1), Ar 11 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 12 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 13 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof. n represents an integer of 0-10.
[0079] [Chemical formula 6]
[0080]
[0081] In the general formula (B-2), Ar 21 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 22 Each independently represents a divalent hydrocarbon group which may have a substituent, Ar 23 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent. m represents an integer of 0-10.
[0082] [Chemical formula 7]
[0083]
[0084] In the general formula (B-3), Ar 21 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 31 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 13 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof. mb and nb each independently represent 0 or more.
[0085] In the general formula (B-1), Ar 11 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent. Examples of the monovalent aromatic hydrocarbon group include phenyl, furyl, pyrrolyl, thienyl, imidazolyl, pyrazolyl, Azolyl, iso A group obtained by removing one hydrogen atom from a monocyclic aromatic compound such as oxazolyl, thiazolyl, isothiazolyl, pyridyl, pyrimidyl, pyridazinyl, pyrazinyl, triazinyl, etc.; a group obtained by removing one hydrogen atom from a condensed-ring aromatic compound such as naphthyl, anthracenyl, phenanthrenyl, quinolyl, isoquinolyl, quinazolyl, phthalazinyl, pteridinyl, coumarinyl, indolyl, benzimidazolyl, benzofuranyl, acridinyl, etc. Among them, from the viewpoint of significantly obtaining the effect of the present invention, Ar 11 Phenyl is preferred.
[0086] Ar 11 It preferably has an allyl group as a substituent. 11 The monovalent aromatic hydrocarbon group represented may have a substituent other than the allyl group. The substituent is the same as the substituent that the aromatic ester skeleton may have.
[0087] In the general formula (B-1), Ar 12 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent. The divalent aromatic hydrocarbon group is as described above.
[0088] Ar 12The divalent aromatic hydrocarbon group represented may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.
[0089] In the general formula (B-1), Ar 13 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof, preferably a divalent group consisting of a combination thereof. The divalent aromatic hydrocarbon group and the divalent saturated aliphatic hydrocarbon group are as described above.
[0090] As the divalent group composed of their combination, a divalent group obtained by combining a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, and an oxygen atom is preferred, and a divalent group obtained by alternately combining a plurality of divalent aromatic hydrocarbon groups which may have a substituent and a plurality of divalent aliphatic hydrocarbon groups which may have a substituent is more preferred. The divalent group composed of their combination is the same as the group composed of their combination described above. As specific examples of the divalent group composed of their combination, the following divalent groups (B1) to (B15) can be cited. In the formula, b1 to b7 represent integers of 0 to 10, preferably integers of 0 to 5. a1 to a9 represent integers of 0 to 10, preferably integers of 0 to 6, and more preferably integers of 0 to 5. "*" represents a bond, and the wavy line represents a structure obtained by reacting an aromatic compound, an acyl halide of an aromatic compound, or an ester of an aromatic compound used in synthesizing component (B).
[0091] [Chemical formula 8]
[0092]
[0093] [Chemical formula 9]
[0094]
[0095] [Chemical formula 10]
[0096]
[0097] Ar 13 The divalent aromatic hydrocarbon group and the divalent aliphatic hydrocarbon group represented may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.
[0098] In general formula (B-1), n represents an integer of 0 to 10, preferably an integer of 0 to 5, and more preferably an integer of 0 to 3. When the compound represented by general formula (B-1) is an oligomer or a polymer, n represents the average value thereof.
[0099] The compound represented by the general formula (B-1) is preferably a compound represented by the general formula (B-4).
[0100] [Chemical formula 11]
[0101]
[0102] In the formula, Ar 31 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 32 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 33 Each independently represents a divalent group consisting of a combination of a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, and an oxygen atom. n1 represents an integer of 0-10.
[0103] Ar 31 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, and Ar in formula (B-1) 11 same.
[0104] Ar 32 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, and Ar in formula (B-1) 12 same.
[0105] Ar 33 Each independently represents a divalent group consisting of a combination of a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, and an oxygen atom, and Ar in formula (B-1) 13 The divalent groups formed by the combination of these represented are the same.
[0106] n1 represents an integer of 0 to 10, which is the same as n in formula (B-1).
[0107] In the general formula (B-2), Ar 21 represents a monovalent aromatic hydrocarbon group which may have a substituent. Examples of the monovalent aromatic hydrocarbon group include a phenyl group, a furyl group, a pyrrolyl group, a thienyl group, an imidazolyl group, a pyrazolyl group, Azolyl, iso A group obtained by removing one hydrogen atom from a monocyclic aromatic compound such as oxazolyl, thiazolyl, isothiazolyl, pyridyl, pyrimidyl, pyridazinyl, pyrazinyl, triazinyl, etc.; a group obtained by removing one hydrogen atom from a condensed-ring aromatic compound such as naphthyl, anthracenyl, phenanthrenyl, quinolyl, isoquinolyl, quinazolyl, phthalazinyl, pteridinyl, coumarinyl, indolyl, benzimidazolyl, benzofuranyl, acridinyl, etc. Among them, from the viewpoint of significantly obtaining the effect of the present invention, Ar 21 Phenyl and naphthyl are preferred. 21 The monovalent aromatic hydrocarbon group represented may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.
[0108] In the general formula (B-2), Ar 22 Each independently represents a divalent hydrocarbon group which may have a substituent. Examples of the divalent hydrocarbon group include a divalent aliphatic hydrocarbon group, a divalent aromatic hydrocarbon group, and a divalent group consisting of a combination thereof, preferably a divalent group consisting of a combination thereof. The divalent aliphatic hydrocarbon group is the same as Ar in the general formula (B-1). 13 The divalent aliphatic hydrocarbon group which may have a substituent is the same as Ar in the general formula (B-1). 12 same.
[0109] As a group consisting of their combination, it is the same as the group consisting of their combination described above. Specifically, a divalent group obtained by combining a divalent aromatic hydrocarbon group that may have a substituent and a divalent aliphatic hydrocarbon group that may have a substituent is preferred, and a divalent group obtained by combining in the order of a divalent aromatic hydrocarbon group that may have a substituent-a divalent aliphatic hydrocarbon group that may have a substituent-a divalent aromatic hydrocarbon group that may have a substituent is more preferred, and a divalent group having in the order of phenylene-1,1-dimethylmethylene-phenylene is further preferred. A divalent group having in the order of phenylene-1,1-dimethylmethylene-phenylene is represented by the above formula (B10).
[0110] Ar 22 It is preferred that the divalent aromatic hydrocarbon group has an allyl group as a substituent. 22 In the case of a group consisting of a combination of these, it is preferred that the divalent aromatic hydrocarbon group has an allyl group. 22 It may have a substituent other than the allyl group. The substituent is the same as the substituent that the aromatic ester skeleton may have.
[0111] In the general formula (B-2), Ar 23 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent. 23 and Ar in the general formula (B-1) 12 The same is true for the divalent aromatic hydrocarbon groups represented by Ar. 23 The divalent aromatic hydrocarbon group represented may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.
[0112] In general formula (B-2), m represents an integer of 0 to 10, preferably an integer of 1 to 5, more preferably an integer of 1 to 3, and particularly preferably 1. When the compound represented by general formula (B-2) is an oligomer or a polymer, n represents the average value thereof.
[0113] The compound represented by the general formula (B-2) is preferably a compound represented by the general formula (B-5).
[0114] [Chemical formula 12]
[0115]
[0116] In the formula, Ar 41 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 42 and Ar 44 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 43 Each independently represents a divalent aliphatic hydrocarbon group which may have a substituent. m1 represents an integer of 0-10.
[0117] Ar 41 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, and Ar in formula (B-2) 21 same.
[0118] Ar 42 and Ar 44 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, and Ar in formula (B-1) 12 same.
[0119] Ar 43 Each independently represents a divalent aliphatic hydrocarbon group which may have a substituent, and Ar in the general formula (B-1) 13 The divalent aliphatic hydrocarbon groups which may have a substituent are the same as those represented.
[0120] m1 represents an integer of 0 to 10, which is the same as m in formula (B-2).
[0121] In the general formula (B-3), Ar 21 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent. 21 With Ar in formula (B-2) 21 same.
[0122] In the general formula (B-3), Ar 31 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent. 31 With Ar in formula (B-1) 12 same.
[0123] In the general formula (B-3), Ar 13 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof. 13 With Ar in formula (B-1) 13 same.
[0124] As specific examples of component (B), the following compounds can be cited. In addition, as specific examples of component (B), the compounds described in paragraphs 0068 to 0071 described in International Publication No. 2018 / 235424 and paragraphs 0113 to 0115 described in International Publication No. 2018 / 235425 can be cited. Among them, component (B) is not limited to these specific examples. In the formula, s represents an integer greater than 0 or 1, and r represents an integer of 1 to 10. The average value of m2 is 1. n and m are greater than 0.
[0125] [Chemical formula 13]
[0126]
[0127] The component (B) may be one synthesized by a known method. The component (B) may be synthesized, for example, by the method described in International Publication No. 2018 / 235424 or International Publication No. 2018 / 235425.
[0128] The weight average molecular weight of the component (B) is preferably 150 or more, more preferably 200 or more, and further preferably 250 or more, and is preferably 5000 or less, more preferably 3000 or less, and further preferably 2000 or less, from the viewpoint of significantly obtaining the effects of the present invention. The weight average molecular weight of the component (B) is a weight average molecular weight of a polystyrene conversion value measured by gel permeation chromatography (GPC).
[0129] The allyl equivalent of the component (B) is preferably 50 g / eq. or more, more preferably 100 g / eq. or more, and further preferably 150 g / eq., and is preferably 2000 g / eq. or less, more preferably 1000 g / eq. or less, and further preferably 500 g / eq. or less, from the viewpoint of significantly obtaining the effects of the present invention. The allyl equivalent is the mass of the component (B) containing 1 equivalent of allyl groups.
[0130] Regarding the quantitative ratio of component (A) to component (B), the ratio of [the total number of epoxy groups of component (A)]:[the total number of allyl groups of component (B)] is preferably in the range of 1:0.01 to 1:10, more preferably 1:0.3 to 1:5, and further preferably 1:0.4 to 1:4. Here, the "total number of epoxy groups of the epoxy resin" refers to the value obtained by adding up all the values obtained by dividing the mass of the non-volatile components of component (A) present in the resin composition by the epoxy equivalent. In addition, the "total number of allyl groups of component (B)" refers to the value obtained by adding up all the values obtained by dividing the mass of the non-volatile components of component (B) present in the resin composition by the allyl equivalent. As component (B), the effect of the present invention can be significantly obtained by making the quantitative ratio with component (A) within the above range.
[0131] From the viewpoint of suppressing the bleed-out amount of the resin, the content of the component (B) is 1% by mass or more, preferably 2% by mass or more, more preferably 3% by mass or more, and is 25% by mass or less, preferably 20% by mass or less, and further preferably 16% by mass or less, when the non-volatile component in the resin composition is set to 100% by mass.
[0132] <(C) Organic fillers>
[0133] The resin composition contains (C) an organic filler as the (C) component. The (C) organic filler as the (C) component does not contain substances corresponding to the above-mentioned (A) to (B) components. By making the resin composition contain the (B) component, a cured product with excellent bending resistance can be obtained, but on the other hand, it is difficult to suppress the amount of resin exudation. However, in the present invention, since the combination contains the (B) component and the specified amount of the (C) component, a cured product with excellent bending resistance can be obtained, and the amount of resin exudation can be suppressed. It is believed that this is because, by making the resin composition contain the (C) component, thixotropy is imparted to the resin composition, and as a result, the fluidity of the resin composition can be appropriately controlled. The (C) component can be used alone or in combination of two or more.
[0134] From the viewpoint of obtaining a cured product having excellent bending resistance, when the non-volatile component in the resin composition is set to 100% by mass, the content of component (C) is 6% by mass or less, preferably 5% by mass or less, more preferably 4% by mass or less, and more preferably 3% by mass or less. From the viewpoint of suppressing the amount of resin exudation, the lower limit is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and further preferably 0.5% by mass or more or 0.8% by mass or more.
[0135] (C) component is present in the resin composition in the form of particles. As (C) component, for example, rubber particles, polyamide microparticles, silicone particles, core-shell particles, etc. can be mentioned. In the present invention, from the viewpoint of significantly obtaining the desired effect of the present invention, it is preferred to use any one of rubber particles and core-shell particles, and it is more preferred to use core-shell particles.
[0136] As the rubber component contained in the rubber particles, for example, there can be mentioned: olefin-based thermoplastic elastomers such as polybutadiene, polyisoprene, polychloroprene, ethylene-vinyl acetate copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-isobutylene copolymer, acrylonitrile-butadiene copolymer, isoprene-isobutylene copolymer, isobutylene-butadiene copolymer, ethylene-propylene-diene terpolymer, ethylene-propylene-butylene terpolymer; thermoplastic elastomers such as acrylic thermoplastic elastomers such as poly(meth)propyl acrylate, poly(meth)butyl acrylate, poly(meth)cyclohexyl acrylate, poly(meth)octyl acrylate, etc., preferably olefin-based thermoplastic elastomers, more preferably styrene-butadiene copolymer. In addition, silicone rubbers such as polyorganosiloxane rubber can be mixed in the rubber component. The glass transition temperature of the rubber component contained in the rubber particles is, for example, 0°C or less, preferably -10°C or less, more preferably -20°C or less, and further preferably -30°C or less.
[0137] As the rubber particles, commercially available products may be used, and examples thereof include "EXL2655" manufactured by Dow Chemical Japan Co., Ltd. and "AC3401N" and "AC3816N" manufactured by AICA Industries, Ltd.
[0138] Core-shell particles refer to granular organic fillers composed of core particles containing the rubber components listed above and more than one shell covering the core particles. Moreover, core-shell particles are preferably core-shell graft copolymer particles composed of core particles containing the rubber components listed above and shells, and the shells are obtained by graft copolymerization of monomer components copolymerizable with the rubber components contained in the core particles. The core-shell type mentioned here does not only refer to the core-shell type in which the core particles and the shells can be clearly distinguished, but also includes the core-shell type in which the boundary between the core particles and the shells is unclear, and the core particles may not be completely covered by the shells.
[0139] The rubber component is preferably contained in the core-shell type graft copolymer particles in an amount of 40% by mass or more, more preferably 50% by mass or more, and further preferably 60% by mass or more. The upper limit of the content of the rubber component in the core-shell type graft copolymer particles is not particularly limited, but from the viewpoint of sufficiently coating the core particles with the shell part, it is, for example, 95% by mass or less, preferably 90% by mass.
[0140] Examples of monomer components that form the shell portion of the core-shell graft copolymer particles include (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, and glycidyl (meth)acrylate; (meth)acrylic acid; N-substituted maleimides such as N-methylmaleimide and N-phenylmaleimide; maleimide; α,β-unsaturated carboxylic acids such as maleic acid and itaconic acid; aromatic vinyl compounds such as styrene, 4-vinyltoluene, and α-methylstyrene; (meth)acrylonitrile, etc., preferably (meth)acrylates, more preferably methyl (meth)acrylate.
[0141] Commercially available products of core-shell type graft copolymer particles include, for example, "CHT" manufactured by Samsung SDI; "B602" manufactured by Techno UMG; "Paraloid EXL2602", "Paraloid EXL2603", "Paraloid EXL2655", "Paraloid EXL2311", "Paraloid EXL2313", "Paraloid EXL2315", "Paraloid KM330", "Paraloid KM336P", and "Paraloid KCZ201" manufactured by Dow Chemical Japan; "METABLEN C-223A", "METABLEN E-901", "METABLEN S-2001", "METABLEN W-450A", and "METABLEN SRK-200" manufactured by Mitsubishi Rayon Co., Ltd.; and "KaneAce M-511", "KaneAce M-600", "KaneAce M-400", and "KaneAce M-580", "KaneAce MR-01", etc. These may be used alone or in combination of two or more.
[0142] The average particle size (average primary particle size) of the core-shell graft copolymer particles is not particularly limited, but is preferably 20 nm or more, more preferably 50 nm or more, further preferably 80 nm or more, and particularly preferably 100 nm or more, and is preferably 5,000 nm or less, more preferably 2,000 nm or less, further preferably 1,000 nm or less, and particularly preferably 500 nm or less. The average particle size (average primary particle size) of the core-shell graft copolymer particles can be measured using a zeta potential particle size distribution measuring device or the like.
[0143] When the non-volatile component in the resin composition is 100% by mass, the mass ratio of the component (B) to the component (C) (component (B) / component (C)) is preferably 1 or more, more preferably 3 or more, further preferably 5 or more or 8 or more, and is preferably 30 or less, more preferably 20 or less, further preferably 15 or less. By adjusting the contents of the component (B) and the component (C) so that the mass ratio of the component (B) to the component (C) is within the above range, a cured product having excellent bending resistance can be obtained, and the amount of resin bleed out can be suppressed.
[0144] When the non-volatile component in the resin composition is 100% by mass, when the contents of the components (A), (B) and (C) are A1, B1 and C1, respectively, A1 / (B1+C1) is preferably 0.1 or more, more preferably 0.3 or more, and further preferably 0.5 or more, and is preferably 5 or less, more preferably 3 or less, and further preferably 1 or less. By adjusting the contents of the components (A), (B) and (C) so that A1 / (B1+C1) is within the above range, a cured product having excellent bending resistance can be obtained, and the amount of resin bleed out can be suppressed.
[0145] <(D) Curing agent>
[0146] The resin composition may further contain (D) a curing agent as an optional component in addition to the above-mentioned components. The (D) curing agent as the (D) component does not contain substances corresponding to the above-mentioned (A) to (C) components. As the (D) curing agent, a compound having a function of reacting with the (A) component to cure the resin composition may be used, for example: a phenol curing agent, a naphthol curing agent, a carbodiimide curing agent, an active ester curing agent (excluding substances corresponding to the (B) component), a benzophenone curing agent, ... Among them, from the viewpoint of significantly obtaining the effect of the present invention, the (D) curing agent preferably includes at least one selected from the following: phenol curing agents, naphthol curing agents, carbodiimide curing agents, active ester curing agents (excluding those corresponding to the (B) component), benzoic acid curing agents, The oxazine-based curing agent and the cyanate-based curing agent more preferably contain at least one of a phenol-based curing agent and a carbodiimide-based curing agent, and more preferably contain a phenol-based curing agent. (D) The curing agent may be used alone or in combination of two or more.
[0147] As the phenolic curing agent and the naphthol curing agent, from the viewpoint of heat resistance and water resistance, a phenolic curing agent having a novolac structure or a naphthol curing agent having a novolac structure is preferred. In addition, from the viewpoint of adhesion with the conductor layer, a nitrogen-containing phenolic curing agent is preferred, and a phenolic curing agent containing a triazine skeleton is more preferred.
[0148] Specific examples of phenol-based curing agents and naphthol-based curing agents include: "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Chemicals; "NHN", "CBN", "GPH", and "KAYAHARD GPH103" manufactured by Nippon Kayaku Co., Ltd.; "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", "SN375", and "SN395" manufactured by Nippon Steel & Sumitomo Chemicals; and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA3018-50P", "EXB-9500", and "KA-1163" manufactured by DIC Corporation.
[0149] The carbodiimide-based curing agent is a compound having one or more carbodiimide groups (—N═C═N—) in one molecule, and the carbodiimide-based curing agent is preferably a compound having two or more carbodiimide groups in one molecule.
[0150] Specific examples of carbodiimide-based curing agents include: CARBODILITE V-03 (carbodiimide group equivalent: 216 g / eq.), V-05 (carbodiimide group equivalent: 262 g / eq.), V-07 (carbodiimide group equivalent: 200 g / eq.), and V-09 (carbodiimide group equivalent: 200 g / eq.) manufactured by Nisshinbo Chemical Co., Ltd.; and Stabaxol P (carbodiimide group equivalent: 302 g / eq.) manufactured by LANXESS.
[0151] As active ester curing agent, there is no particular restriction, and it is usually preferred to use compounds having ester groups with more than 2 high reactive activities in 1 molecule, such as esters of phenolic esters, thiophenolic esters, N-hydroxylamine esters, and heterocyclic hydroxy compounds. The active ester curing agent is preferably obtained by the condensation reaction of carboxylic acid compounds and / or thiocarboxylic acid compounds with hydroxy compounds and / or thiol compounds. In particular, from the viewpoint of improving heat resistance, the active ester curing agent preferably obtained by carboxylic acid compounds and hydroxy compounds, more preferably the active ester curing agent obtained by carboxylic acid compounds and phenolic compounds and / or naphthol compounds. As carboxylic acid compounds, for example, benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, pyromellitic acid, etc. can be mentioned. Examples of the phenol compound or naphthol compound include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the "dicyclopentadiene-type diphenol compound" refers to a diphenol compound obtained by condensing two molecules of phenol with one molecule of dicyclopentadiene.
[0152] Specifically, preferred are active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing acetylated products of phenol novolac, and active ester compounds containing benzoylated products of phenol novolac, among which active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. "Dicyclopentadiene-type diphenol structure" means a divalent structural unit composed of phenylene-dicyclopentenylene-phenylene.
[0153] As commercially available active ester curing agents, as active ester compounds containing a dicyclopentadiene-type diphenol structure, there are "EXB-9451", "EXB-9460", "EXB-9460S", "HPC-8000-65T", "HPC-8000H-65TM", "HPC-8000L-65TM" (manufactured by DIC Corporation); as active ester compounds containing a naphthalene structure, there are "EXB-9416-70BK", "EXB-8100L-65T", "EXB-8150-65T", "EXB-8150L-65T", "HPC-8150-60T", "HPC-8150-62T", "HP-B-8151-62T" (manufactured by DIC Corporation). As an active ester compound containing an acetylated product of phenol novolac, "DC808" (manufactured by Mitsubishi Chemical Corporation) can be cited; as an active ester compound containing a benzoylated product of phenol novolac, "YLH1026" (manufactured by Mitsubishi Chemical Corporation) can be cited; regarding an active ester curing agent which is an acetylated product of phenol novolac, "DC808" (manufactured by Mitsubishi Chemical Corporation) can be cited; regarding an active ester curing agent which is a benzoylated product of phenol novolac, "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) can be cited; as an active ester compound containing a styryl group, "PC1300-02-65MA" (manufactured by AIR WATER Co., Ltd.) and the like can be cited.
[0154] As benzo Specific examples of the oxazine-based curing agent include "HFB2006M" manufactured by Showa Polymer Co., Ltd. and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0155] Examples of the cyanate curing agent include difunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenylcyanate), 4,4'-ethylenediphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanatephenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanatephenyl-1-(methylethylene))benzene, bis(4-cyanatephenyl)sulfide and bis(4-cyanatephenyl)ether, polyfunctional cyanate resins derived from phenol novolac and cresol novolac, and prepolymers obtained by partially triazinizing these cyanate resins. Specific examples of cyanate curing agents include: "PT30" and "PT60" manufactured by Arxada (phenol novolac type multifunctional cyanate resins), "ULL-950S" (multifunctional cyanate resin), "BA230", "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate is triazine-treated to become trimers), etc.
[0156] Regarding the quantitative ratio of component (A) to component (D), the ratio of [the total number of epoxy groups of component (A)]:[the total number of active groups of component (D)] is preferably in the range of 1:0.01 to 1:10, more preferably 1:0.05 to 1:5, and further preferably 1:0.08 to 1:3. Here, the "total number of epoxy groups of the epoxy resin" refers to the value obtained by adding up all the values obtained by dividing the mass of the non-volatile components of component (A) present in the resin composition by the epoxy equivalent. In addition, the "total number of active groups of component (D)" refers to the value obtained by adding up all the values obtained by dividing the mass of the non-volatile components of component (D) present in the resin composition by the active group equivalent. As component (D), the effect of the present invention can be significantly obtained by making the quantitative ratio with component (A) within the above range.
[0157] The ratio of the amount of component (A) to the amount of component (B) and component (D) is preferably in the range of 1:0.01 to 1:10, more preferably 1:0.3 to 1:5, and even more preferably 1:0.4 to 1:4, in terms of the ratio of [the total number of epoxy groups of component (A)]:[the total number of active groups of component (B) and component (D)]. Here, the "total number of active groups of component (B) and component (D)" refers to the value obtained by adding all the values obtained by dividing the mass of the non-volatile components of component (B) and component (D) present in the resin composition by the active group equivalent. By making the ratio of the amount of component (A) to the amount of component (B) and component (D) within the above range, the effect of the present invention can be significantly obtained.
[0158] From the viewpoint of significantly obtaining the desired effect of the present invention, when the non-volatile component in the resin composition is set to 100% by mass, the content of component (D) is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and more preferably 1% by mass or more. The upper limit is preferably 25% by mass or less, more preferably 20% by mass or less, and more preferably 15% by mass or less.
[0159] <(E) Inorganic fillers>
[0160] The resin composition of the present invention may contain (E) an inorganic filler as an optional component. The (E) inorganic filler is contained in the resin composition in the form of particles.
[0161] As the material of (E) inorganic filler, an inorganic compound is used. As the material of (E) inorganic filler, for example, silica, aluminum oxide, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate, calcium zirconate, zirconium phosphate and zirconium tungstate phosphate, etc. Among these, silica is particularly suitable. As silica, for example, amorphous silica, fused silica, crystalline silica, synthetic silica, hollow silica, etc. can be mentioned. In addition, as silica, spherical silica is preferred. (E) The inorganic filler may be used alone or in combination of two or more at any ratio.
[0162] There is no particular limitation on the average particle size of the (E) inorganic filler material, preferably 10 μm or less, more preferably 5 μm or less, further preferably 2 μm or less, further preferably 1 μm or less, and particularly preferably 0.7 μm or less. There is no particular limitation on the lower limit of the average particle size of the (E) inorganic filler material, preferably 0.01 μm or more, more preferably 0.05 μm or more, further preferably 0.1 μm or more, and particularly preferably 0.2 μm or more. The average particle size of the (E) inorganic filler material can be measured by a laser diffraction / scattering method based on Mie scattering theory. Specifically, a particle size distribution of an inorganic filler material can be prepared on a volume basis by a laser diffraction scattering particle size distribution measuring device, and the median particle size can be measured as the average particle size. The sample can be measured by weighing 100 mg of an inorganic filler material and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. For the measurement sample, a laser diffraction particle size distribution measuring device is used, and the wavelength of the light source is set to blue and red, and the volume-based particle size distribution of the inorganic filler is measured in a flow cell mode, and the average particle size as the median particle size is calculated according to the obtained particle size distribution. As a laser diffraction particle size distribution measuring device, for example, "LA-960" manufactured by Horiba Manufacturing Co., Ltd. can be cited.
[0163] The specific surface area of the inorganic filler (E) is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 The upper limit of the specific surface area of the inorganic filler (E) is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 40m 2 The specific surface area of the inorganic filler can be obtained by adsorbing nitrogen gas on the sample surface using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech) according to the BET method and calculating the specific surface area by the BET multipoint method.
[0164] (E) The inorganic filling material may be a non-hollow inorganic filling material (preferably non-hollow silica) having a porosity of 0 volume %, or a hollow inorganic filling material (preferably hollow silica) having a porosity exceeding 0 volume %, or may include both. The porosity of the hollow inorganic filling material is preferably 70 volume % or less, more preferably 50 volume % or less, and particularly preferably 30 volume % or less. Regarding the lower limit of the porosity of the (E) inorganic filling material, for example, it may be set to exceed 0 volume %, 1 volume % or more, 5 volume % or more, 10 volume % or more, etc. The porosity P (volume %) of the inorganic filling material is defined as: the volume-based ratio of the total volume of one or more pores existing inside the particle to the volume of the entire particle based on the outer surface of the particle (total volume of pores / volume of the particle), for example, using the measured value D of the actual density of the inorganic filling material. M (g / cm 3 ) and the theoretical value D of the material density of the material forming the inorganic filler T (g / cm 3 ), calculated by the following formula (1).
[0165] [Mathematical formula 1]
[0166]
[0167] (E) The actual density of the inorganic filler can be measured, for example, using a true density measuring device. Examples of the true density measuring device include ULTRAPYCNOMETER 1000 manufactured by QUANTACHROME. For example, nitrogen can be used as the measuring gas.
[0168] (E) Inorganic fillers can be commercially available. Examples of commercially available inorganic fillers include: "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemicals; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka; "SILFIL NSS-3N", "SILFIL NSS-4N", and "SILFIL NSS-5N" manufactured by Tokuyama; "CellSpheres" and "MGH-005" manufactured by Pacific Cement; and "LPH-208" manufactured by Ube Exsymo.
[0169] From the viewpoint of improving moisture resistance and dispersibility, the (E) inorganic filler is preferably treated with a surface treatment agent. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, and titanate coupling agents. In addition, the surface treatment agent may be used alone or in any combination of two or more.
[0170] Commercially available products of the surface treatment agent include, for example, “KBM403” (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM803” (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBE903” (3-aminopropyltriethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM573” (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “SZ-31” (hexamethyldisilazane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM103” (phenyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., “KBM-4803” (long-chain epoxy-type silane coupling agent) manufactured by Shin-Etsu Chemical Co., Ltd., and “KBM-7103” (3,3,3-trifluoropropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd.
[0171] The degree of surface treatment by the surface treatment agent is preferably controlled within a specified range from the viewpoint of improving the dispersibility of the inorganic filler. Specifically, 100% by mass of the inorganic filler is preferably surface treated with 0.2% by mass to 5% by mass of the surface treatment agent, more preferably with 0.2% by mass to 3% by mass, and further preferably with 0.3% by mass to 2% by mass.
[0172] The degree of surface treatment by the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is preferably 0.02 mg / m 2 More preferably 0.1 mg / m 2 More preferably 0.2 mg / m 2 On the other hand, from the viewpoint of preventing the increase of the melt viscosity of the resin composition or the melt viscosity in the form of a sheet, 1.0 mg / m 2 Below, more preferably 0.8 mg / m 2 Below, more preferably 0.5 mg / m 2 the following.
[0173] The amount of carbon per unit surface area of the (E) inorganic filler can be measured after washing the surface-treated inorganic filler with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler surface-treated with a surface treatment agent, and ultrasonic washing is performed for 5 minutes at 25°C. After removing the supernatant and drying the solid components, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. As a carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., etc. can be used.
[0174] From the viewpoint of significantly obtaining the effects of the present invention, when the non-volatile component in the resin composition is set to 100 mass %, the content of the (E) inorganic filler is preferably 55 mass % or more, more preferably 60 mass % or more, further preferably 65 mass % or more or 70 mass % or more, and is preferably 85 mass % or less, more preferably 80 mass % or less, and further preferably 75 mass % or less.
[0175] <(F) Curing accelerator>
[0176] The resin composition may further contain a curing accelerator as a component (F) as an optional component in addition to the above-mentioned components. The (F) curing accelerator as the component (F) does not contain substances corresponding to the above-mentioned components (A) to (D). By containing the (F) component, the curing of the (A) component can be further accelerated. The (F) component can be used alone or in combination of two or more.
[0177] As the component (F), for example, phosphorus curing accelerators, urea curing accelerators, guanidine curing accelerators, imidazole curing accelerators, metal curing accelerators, amine curing accelerators, etc. Among them, a curing accelerator selected from amine curing accelerators and metal curing accelerators is preferred, and an amine curing accelerator is particularly preferred.
[0178] Examples of the phosphorus-based curing accelerator include tetrabutylphosphonium bromide, tetrabutylphosphonium chloride, tetrabutylphosphonium acetate, tetrabutylphosphonium decanoate, tetrabutylphosphonium laurate, bis(tetrabutylphosphonium)pyromellitic acid salt, tetrabutylphosphonium hexahydrophthalate, and tetrabutylphosphonium bis(tetrabutylphosphonium) pyromellitic acid salt. aliphatic phosphonium salts such as tetrabutylphosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate and di-tert-butyldimethylphosphonium tetraphenylborate; methyltriphenylphosphonium bromide, ethyltriphenylphosphonium bromide, propyltriphenylphosphonium bromide, Aromatic phosphonium salts such as butyltriphenylphosphonium, benzyltriphenylphosphonium chloride, tetraphenylphosphonium bromide, p-tolyltriphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone addition products such as triphenylphosphine-p-benzoquinone addition products reactants; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine; dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tri(4-ethylphenyl)phosphine, tri(4-propylphenyl)phosphine, tri(4-isopropylphenyl)phosphine, tri(4-butylphenyl)phosphine, tri(4-tert-butylphenyl)phosphine, tri(2,4-dimethylphenyl)phosphine, tri(2,5-dimethylphenyl)phosphine phenyl)phosphine, tri(2,6-dimethylphenyl)phosphine, tri(3,5-dimethylphenyl)phosphine, tri(2,4,6-trimethylphenyl)phosphine, tri(2,6-dimethyl-4-ethoxyphenyl)phosphine, tri(2-methoxyphenyl)phosphine, tri(4-methoxyphenyl)phosphine, tri(4-ethoxyphenyl)phosphine, tri(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, 2,2'-bis(diphenylphosphino)diphenyl ether and the like.
[0179] Examples of the urea curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, 3-(3,4-dimethylphenyl)-1, Aromatic dimethyl urea such as 1-dimethyl urea, 3-(4-isopropylphenyl)-1,1-dimethyl urea, 3-(4-methoxyphenyl)-1,1-dimethyl urea, 3-(4-nitrophenyl)-1,1-dimethyl urea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethyl urea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethyl urea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethyl urea, N,N-(1,4-phenylene)bis(N',N'-dimethyl urea), N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethyl urea)[toluene bis(dimethyl urea)].
[0180] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanidine, 1-ethylbiguanidine, 1-n-butylbiguanidine, 1-n-octadecylbiguanidine, 1,1-dimethylbiguanidine, 1,1-diethylbiguanidine, 1-cyclohexylbiguanidine, 1-allylbiguanidine, 1-phenylbiguanidine, and 1-(o-tolyl)biguanidine.
[0181] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1' imidazole compounds such as 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline, and adducts of imidazole compounds with epoxy resins.
[0182] As the imidazole-based curing accelerator, a commercially available product may be used, and examples thereof include "1B2PZ", "2MZA-PW", "2PHZ-PW", and "C11Z-A" manufactured by Shikoku Chemical Industries, Ltd.; and "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0183] As metal curing accelerators, for example, organic metal complexes or organic metal salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin can be cited. Specific examples of organic metal complexes include organic cobalt complexes such as cobalt acetylacetonate (II) and cobalt acetylacetonate (III), organic copper complexes such as copper acetylacetonate (II), organic zinc complexes such as zinc acetylacetonate (II), organic iron complexes such as iron acetylacetonate (III), organic nickel complexes such as nickel acetylacetonate (II), and organic manganese complexes such as manganese acetylacetonate (II). As organic metal salts, for example, zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, zinc stearate, and the like can be cited.
[0184] Examples of the amine-based curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.
[0185] As the amine-based curing accelerator, a commercially available product may be used, and examples thereof include "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd. and the like.
[0186] From the viewpoint of significantly obtaining the desired effect of the present invention, when the non-volatile component in the resin composition is set to 100% by mass, the content of the component (F) is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and further preferably 0.1% by mass or more, and is preferably 1% by mass or less, more preferably 0.8% by mass or less, and further preferably 0.5% by mass or less.
[0187] <(G) Other additives>
[0188] In addition to the above-mentioned components, the resin composition may further contain other additives as optional components. Examples of (G) other additives include: free radical polymerizable compounds (excluding substances corresponding to component (C)); thermoplastic resins; elastomers; polymerization initiators; organic metal compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone leveling agents and acrylic polymer leveling agents; thickeners such as Benton and montmorillonite; defoamers such as silicone defoamers, acrylic defoamers, fluorine defoamers, and vinyl resin defoamers; ultraviolet absorbers such as benzotriazole ultraviolet absorbers; adhesion enhancers such as urea silane; adhesion enhancers such as triazole adhesion enhancers, tetrazole adhesion enhancers, and triazine adhesion enhancers imparting agent; antioxidants such as hindered phenol antioxidants; fluorescent whitening agents such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (such as phosphate compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (such as melamine sulfate), halogen-based flame retardants, inorganic flame retardants (such as antimony trioxide); dispersants such as phosphate-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers; photopolymerization initiation aids such as tertiary amines; photosensitizers such as pyrazolines, anthracenes, coumarins, xanthones, and thioxanthones. (G) Other additives can be used alone or in combination of two or more.
[0189] <(H)Solvent>
[0190] The resin composition may contain, in addition to the above-mentioned non-volatile components, an optional solvent as a volatile component. As the (H) solvent, a known solvent may be used as appropriate, and its type is not particularly limited, and an organic solvent is preferred. Examples of the (H) solvent include: ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; tetrahydropyran, tetrahydrofuran, 1,4-dihydropyran, and 1,4-dihydrofuran. Ether solvents such as alkane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, anisole, etc.; alcohol solvents such as methanol, ethanol, propanol, butanol, ethylene glycol, etc.; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, carbitol acetate (ethyl diglycol Ether ester solvents such as acetate, γ-butyrolactone, and methyl methoxypropionate; ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. (H) Solvents may be used alone or in combination of two or more in any ratio.
[0191] Regarding the resin composition, from the viewpoint of significantly obtaining the effect of the present invention, relative to 100% by mass of all the components of the resin composition, it is preferred to include 0.5% by mass or more and 3% by mass or less of the (H) solvent. Specifically, relative to 100% by mass of all the components of the resin composition, it is preferred to include: preferably 3% by mass or less, more preferably 2% by mass or less, further preferably 1.5% by mass or less and preferably 0.5% by mass or more, more preferably 0.8% by mass or more, further preferably 1% by mass or more of the (H) solvent.
[0192] The method for preparing the resin composition of the present invention is not particularly limited, and examples thereof include a method in which a solvent or the like is added as necessary, and the blending components are mixed and dispersed using a rotary mixer or the like.
[0193] <Physical properties and uses of resin composition>
[0194] The resin composition comprises component (A), component (B) and a predetermined amount of component (C). Thus, a cured product having excellent bending resistance can be obtained, while the amount of resin exudation can be suppressed. Furthermore, a cured product having a low dielectric loss tangent and a low dielectric constant can be obtained.
[0195] Since the resin composition combination includes (B) component and a specified amount of (C) component, it shows the characteristic of suppressing the amount of resin exudation. Specifically, after laminating the resin composition layer of the resin sheet on the glass cloth substrate epoxy resin double-sided copper-clad laminate with a copper foil thickness of 18 μm, it is thermally cured at 130°C for 30 minutes and then at 170°C for 30 minutes to form an insulating layer. The resin composition flows during lamination, and the amount of the resin composition exuded from the support is measured as the distance from the end of the support to the end of the exuded resin. The distance at this time is set to the resin exudation amount, and the resin exudation amount is preferably less than 5 mm. There is no particular restriction on the lower limit, and it can be set to more than 0 mm, more than 0.01 mm, etc. The amount of resin exudation can be measured according to the method described in the embodiments described later.
[0196] Since the resin composition combination includes component (B) and a specified amount of component (C), the cured product of the resin composition being heat cured at 190°C for 90 minutes exhibits excellent bending resistance. Therefore, the cured product provides an insulating layer with excellent bending resistance. Regarding bending resistance, the MIT test apparatus is used under the measurement conditions of a load of 2.5N, a bending angle of 90 degrees, a bending radius of 1.0mm, and a bending speed of 175 times / minute. The number of bends of the cured product under the above conditions is preferably more than 300 times, more preferably more than 380 times, and further preferably more than 400 times and more than 450 times. There is no particular restriction on the upper limit, and it can be set to less than 10,000 times, etc. Bending resistance can be measured according to the method described in the embodiments described later.
[0197] The cured product obtained by heat curing the resin composition at 190° C. for 90 minutes generally exhibits the property of low dielectric loss tangent. Therefore, the cured product provides an insulating layer with low dielectric loss tangent. The dielectric loss tangent is preferably less than 0.005, more preferably less than 0.004, and further preferably less than 0.003. The lower limit of the dielectric loss tangent can be set to 0.0001 or more. The dielectric loss tangent can be measured according to the method described in the embodiments described below.
[0198] The cured product of the resin composition subjected to heat curing at 190° C. for 90 minutes generally exhibits the property of low dielectric constant. Therefore, the cured product provides an insulating layer with low dielectric constant. The dielectric constant is preferably less than 4, more preferably less than 3.8, and further preferably less than 3.5. The lower limit of the dielectric constant can be set to 0.001 or more. The dielectric constant can be measured according to the method described in the embodiments described below.
[0199] The resin composition of the present invention can obtain a cured product with excellent bending resistance, and can suppress the amount of resin exudation. In addition, a cured product with a low dielectric loss tangent and a low dielectric constant can be obtained. Therefore, the resin composition of the present invention can be suitably used as a resin composition for insulating purposes. Specifically, it can be suitably used as a resin composition for forming an insulating layer, which is used to form a conductor layer (including a rewiring layer) formed on the insulating layer (resin composition for forming an insulating layer for forming a conductor layer)
[0200] In addition, in the multilayer printed wiring board described later, it can be suitably used as: a resin composition for forming an insulating layer of a multilayer printed wiring board (resin composition for forming an insulating layer of a multilayer printed wiring board), and a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for forming an interlayer insulating layer of a printed wiring board).
[0201] In addition, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition of the present invention can also be suitably used as a resin composition for forming a rewiring forming layer as an insulating layer (resin composition for forming a rewiring forming layer) and a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When manufacturing a semiconductor chip package, a rewiring layer can be further formed on the sealing layer.
[0202] Step (1), laminating a temporary fixing film on a substrate;
[0203] Step (2), temporarily fixing the semiconductor chip on a temporary fixing film;
[0204] Step (3), forming a sealing layer on the semiconductor chip;
[0205] Step (4), peeling the substrate and the temporary fixing film from the semiconductor chip;
[0206] Step (5), forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the substrate and the temporary fixing film have been peeled off; and
[0207] Step (6) is to form a rewiring layer as a conductor layer on the rewiring formation layer.
[0208] [Resin sheet]
[0209] The resin sheet of the present invention comprises a support and a resin composition layer formed from the resin composition of the present invention and provided on the support.
[0210] The thickness of the resin composition layer is preferably 100 μm or less, more preferably 80 μm or less, and further preferably 50 μm or less, from the viewpoint of thinning the printed wiring board and providing a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, and can usually be set to 5 μm or more.
[0211] Examples of the support include films made of plastic materials, metal foils, and release papers, and films made of plastic materials and metal foils are preferred.
[0212] When a film made of a plastic material is used as a support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes referred to as "PET") and polyethylene naphthalate (hereinafter sometimes referred to as "PEN"), polycarbonate (hereinafter sometimes referred to as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among them, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0213] When a metal foil is used as a support, examples of the metal foil include copper foil and aluminum foil, preferably copper foil. The copper foil may be a foil made of a single metal such as copper or an alloy of copper and other metals (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.).
[0214] The surface of the support to be in contact with the resin composition layer may be subjected to matte treatment, corona treatment, or antistatic treatment.
[0215] In addition, as the support, a support with a release layer having a release layer on the surface bonded to the resin composition layer can be used. As a release agent for the release layer in the support with a release layer, for example, there can be mentioned: one or more release agents selected from alkyd resins, polyolefin resins, urethane resins and silicone resins. The support with a release layer can use commercially available products, for example, there can be mentioned: "SK-1", "AL-5", "AL-7" manufactured by LINTEC, which is a PET film having a release layer with an alkyd resin-based release agent as a main component; "Lumirror T60" manufactured by Toray Industries, Inc.; "Purex" manufactured by Teijin Co., Ltd.; "Unipeel" manufactured by UNITIKA Co., Ltd., etc.
[0216] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, the thickness of the entire support with a release layer is preferably in the above range.
[0217] In one embodiment, the resin sheet may further include other layers as needed. As the other layers, for example, a protective film selected according to the support and arranged on the surface of the resin composition layer that is not bonded to the support (i.e., the surface on the opposite side of the support) can be cited. The thickness of the protective film is not particularly limited, for example, 1 μm to 40 μm. By laminating the protective film, dust can be prevented from adhering to the surface of the resin composition layer or causing damage to the surface of the resin composition layer.
[0218] The resin sheet can be produced, for example, by preparing a resin varnish obtained by dissolving the resin composition in a solvent, applying the resin varnish on a support using a die coater or the like, and further drying to form a resin composition layer. The solvent is as described above.
[0219] Drying can be carried out by known methods such as heating and blowing hot air. The drying conditions are not particularly limited, and the drying is carried out in a manner such that the content of the solvent in the resin composition layer is 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the solvent in the resin varnish, for example, in the case of using a resin varnish containing 30% to 60% by mass of a solvent, a resin composition layer can be formed by drying at 50° C. to 150° C. for 3 minutes to 10 minutes.
[0220] The resin sheet can be stored by winding it into a roll. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0221] [Printed wiring board]
[0222] The printed wiring board of the present invention includes an insulating layer formed of a cured product of the resin composition of the present invention.
[0223] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet and a method including the following steps (I) and (II).
[0224] Step (I), laminating on the inner substrate in such a manner that the resin composition layer of the resin sheet is bonded to the inner substrate;
[0225] In step (II), the resin composition layer is thermally cured to form an insulating layer.
[0226] The "inner layer substrate" used in step (I) refers to a member that becomes a substrate of a printed wiring board, and examples thereof include: a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, and the like. In addition, the substrate may have a conductor layer on one or both sides thereof, and the conductor layer may also be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of a substrate is sometimes referred to as an "inner layer circuit substrate". In addition, when manufacturing a printed wiring board, an intermediate product to be further formed with an insulating layer and / or a conductor layer is also included in the "inner layer substrate" mentioned in the present invention. In the case where the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components can be used.
[0227] The lamination of the inner substrate and the resin sheet can be performed, for example, by heat-pressing the resin sheet to the inner substrate from the support body side. As a component for heat-pressing the resin sheet to the inner substrate (hereinafter, also referred to as a "heat-pressing component"), for example, a heated metal plate (SUS end plate, etc.) or a metal roller (SUS roller) can be cited. It should be noted that it is preferred not to press the heat-pressing component directly onto the resin sheet, but to press it through an elastic material such as heat-resistant rubber, so that the resin sheet can fully follow the surface unevenness of the inner substrate.
[0228] The lamination of the inner substrate and the resin sheet can be implemented by vacuum lamination. In the vacuum lamination method, the heating and pressing temperature is preferably 60°C to 160°C, more preferably 80°C to 140°C, the heating and pressing pressure is preferably 0.098MPa to 1.77MPa, more preferably 0.29MPa to 1.47MPa, and the heating and pressing time is preferably 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. Lamination is preferably implemented under reduced pressure conditions of 26.7hPa or less.
[0229] Lamination can be performed using a commercially available vacuum laminator. Examples of the commercially available vacuum laminator include a vacuum pressure laminator manufactured by Meiki Manufacturing Co., Ltd., a vacuum applicator manufactured by Nikko-Materials Co., Ltd., and a batch vacuum pressure laminator.
[0230] After lamination, the laminated resin sheet can also be smoothed by pressing the heated pressing member at normal pressure (atmospheric pressure), for example, from the support side. The pressing conditions for the smoothing treatment can be set to the same conditions as the heated pressing conditions for the above-mentioned lamination. The smoothing treatment can be performed using a commercially available laminator. It should be noted that the lamination and smoothing treatment can be performed continuously using the above-mentioned commercially available vacuum laminator.
[0231] The support may be removed between step (I) and step (II), or may be removed after step (II).
[0232] In step (II), the resin composition layer is thermally cured to form an insulating layer. The thermal curing conditions of the resin composition layer are not particularly limited, and conditions generally used when forming an insulating layer of a printed wiring board can be used.
[0233] For example, the heat curing conditions of the resin composition layer may vary depending on the type of the resin composition, and the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and further preferably 170° C. to 210° C. The curing time may be preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and further preferably 15 minutes to 100 minutes.
[0234] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature of 50° C. or higher and lower than 120° C. (preferably 60° C. or higher and 115° C. or lower, more preferably 70° C. or higher and 110° C. or lower) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes).
[0235] When manufacturing a printed wiring board, the step of (III) opening a hole in the insulating layer, the step of (IV) roughening the insulating layer, and the step of (V) forming a conductor layer can be further implemented. These steps (III) to (V) can be implemented according to various methods known to those skilled in the art for manufacturing a printed wiring board. It should be noted that, when the support body is removed after step (II), the removal of the support body can be implemented between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, as necessary, the formation of the insulating layer and the conductor layer of steps (II) to (V) can be repeatedly implemented to form a multilayer wiring board.
[0236] Step (III) is a step of drilling holes in the insulating layer, thereby forming holes such as via holes and through holes in the insulating layer. Step (III) can be performed using, for example, a drill, laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The size or shape of the hole can be appropriately determined according to the design of the printed wiring board.
[0237] Step (IV) is a step of roughening the insulating layer. Usually, in this step (IV), contamination is also removed. There are no particular restrictions on the steps and conditions of the roughening treatment, and the known steps and conditions commonly used when forming the insulating layer of the printed wiring board can be adopted. For example, swelling treatment based on a swelling solution, roughening treatment based on an oxidant, and neutralization treatment based on a neutralizing solution can be sequentially implemented to roughen the insulating layer. The swelling solution used for the roughening treatment is not particularly limited, and examples include: alkaline solutions, surfactant solutions, etc., preferably alkaline solutions, and more preferably sodium hydroxide solutions and potassium hydroxide solutions. As commercially available swelling solutions, for example, "Swelling Dip Securiganth P", "Swelling Dip Securiganth SBU", "Swelling DipSecurigant P" manufactured by Atotech Japan Co., Ltd. are mentioned. There is no particular restriction on the swelling treatment based on the swelling solution, for example, it can be carried out by immersing the insulating layer in a swelling solution at 30°C to 90°C for 1 minute to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferred to immerse the insulating layer in a swelling solution at 40°C to 80°C for 5 minutes to 15 minutes. As the oxidizing agent used for the roughening treatment, there is no particular limitation, and examples thereof include: an alkaline permanganate solution obtained by dissolving potassium permanganate or sodium permanganate in an aqueous solution of sodium hydroxide. The roughening treatment based on an oxidizing agent such as an alkaline permanganate solution is preferably carried out by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. In addition, the concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. As commercially available oxidizing agents, for example, alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securiganth P" manufactured by Atotech Japan can be cited. In addition, as a neutralizing solution used for the roughening treatment, an acidic aqueous solution is preferred, and as a commercially available product, for example, "Reduction Solution Securiganth P" manufactured by Atotech Japan can be cited. The treatment with the neutralizing solution can be performed by immersing the treated surface subjected to the roughening treatment with the oxidizing agent in the neutralizing solution at 30° C. to 80° C. for 1 to 30 minutes. In view of operability, etc., it is preferable to immerse the object subjected to the roughening treatment with the oxidizing agent in the neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes.
[0238] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after the roughening treatment is preferably 300 nm or less, more preferably 250 nm or less, and further preferably 200 nm or less. The lower limit is not particularly limited, but is preferably 30 nm or more, more preferably 40 nm or more, and further preferably 50 nm or more. The arithmetic mean roughness (Ra) of the insulating layer surface can be measured using a non-contact surface roughness meter.
[0239] Step (V) is a step of forming a conductor layer, and a conductor layer is formed on the insulating layer. There is no particular limitation on the conductor material used for the conductor layer. In a suitable embodiment, the conductor layer comprises one or more metals selected from gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer. As the alloy layer, for example, a layer formed by an alloy of two or more metals selected from the above (for example, nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy) can be cited. Among them, from the viewpoints of versatility, cost, ease of patterning, etc. of the formation of the conductor layer, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy, copper-nickel alloy, or copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy is more preferred, and a single metal layer of copper is further preferred.
[0240] The conductor layer may be a single-layer structure, or a multi-layer structure in which two or more single metal layers or alloy layers composed of different types of metals or alloys are stacked. In the case where the conductor layer is a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0241] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is usually 3 μm to 35 μm, preferably 5 μm to 30 μm.
[0242] In one embodiment, the conductor layer can be formed by electroplating. For example, the surface of the insulating layer can be electroplated using a conventionally known technique such as a semi-additive method or a full-additive method to form a conductor layer having a desired wiring pattern. From the perspective of manufacturing simplicity, it is preferably formed using a semi-additive method. An example of forming a conductor layer using a semi-additive method is shown below.
[0243] First, a plating seed layer is formed on the surface of the insulating layer by electroless plating. Then, a mask pattern is formed on the formed plating seed layer to expose a portion of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, the unnecessary plating seed layer is removed by etching or the like, and a conductor layer having a desired wiring pattern can be formed.
[0244] [Semiconductor devices]
[0245] The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be produced using the printed wiring board of the present invention.
[0246] Examples of the semiconductor device include various semiconductor devices provided for electrical products (eg, computers, mobile phones, digital cameras, and televisions) and vehicles (eg, motorcycles, cars, trains, ships, and airplanes).
[0247] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. "Conductive portion" refers to "a portion of a printed wiring board that transmits an electrical signal", and the position may be a surface or an embedded portion, either of which is acceptable. In addition, the semiconductor chip is not particularly limited as long as it is a circuit element made of semiconductor.
[0248] Regarding the method for mounting a semiconductor chip when manufacturing a semiconductor device, there is no particular limitation as long as the semiconductor chip can function effectively, and specifically, there can be cited: a wire bonding mounting method, a flip chip mounting method, a mounting method based on a bumpless build-up layer (BBUL), a mounting method based on an anisotropic conductive film (ACF), a mounting method based on a non-conductive film (NCF), etc. Here, the "mounting method based on a bumpless build-up layer (BBUL)" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess of a printed wiring board to connect the semiconductor chip to the wiring on the printed wiring board".
[0249] Example
[0250] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited to these examples. It should be noted that in the following description, "parts" and "%" refer to "parts by mass" and "mass %" respectively, unless otherwise specified.
[0251] <Synthesis Example 1: Synthesis of Active Ester Resin A>
[0252] In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 165 g of a polyaddition reaction resin of dicyclopentadiene and phenol (hydroxyl equivalent: 165 g / eq., softening point 85°C), 134 g (1.0 mol) of o-allylphenol, and 1200 g of toluene were placed, and the system was replaced with nitrogen under reduced pressure. Next, 203 g (1.0 mol) of isophthaloyl chloride was placed, and the system was replaced with nitrogen under reduced pressure. 0.6 g of tetrabutylammonium bromide was added, and the system was controlled at below 60°C while nitrogen purging was performed. 412 g of a 20% aqueous sodium hydroxide solution was added dropwise over 3 hours, and after the addition was completed, the mixture was stirred for 1.0 hour. After the reaction was completed, the water layer was removed by standing and separating the liquids. Water was further added to the obtained toluene layer, and the mixture was stirred for 15 minutes. The water layer was removed by standing and separating the liquids. This operation was repeated until the pH of the water layer reached 7. Then, the non-volatile content was adjusted to 70% by mass by heat drying, thereby obtaining an active ester resin A represented by the following formula.
[0253] [Chemical formula 14]
[0254]
[0255] In the above chemical formula, s is independently an integer of 0 or 1 or more, and the average value of r calculated according to the feed ratio is 1. In addition, the dotted line in the chemical formula is a structure obtained by reacting isophthaloyl chloride, a polyaddition reaction resin of phenol and / or o-allylphenol. The ester equivalent of the obtained active ester resin A was calculated according to the feed ratio, and the result was 214 g / eq.
[0256] <Synthesis Example 2: Synthesis of Active Ester Resin B>
[0257] In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 320 g of diallyl bisphenol A and 1500 g of toluene are placed, and the contents are dissolved while the flask is replaced with nitrogen under reduced pressure. Next, 240 g of benzoyl chloride and 102 g of isophthaloyl chloride are placed, and the contents are dissolved while the flask is replaced with nitrogen under reduced pressure. Further, 0.8 g of tetrabutylammonium bromide is added to dissolve it. While nitrogen purging, the system is controlled below 60°C, and 412 g of a 20% aqueous sodium hydroxide solution is added dropwise over 3 hours. After the addition is completed, stirring is continued for 1.0 hour under the same conditions. After the reaction is completed, the reaction mixture is allowed to stand and separate, and the water layer is removed. Water is added to the remaining toluene phase, stirred and mixed for about 15 minutes, and the water layer is removed after standing. Repeat this operation until the pH of the water layer reaches 7. Then, the non-volatile content was adjusted to 70% by mass by heat drying, thereby obtaining an active ester resin B represented by the following formula.
[0258] [Chemical formula 15]
[0259]
[0260] In the above formula, the average value of m2 calculated from the feed ratio is 1. The ester group equivalent of the obtained active ester resin B was calculated from the feed ratio and the result was 245 g / eq.
[0261] <Example 1: Preparation of resin composition 1>
[0262] 5 parts of naphthalene epoxy resin ("HP-4032-SS" manufactured by DIC Corporation, epoxy equivalent 144 g / eq.), 10 parts of naphthalene aralkyl epoxy resin ("ESN-475V" manufactured by Nippon Steel Chemicals Co., Ltd., epoxy equivalent 330 g / eq.), 5 parts of biphenyl aralkyl epoxy resin ("NC-3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 269 g / eq.), 30 parts of active ester resin A synthesized in Synthesis Example 1, 2 parts of rubber particles (Dow Chemical Japan Co., Ltd., "EXL2655"), 5 parts of other curing agents (phenol curing agent, DIC Corporation, "LA-3018-50P", 1-methoxy-2-propanol solution with a hydroxyl equivalent of 151 g / eq. and a non-volatile content of 50% by mass), 130 parts of inorganic fillers (spherical silica surface-treated with an amine-based alkoxysilane compound (Shin-Etsu Chemical Co., Ltd., "KBM573"), Admatechs Corporation, "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m 2 / g), 0.3 parts of a curing accelerator (manufactured by Shikoku Chemical Industry Co., Ltd., "1B2PZ"), 20 parts of MEK, and 10 parts of cyclohexanone were uniformly dispersed using a high-speed rotary mixer to obtain a resin composition 1.
[0263] <Example 2: Preparation of resin composition 2>
[0264] In Example 1, 30 parts of the active ester resin A synthesized in Synthesis Example 1 was replaced with 30 parts of the active ester resin B synthesized in Synthesis Example 2.
[0265] Resin composition 2 was obtained in the same manner as in Example 1 except for the above matters.
[0266] <Example 3: Preparation of resin composition 3>
[0267] In Example 1, 2 parts of rubber particles ("EXL2655" manufactured by Dow Chemical Japan Ltd.) were replaced with 2 parts of rubber particles ("AC3816N" manufactured by AICA Industries Ltd.).
[0268] Resin composition 3 was obtained in the same manner as in Example 1 except for the above matters.
[0269] <Example 4: Preparation of resin composition 4>
[0270] In Example 1, 4 parts of a carbodiimide curing agent ("V-03" manufactured by Nisshinbo Chemical Co., Ltd., active group equivalent of about 216 / eq., toluene solution containing 50% of nonvolatile matter) were used.
[0271] Resin composition 4 was obtained in the same manner as in Example 1 except for the above matters.
[0272] <Example 5: Preparation of resin composition 5>
[0273] In Example 4, 30 parts of the active ester resin A synthesized in Synthesis Example 1 was replaced with 30 parts of the active ester resin B synthesized in Synthesis Example 2.
[0274] Resin composition 5 was obtained in the same manner as in Example 4 except for the above matters.
[0275] <Example 6: Preparation of Resin Composition 6>
[0276] In Example 1, the amount of rubber particles ("EXL2655" manufactured by Dow Chemical Japan Ltd.) was changed from 2 parts to 6 parts.
[0277] Except for the above matters, a resin composition 6 was obtained in the same manner as in Example 1.
[0278] <Example 7: Preparation of resin composition 7>
[0279] In Example 1,
[0280] 1) An inorganic filler (spherical silica (SO-C2 manufactured by Admatechs, average particle size 0.5 μm, specific surface area 5.8 m2) surface-treated with an amine alkoxysilane compound (KBM573 manufactured by Shin-Etsu Chemical Co., Ltd.) 2 / g) was changed from 130 parts to 65 parts,
[0281] 2) 25 parts of an inorganic filler material having a hollow portion (spherical silica having a hollow portion (average particle size 0.5 μm, porosity 50 vol %, “LHP-208” manufactured by Ube Exsymo Co., Ltd.) surface-treated with an amine alkoxysilane compound (“KBM573” manufactured by Shin-Etsu Chemical Co., Ltd.)) were used.
[0282] Except for the above matters, a resin composition 7 was obtained in the same manner as in Example 1.
[0283] <Example 8: Preparation of resin composition 8>
[0284] In Example 4, 5 parts of other curing agent (phenol-based curing agent, "LA-3018-50P" manufactured by DIC Corporation, hydroxyl equivalent 151 g / eq., 1-methoxy 2-propanol solution with 50% by mass of non-volatile components) are replaced with 5 parts of 50% by mass MEK solution of other curing agent (phenol-based curing agent, "KAYAHARD GPH103" manufactured by Nippon Kayaku Co., Ltd., hydroxyl equivalent 231 g / eq.).
[0285] Resin composition 8 was obtained in the same manner as in Example 4 except for the above matters.
[0286] <Example 9: Preparation of Resin Composition 9>
[0287] In Example 4,
[0288] 1) The amount of active ester resin A synthesized in Synthesis Example 1 was changed from 30 parts to 20 parts,
[0289] 2) 10.8 parts of an active ester curing agent ("HPC-8000-65T" manufactured by DIC Corporation, active group equivalent 223 g / eq., toluene solution containing 65% by mass of nonvolatile components) was further used.
[0290] Resin composition 9 was obtained in the same manner as in Example 4 except for the above matters.
[0291] <Example 10: Preparation of resin composition 10>
[0292] In Example 4,
[0293] 1) The amount of active ester resin A synthesized in Synthesis Example 1 was changed from 30 parts to 10 parts,
[0294] 2) Furthermore, 21.5 parts of an active ester curing agent ("HPC-8000-65T" manufactured by DIC Corporation, active group equivalent 223 g / eq., toluene solution containing 65% by mass of nonvolatile components) was used.
[0295] Except for the above matters, a resin composition 10 was obtained in the same manner as in Example 4.
[0296] <Example 11: Preparation of resin composition 11>
[0297] In Example 2,
[0298] 1) The amount of active ester resin B synthesized in Synthesis Example 2 was changed from 30 parts to 15 parts,
[0299] 2) 16.2 parts of an active ester curing agent ("HPC-8000-65T" manufactured by DIC Corporation, active group equivalent 223 g / eq., toluene solution containing 65% by mass of nonvolatile components) was further used.
[0300] Except for the above matters, a resin composition 11 was obtained in the same manner as in Example 2.
[0301] <Example 12: Preparation of resin composition 12>
[0302] In Example 2, 30 parts of the active ester resin B synthesized in Synthesis Example 2 was replaced with 30 parts of the active ester resin C shown below (wherein m, n ≥ 0, toluene solution with a nonvolatile content of 70% by mass, functional group equivalent of 250 g / eq.).
[0303] Except for the above matters, a resin composition 12 was obtained in the same manner as in Example 2.
[0304] [Chemical formula 16]
[0305]
[0306] <Example 13: Preparation of resin composition 13>
[0307] In Example 11, 15 parts of active ester resin B synthesized in Synthesis Example 2 was replaced with 15 parts of active ester resin C.
[0308] Except for the above matters, a resin composition 13 was obtained in the same manner as in Example 11.
[0309] <Comparative Example 1: Preparation of Resin Composition 14>
[0310] In Example 1, 2 parts of rubber particles ("EXL2655" manufactured by Dow Chemical Japan Co., Ltd.) were not used.
[0311] Except for the above matters, a resin composition 14 was obtained in the same manner as in Example 1.
[0312] <Comparative Example 2: Preparation of Resin Composition 15>
[0313] In Example 1, 30 parts of the active ester A resin synthesized in Synthesis Example 1 was replaced with 32.3 parts of an active ester curing agent ("HPC-8000-65T" manufactured by DIC Corporation, active group equivalent 223 g / eq., toluene solution containing 65% by mass of nonvolatile components).
[0314] Except for the above matters, a resin composition 15 was obtained in the same manner as in Example 1.
[0315] <Comparative Example 3: Preparation of Resin Composition 16>
[0316] In Example 1, the amount of rubber particles ("EXL2655" manufactured by Dow Chemical Japan Ltd.) was changed from 2 parts to 12 parts.
[0317] Except for the above matters, a resin composition 16 was obtained in the same manner as in Example 1.
[0318] <Measurement of average particle size of inorganic filler>
[0319] 100 mg of inorganic filler, 0.1 g of dispersant ("SN9228" manufactured by San Nopco), and 10 g of methyl ethyl ketone were weighed into a vial and dispersed by ultrasonic wave for 20 minutes. The particle size distribution was measured by batch unit (CELL) using a laser diffraction particle size distribution measuring device ("SALD-2200" manufactured by Shimadzu Corporation), and the average particle size based on the median particle size was calculated.
[0320] <Production of resin sheets>
[0321] As a support, a polyethylene terephthalate film ("Lumirror R80" manufactured by Toray Industries, Ltd., thickness 38 μm, softening point 130° C.) subjected to release treatment with an alkyd resin-based release agent ("AL-5" manufactured by LINTEC) was prepared.
[0322] Resin compositions 1 to 16 were uniformly applied to respective supports using a die coater so that the thickness of the dried resin composition layer was 40 μm, and the resin composition layer was formed on the support by drying at 70° C. to 100° C. for 3 minutes. Next, the rough surface of a polypropylene film (“ALPHAN MA-411” manufactured by Prince FTEX Co., Ltd., thickness 15 μm) as a protective film was attached to the surface of the resin composition layer not bonded to the support. Thus, a resin sheet having a support, a resin composition layer, and a protective film in this order was obtained.
[0323] <Test Example 1: Measurement of dielectric properties (dielectric constant, dielectric loss tangent)>
[0324] The protective film was peeled off from the prepared resin sheet, heated at 190°C for 90 minutes, and after the resin composition layer was thermally cured, the support was peeled off. It is called evaluation cured product C. The obtained evaluation cured product C was cut into test pieces with a width of 2 mm and a length of 80 mm. For the test piece, the "HP8362B" manufactured by Agilent Technologies was used, and the dielectric constant and dielectric loss tangent were measured by the cavity resonator perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23°C. Three test pieces were measured and the average value was calculated.
[0325] <Test Example 2: Measurement of MIT folding resistance>
[0326] The same evaluation cured product C as obtained in Test Example 1 was cut into test pieces with a width of 15 mm and a length of 110 mm. A bending test was carried out using an MIT testing apparatus (manufactured by Toyo Seiki Seisaku-sho, Ltd., MIT folding fatigue testing machine "MIT-DA") under the measuring conditions of a load of 2.5 N, a bending angle of 90 degrees, a bending radius of 1.0 mm, and a bending speed of 175 times / min, and the test was evaluated according to the following criteria.
[0327] ○: The number of bending times until the evaluation cured product C broke was 300 or more;
[0328] ×: The number of bending times until the evaluation cured product C broke was less than 300 times.
[0329] <Test Example 3: Measurement of Resin Bleeding Amount (Resin Flow Amount)>
[0330] (1) Preparation of inner substrate
[0331] The copper surface was roughened by etching 1 μm on both sides of a glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.4 mm, substrate size 340 mm×255 mm, "R1515A" manufactured by Panasonic) with an inner layer circuit using a microetchant ("CZ8101" manufactured by MEC).
[0332] (2) Lamination of resin sheets
[0333] The protective film was peeled off from the produced resin sheet (200mm×250mm) to expose the resin composition layer. An intermittent vacuum pressurized laminator (Nikko-Materials, 2-stage laminator "CVP700") was used to laminate the resin composition layer on both sides of the inner substrate in such a way that the inner substrate was in contact with the inner substrate. Lamination was performed by reducing the pressure for 30 seconds to adjust the air pressure to below 13hPa, and then pressing at 120°C and a pressure of 0.98MPa for 30 seconds. Next, hot pressing was performed at 120°C and a pressure of 0.54MPa for 60 seconds.
[0334] (3) Thermal curing of resin composition layer
[0335] Thereafter, the inner layer substrate laminated with the resin sheet was placed in an oven at 130° C. and heated for 30 minutes, and then transferred to an oven at 170° C. and heated for 30 minutes to thermally cure the resin composition layer, thereby forming an insulating layer.
[0336] (4) Observation of resin exudation
[0337] On the insulating layer, a resin seepage portion is formed outside the support due to the flow of the resin composition during lamination. The amount of the resin composition seeping out from the support is determined by measuring the distance from the end of the support to the end of the seeped resin, and evaluated according to the following criteria.
[0338] ○: The amount of seepage is less than 5 mm;
[0339] ×: The amount of seepage is greater than 5 mm.
[0340] [Table 1]
[0341] Table 1
[0342]
[0343] * In the table, the content of each component is a value when the non-volatile component in the resin composition is 100 mass %.
Claims
1. A resin composition comprising (A) an epoxy resin, (B) an active ester resin having an allyl group, and (C) an organic filler, in, When the nonvolatile component in the resin composition is 100 mass %, content of the component (C) is 6 mass % or less. 2 . The resin composition according to claim 1 , further comprising (D) a curing agent.
3. The resin composition according to claim 2, wherein The component (D) contains at least one selected from the group consisting of phenol-based curing agents, naphthol-based curing agents, carbodiimide-based curing agents, active ester-based curing agents (excluding those corresponding to the component (B)), benzoic acid, Oxazine-based curing agents and cyanate-based curing agents. The resin composition according to claim 1 , further comprising (E) an inorganic filler.
5. The resin composition according to claim 1, wherein The component (B) includes any one of a compound represented by the general formula (B-1), a compound represented by the general formula (B-2), and a compound represented by the general formula (B-3): [Chemical formula 1] In the general formula (B-1), Ar 11 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 12 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 13 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof, and n represents an integer of 0 to 10; [Chemical formula 2] In the general formula (B-2), Ar 21 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 22 Each independently represents a divalent hydrocarbon group which may have a substituent, Ar 23 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, and m represents an integer of 0 to 10; [Chemical formula 3] In the general formula (B-3), Ar 21 Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent, Ar 31 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, Ar 13 Each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof, and mb and nb each independently represent 0 or more.
6. The resin composition according to claim 1, wherein When the nonvolatile component in the resin composition is 100 mass %, the content of the component (B) is 1 mass % or more and 25 mass % or less.
7. The resin composition according to claim 1, wherein The component (C) includes core-shell type particles. 8 . A resin sheet comprising: a support and a resin composition layer provided on the support and containing the resin composition according to claim 1 . 9 . A printed wiring board comprising an insulating layer formed from a cured product of the resin composition according to claim 1 . 10 . A semiconductor device comprising the printed wiring board according to claim 9 .