High-temperature-resistant aerospace cable

The existing materials have been solved by using modified calcium sulfate whiskers in the protective layer materials of aerospace cables, combining acrylonitrile-butadiene-styrene copolymers and sodium gluconate to form chemical bonds. The problem of insufficient high-temperature performance has significantly improved the performance of the material and adapted to extreme environments in the aerospace field.

CN118931190APending Publication Date: 2024-11-12HEBEI PROVINCIAL INST OF PROD QUALITY SUPERVISION & INSPECTION +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411222278.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The protective layer materials of existing aerospace cables are poor in tensile strength and high temperature resistance, making it difficult to meet the operation needs of aerospace vehicles.

Method used

Using protective layer materials including phenyl silicone rubber, styrene butadiene rubber, modified calcium sulfate whiskers, anti-aging agents, vulcanizing agents and plasticizers, the modified calcium sulfate whiskers are passed through acrylonitrile-butadiene-styrene copolymers Combination with sodium gluconate forms chemical bonds to improve the tensile strength and high temperature resistance of the material.

Benefits of technology

The tensile strength and high temperature resistance of the protective layer material are significantly improved, and can better adapt to the extreme environmental requirements of the aerospace field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of cables, and provides a high-temperature-resistant aerospace cable which comprises a conductor and a protective layer extruded on the surface of the conductor, and the protective layer is prepared from the following raw materials in parts by weight: 100 parts of phenyl siloxane rubber, 30-40 parts of butadiene styrene rubber, 20-30 parts of modified calcium sulfate whiskers, 1-3 parts of an anti-aging agent, 3-5 parts of a vulcanizing agent and 6-10 parts of a plasticizer; the modified calcium sulfate whisker comprises the following components: acrylonitrile-butadiene-styrene copolymer and calcium sulfate whisker. According to the technical scheme, the problem that the tensile strength and the high-temperature resistance of a cable protection layer material for aerospace in the related technology are poor is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cables, and in particular to a high-temperature resistant cable for aerospace use. Background Art

[0002] Aerospace cables are special wires and cables used in aerospace vehicles and related equipment to transmit power, signals, and data. With the rapid development of the aerospace field, the operating environment of aircraft has become more complex and extreme. As a result, the market's performance requirements for aerospace cables are becoming increasingly stringent. Among them, the tensile properties and high temperature resistance of the cable protective layer material have attracted much attention.

[0003] At present, the existing aerospace cable shielding materials have poor performance in tensile strength and high temperature resistance, which makes it difficult to meet the operation requirements of aerospace vehicles. In view of this, in order to meet the special requirements of the aerospace field for cables, it is of great significance to develop an aerospace cable with high tensile strength and good high temperature resistance of the shielding material. Summary of the invention

[0004] The present invention provides a high temperature resistant aerospace cable, which solves the problem of poor tensile strength and high temperature resistance of aerospace cable protective layer materials in the related art.

[0005] The technical solution of the present invention is as follows: The present invention provides a high temperature resistant aerospace cable, comprising a conductor and a protective layer extruded on the surface of the conductor, wherein the raw materials of the protective layer include the following components in parts by weight: 100 parts of phenyl silicone rubber, 30-40 parts of styrene-butadiene rubber, 20-30 parts of modified calcium sulfate whiskers, 1-3 parts of antioxidant, 3-5 parts of vulcanizer, and 6-10 parts of plasticizer; The modified calcium sulfate whisker comprises acrylonitrile-butadiene-styrene copolymer and calcium sulfate whisker.

[0006] As a further technical solution, the conductor is an aluminum conductor or a copper conductor.

[0007] As a further technical solution, in the phenyl silicone rubber, the phenyl content is 15wt%~20wt%.

[0008] As a further technical solution, the weight ratio of the acrylonitrile-butadiene-styrene copolymer to the calcium sulfate whisker is 4-14:1.

[0009] In the present invention, when the weight ratio of acrylonitrile-butadiene-styrene copolymer to calcium sulfate whisker in the modified calcium sulfate whisker is 4-14:1, it helps to further improve the tensile strength and high temperature resistance of the protective layer material.

[0010] As a further technical solution, the preparation method of the modified calcium sulfate whisker comprises the following steps: dissolving acrylonitrile-butadiene-styrene copolymer in cyclohexanone, adding calcium sulfate whisker, dispersing evenly, and drying to obtain the modified calcium sulfate whisker.

[0011] As a further technical solution, the modified calcium sulfate whisker also includes sodium gluconate as a component.

[0012] In the present invention, the inventors found that when the modified calcium sulfate whisker also includes sodium gluconate, it helps to further improve the tensile strength and high temperature resistance of the protective layer material. It is speculated that this is because the addition of sodium gluconate can, on the one hand, complex the calcium ions in the calcium sulfate whisker, and on the other hand, can produce a chemical bond with the acrylonitrile-butadiene-styrene copolymer, thereby improving the overall stability of the modified calcium sulfate whisker.

[0013] As a further technical solution, the weight ratio of the calcium sulfate whisker, acrylonitrile-butadiene-styrene copolymer and sodium gluconate is 24:3~4.5:1.5~3.

[0014] In the present invention, when the weight ratio of calcium sulfate whiskers, acrylonitrile-butadiene-styrene copolymer and sodium gluconate in the modified calcium sulfate whiskers is 24:3-4.5:1.5-3, it helps to further improve the tensile strength and high temperature resistance of the protective layer material.

[0015] As a further technical solution, the preparation method of the modified calcium sulfate whisker comprises the following steps: A1. Dissolve sodium gluconate in water, add calcium sulfate whiskers, disperse evenly, react, and dehydrate to obtain a precursor; A2. Dissolve acrylonitrile-butadiene-styrene copolymer in cyclohexanone, add the precursor, disperse evenly, and dry to obtain the modified calcium sulfate whisker.

[0016] As a further technical solution, in step A1, during the reaction, the temperature is 70-80°C and the reaction time is 1-2h.

[0017] As a further technical solution, the antioxidant includes one or more of antioxidant MB, antioxidant 2246, and antioxidant AW, preferably antioxidant AW.

[0018] As a further technical solution, the vulcanizing agent includes one or more of the vulcanizing agent DCP, the vulcanizing agent DTBP, and the vulcanizing agent TMTD, preferably the vulcanizing agent DCP.

[0019] As a further technical solution, the plasticizer includes one or more of plasticizer DOA, plasticizer DOTP, and plasticizer DOP, preferably plasticizer DOA.

[0020] The present invention also provides a method for preparing the high temperature resistant aerospace cable, comprising the following steps: S1. Mixing the components of the protective layer raw material except the vulcanizing agent, adding the vulcanizing agent, and extruding to obtain the protective layer material; S2. Extruding the protective layer material onto the surface of the conductor to obtain a high temperature resistant aerospace cable.

[0021] As a further technical solution, in step S1, the temperature during the mixing is 80-90°C.

[0022] As a further technical solution, in step S1, the temperature during extrusion is 180-220°C.

[0023] The working principle and beneficial effects of the present invention are: In the present invention, modified calcium sulfate whiskers are added to the protective layer of the high-temperature resistant aerospace cable. The calcium sulfate whiskers are modified by acrylonitrile-butadiene-styrene copolymer, so that the modified calcium sulfate whiskers can form aromatic accumulation in the protective layer, and the simple physical dispersion is converted into chemical bonding, thereby enhancing the functionality of the calcium sulfate whiskers, and further significantly improving the tensile strength and high-temperature resistance of the protective layer material. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In the following embodiments and comparative examples, unless otherwise specified, the conductor is a copper conductor, model C19400; the weight average molecular weight of the phenyl silicone rubber is 600,000, and the phenyl content is 15wt%; the model of the styrene-butadiene rubber is SBS-1201E; the model of the acrylonitrile-butadiene-styrene copolymer is CF-610A; the model of the styrene-acrylonitrile copolymer is NF-2200AR; and the model of the calcium sulfate whisker is NP-G02.

[0026] Example 1 A method for preparing a high temperature resistant aerospace cable comprises the following steps: S1. By weight, 100 parts of phenyl silicone rubber, 30 parts of styrene-butadiene rubber, 20 parts of modified calcium sulfate whiskers, 1 part of antioxidant AW, and 6 parts of plasticizer DOA are mixed at 85° C., 3 parts of vulcanizing agent DCP are added, and extruded to obtain a protective layer material; Among them, during extrusion, the temperature of zone 1 is 180°C, the temperature of zone 2 is 220°C, and the temperature of zone 3 is 200°C; The preparation method of modified calcium sulfate whisker comprises the following steps: dissolving 1 part of acrylonitrile-butadiene-styrene copolymer in 40 parts of cyclohexanone, adding 19 parts of calcium sulfate whisker, dispersing evenly, and drying to obtain modified calcium sulfate whisker; S2. Extruding the protective layer material onto the surface of the conductor to obtain a high temperature resistant aerospace cable.

[0027] Example 2 A method for preparing a high temperature resistant aerospace cable comprises the following steps: S1. By weight, 100 parts of phenyl silicone rubber, 40 parts of styrene-butadiene rubber, 30 parts of modified calcium sulfate whiskers, 3 parts of antioxidant AW, and 10 parts of plasticizer DOA are mixed at 85° C., 5 parts of vulcanizing agent DCP are added, and extruded to obtain a protective layer material; Among them, during extrusion, the temperature of zone 1 is 180°C, the temperature of zone 2 is 220°C, and the temperature of zone 3 is 200°C; The preparation method of modified calcium sulfate whisker comprises the following steps: dissolving 1 part of acrylonitrile-butadiene-styrene copolymer in 60 parts of cyclohexanone, adding 29 parts of calcium sulfate whisker, dispersing evenly, and drying to obtain modified calcium sulfate whisker; S2. Extruding the protective layer material onto the surface of the conductor to obtain a high temperature resistant aerospace cable.

[0028] Example 3 The only difference between this embodiment and embodiment 2 is that, in this embodiment, when preparing the modified calcium sulfate whisker, the weight parts of acrylonitrile-butadiene-styrene copolymer are 8 parts, and the weight parts of calcium sulfate whisker are 22 parts.

[0029] Example 4 The only difference between this embodiment and embodiment 2 is that, in this embodiment, when preparing the modified calcium sulfate whisker, the weight parts of acrylonitrile-butadiene-styrene copolymer are 2 parts, and the weight parts of calcium sulfate whisker are 28 parts.

[0030] Example 5 The only difference between this embodiment and embodiment 2 is that, in this embodiment, when preparing the modified calcium sulfate whisker, the weight parts of acrylonitrile-butadiene-styrene copolymer are 6 parts, and the weight parts of calcium sulfate whisker are 24 parts.

[0031] Example 6 The difference between this embodiment and embodiment 2 is that, in this embodiment, the preparation method of modified calcium sulfate whiskers comprises the following steps: A1. Dissolve 4 parts of sodium gluconate in 30 parts of water, add 24 parts of calcium sulfate whiskers, disperse evenly, react at 75°C for 1.5 hours, dehydrate, and obtain a precursor; A2. Dissolve 2 parts of acrylonitrile-butadiene-styrene copolymer in 60 parts of cyclohexanone, add the precursor, disperse evenly, and dry to obtain modified calcium sulfate whiskers.

[0032] Example 7 The only difference between this embodiment and embodiment 6 is that, in this embodiment, when preparing the modified calcium sulfate whisker, the weight portion of sodium gluconate is 0.5 parts, and the weight portion of acrylonitrile-butadiene-styrene copolymer is 5.5 parts.

[0033] Example 8 The only difference between this embodiment and embodiment 6 is that, in this embodiment, when preparing the modified calcium sulfate whisker, the weight parts of sodium gluconate are 3 parts and the weight parts of acrylonitrile-butadiene-styrene copolymer are 3 parts.

[0034] Example 9 The only difference between this embodiment and embodiment 6 is that, in this embodiment, when preparing the modified calcium sulfate whisker, the weight parts of sodium gluconate are 1.5 parts, and the weight parts of acrylonitrile-butadiene-styrene copolymer are 4.5 parts.

[0035] Comparative Example 1 The only difference between this comparative example and Example 1 is that in this comparative example, the modified calcium sulfate whisker is replaced by an equal amount of calcium sulfate whisker.

[0036] Comparative Example 2 The only difference between this comparative example and Example 1 is that in this comparative example, the preparation method of modified calcium sulfate whiskers comprises the following steps: dissolving 1 part of styrene-acrylonitrile copolymer in 40 parts of cyclohexanone, adding 19 parts of calcium sulfate whiskers, dispersing evenly, and drying to obtain modified calcium sulfate whiskers.

[0037] The following performance tests were performed on the protective layer materials in Examples 1 to 9 and Comparative Examples 1 to 2: ① Tensile strength: refer to GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber" to test the tensile strength, where the specimen is a type 1 dumbbell specimen, and the average value of 3 specimens in each group is taken as the final result; ②High temperature resistance: Refer to GB / T 3512-2014 "Hot air accelerated aging and heat resistance test for vulcanized rubber or thermoplastic rubber" to test the change rate of tensile strength. The test temperature is 200℃, the test time is 10 days, and the average value of 3 samples in each group is taken as the final result.

[0038] The test results are shown in Table 1 below.

[0039] Table 1 Test results

[0040] Comparison between Example 1 and Comparative Examples 1 to 2 shows that by modifying calcium sulfate whiskers by acrylonitrile-butadiene-styrene copolymer, the tensile strength and high temperature resistance of the protective layer material can be significantly improved. Comparison between Examples 2 to 3 and Examples 4 to 5 shows that when the weight ratio of acrylonitrile-butadiene-styrene copolymer and calcium sulfate whiskers in the modified calcium sulfate whiskers is 4 to 14:1, it helps to further improve the tensile strength and high temperature resistance of the protective layer material. Comparison between Examples 2 to 5 and Examples 6 to 9 shows that when the components of the modified calcium sulfate whiskers also include sodium gluconate, it helps to further improve the tensile strength and high temperature resistance of the protective layer material. Comparison between Examples 6 to 7 and Examples 8 to 9 shows that when the weight ratio of calcium sulfate whiskers, acrylonitrile-butadiene-styrene copolymer and sodium gluconate in the modified calcium sulfate whiskers is 24:3 to 4.5:1.5 to 3, it helps to further improve the tensile strength and high temperature resistance of the protective layer material.

[0041] The present invention is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high temperature resistant aerospace cable, comprising a conductor and a protective layer extruded on the surface of the conductor, characterized in that: The raw materials of the protective layer include the following components in parts by weight: 100 parts of phenyl silicone rubber, 30-40 parts of styrene-butadiene rubber, 20-30 parts of modified calcium sulfate whiskers, 1-3 parts of antioxidant, 3-5 parts of vulcanizing agent, and 6-10 parts of plasticizer; The modified calcium sulfate whisker comprises acrylonitrile-butadiene-styrene copolymer and calcium sulfate whisker.

2. A high temperature resistant aerospace cable according to claim 1, characterized in that: The weight ratio of the acrylonitrile-butadiene-styrene copolymer to the calcium sulfate whisker is 4-14:

1.

3. The high temperature resistant aerospace cable according to claim 1, characterized in that: The preparation method of the modified calcium sulfate whisker comprises the following steps: dissolving acrylonitrile-butadiene-styrene copolymer in cyclohexanone, adding calcium sulfate whisker, dispersing evenly, and drying to obtain the modified calcium sulfate whisker.

4. The high temperature resistant aerospace cable according to claim 1, characterized in that: The modified calcium sulfate whisker also includes sodium gluconate as a component.

5. A high temperature resistant aerospace cable according to claim 4, characterized in that: The weight ratio of the calcium sulfate whisker, acrylonitrile-butadiene-styrene copolymer and sodium gluconate is 24:3-4.5:1.5-3.

6. A high temperature resistant aerospace cable according to claim 4, characterized in that: The preparation method of the modified calcium sulfate whisker comprises the following steps: A1. Dissolve sodium gluconate in water, add calcium sulfate whiskers, disperse evenly, react, and dehydrate to obtain a precursor; A2. Dissolve acrylonitrile-butadiene-styrene copolymer in cyclohexanone, add the precursor, disperse evenly, and dry to obtain the modified calcium sulfate whisker.

7. A high temperature resistant aerospace cable according to any one of claims 1 to 6, characterized in that: The antioxidant includes one or more of antioxidant MB, antioxidant 2246, and antioxidant AW.

8. A high temperature resistant aerospace cable according to any one of claims 1 to 6, characterized in that: The vulcanizing agent includes one or more of DCP, DTBP and TMTD.

9. A high temperature resistant aerospace cable according to any one of claims 1 to 6, characterized in that: The plasticizer includes one or more of DOA, DOTP and DOP.

10. A method for preparing a high temperature resistant aerospace cable according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Mixing the components of the protective layer raw material except the vulcanizing agent, adding the vulcanizing agent, and extruding to obtain the protective layer material; S2. Extruding the protective layer material onto the surface of the conductor to obtain a high temperature resistant aerospace cable.

Citation Information

Cited By

  • High-temperature-resistant hydraulic rubber tube and preparation method thereof

    CN119307024A

  • High-temperature-resistant cable for aerospace and preparation method and application of high-temperature-resistant cable

    CN119314724A