Insulation sealing cold shrink tube
By using a combination of methyl vinyl silicone rubber and imidazolylthiourea compound crosslinking agent in the cold shrink tube, the problem of lax sealing of the cold shrink tube in harsh environments is solved, and its strength and insulation performance are improved, ensuring that Sealing effect and durability in high temperature, high humidity and high pressure environments.
Patent Information
- Application Number
- CN202411229024.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
The existing cold shrink pipe is not tightly sealed in harsh environments, resulting in invasion of moisture and pollutants, low strength, unable to provide sufficient protection, and affecting the performance of the equipment.
Using a combination of methylvinyl silicone rubber and imidazolylthiourea compound crosslinking agent, the three-dimensional network structure of the material is increased by regulating the crosslinking density and molecular structure, and the strength and sealing performance of the cold shrink tube are improved, and the appropriate Vinyl content and other additives optimize insulation properties.
It significantly improves the strength and insulation sealing performance of the cold-condensing pipe, and can maintain the sealing effect in harsh environments such as high temperature, high humidity, and high pressure, extends the service life, and enhances the resistance to external force impacts.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cold shrink tubes, and in particular to an insulating and sealed cold shrink tube. Background Art
[0002] Cold shrink tubing is a tubular product made of special rubber material. It has the characteristics of shrinking at room temperature and fitting tightly to the wrapped object. It does not require heating and is easy and quick to install. It is widely used in the fields of electricity, communications, electronic equipment, etc. However, in some harsh environments, such as high temperature, high humidity, high pressure, etc., cold shrink tubing is prone to poor sealing, resulting in the intrusion of moisture and other pollutants, affecting the performance of the equipment. After long-term use, cold shrink tubing may age and crack, reducing its insulation and sealing effect. When subjected to external impact or stretching, the cold shrink tubing may break or be damaged and cannot provide adequate protection. Therefore, the development of a high-strength cold shrink tubing with good insulation and sealing performance is an urgent problem to be solved. Summary of the invention
[0003] The invention provides an insulating sealed cold shrink tube, which solves the problems of low strength and poor insulating and sealing performance of the cold shrink tube in the related art.
[0004] The technical scheme of the present invention is as follows: The present invention provides an insulating sealed cold shrink tube, comprising the following component raw materials in parts by weight: 100 parts of methyl vinyl silicone rubber, 30-40 parts of trifluoropropyl methyl vinyl silicone rubber, 2.4 parts of a crosslinking agent, 1-3 parts of a coupling agent, 8-10 parts of a plasticizer, 5-20 parts of a filler, 2-4 parts of a vulcanizing agent, 1-3 parts of an antioxidant, and 10-30 parts of a flame retardant; The cross-linking agent is an imidazolylthiourea compound.
[0005] As a further technical solution, the imidazolyl thiourea compound consists of (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea.
[0006] As a further technical solution, the mass ratio of the (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea is 2:1~3.
[0007] In the present invention, by controlling the mass ratio of (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea, the crosslinking density and molecular structure of the imidazole thiourea compound and the methyl vinyl silicone rubber are regulated, thereby obtaining a high-strength cold shrink tube.
[0008] As a further technical solution, the mass ratio of the (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea is 1:1.
[0009] As a further technical solution, the vinyl content of the methyl vinyl silicone rubber is 0.13 mol% to 1.79 mol%.
[0010] In the present invention, methyl vinyl silicone rubber with different vinyl contents is selected as the raw material. When the vinyl content is 0.13 mol% to 1.79 mol%, the strength and insulation performance of the cold shrink tube can be further improved.
[0011] As a further technical solution, the vinyl content of the methyl vinyl silicone rubber is 0.50 mol% to 0.79 mol%.
[0012] As a further technical solution, the plasticizer includes one or more of dioctyl phthalate, dioctyl sebacate, and dioctyl adipate.
[0013] As a further technical solution, the coupling agent includes one or more of vinyl triethoxy silane, vinyl trimethoxy silane, and vinyl tri(β-methoxyethoxy) silane.
[0014] As a further technical solution, the filler includes one or more of calcium carbonate, talc, and kaolin.
[0015] As a further technical solution, the vulcanizing agent includes one or more of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, benzoyl peroxide, and diisopropylbenzene peroxide.
[0016] As a further technical solution, the antioxidant includes one or two of dibutyl nickel dithiocarbamate and N-isopropyl-N'-phenyl-p-phenylenediamine.
[0017] As a further technical solution, the flame retardant includes one or more of aluminum hydroxide, magnesium hydroxide, and molybdenum trioxide.
[0018] The present invention also provides a method for preparing an insulating sealed cold shrink tube, comprising the following steps: S1. Weigh methyl vinyl silicone rubber, trifluoropropyl methyl vinyl silicone rubber, coupling agent, plasticizer, filler, vulcanizer, antioxidant, and flame retardant, knead and mix, heat and evacuate, add crosslinking agent, and cut to obtain silicone rubber masterbatch; S2. After the silicone rubber masterbatch is extruded, passed through a drying tunnel, and cooled, an insulating and sealed cold shrink tube is obtained.
[0019] As a further technical solution, the kneading and mixing time is 1 to 3 hours, the heating temperature is 100 to 150°C, the vacuuming time is 0.5 to 1.5 hours, the vacuum degree of the vacuuming is -0.05 to -0.1 MPa, the extrusion temperature is 15 to 30°C, the drying tunnel temperature is 120 to 180°C, and the drying tunnel time is 10 to 30 minutes.
[0020] The working principle and beneficial effects of the present invention are: In the present invention, an imidazolyl thiourea compound is added as a crosslinking agent, which reacts with methyl vinyl silicone rubber to form a crosslinking structure and hydrogen bonding force, thereby increasing the three-dimensional network structure of the material, thereby improving the strength and sealing performance of the cold shrink tube. The present invention also adds methyl vinyl silicone rubber with a certain vinyl content as a raw material, affects the insulation performance of the cold shrink tube through resistivity and dielectric strength, and obtains a cold shrink tube with the best insulation effect. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] Example 1 S1. Weigh 100 parts of methyl vinyl silicone rubber (vinyl content 0.03 mol% to 0.06 mol%, model 112-0), 30 parts of trifluoropropyl methyl vinyl silicone rubber, 1 part of vinyl triethoxysilane, 8 parts of dioctyl phthalate, 5 parts of calcium carbonate, 2 parts of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 1 part of nickel dibutyl dithiocarbamate, and 10 parts of aluminum hydroxide, knead and mix for 1 hour, evacuate at 100°C for 0.5 hour, and the vacuum degree is -0.05 MPa. After cooling, add 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea, and cut to obtain a silicone rubber masterbatch; S2. Put the silicone rubber masterbatch into a cold feed extruder at a temperature of 15°C. After extrusion molding, pass through a drying tunnel for 10 minutes at a temperature of 120°C. After cooling, an insulating and sealed cold shrink tube is obtained.
[0023] Example 2 S1. Weigh 100 parts of methyl vinyl silicone rubber (vinyl content 0.03 mol%~0.06 mol%, model 112-0), 35 parts of trifluoropropyl methyl vinyl silicone rubber, 2 parts of vinyl trimethoxysilane, 9 parts of dioctyl sebacate, 15 parts of talc, 3 parts of benzoyl peroxide, 2 parts of nickel dibutyl dithiocarbamate, and 20 parts of magnesium hydroxide, knead and mix for 2 hours, evacuate at 125°C for 1 hour, and the vacuum degree is -0.08 MPa. After cooling, add 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea, and cut to obtain a silicone rubber masterbatch; S2. Put the silicone rubber masterbatch into a cold feed extruder at a temperature of 22°C. After extrusion molding, pass through a drying tunnel for 20 minutes at a temperature of 150°C. After cooling, an insulating and sealed cold shrink tube is obtained.
[0024] Example 3 S1. Weigh 100 parts of methyl vinyl silicone rubber (vinyl content 0.03 mol%~0.06 mol%, model 112-0), 40 parts of trifluoropropyl methyl vinyl silicone rubber, 3 parts of vinyl tri(β-methoxyethoxy) silane, 10 parts of dioctyl adipate, 20 parts of kaolin, 4 parts of diisopropyl peroxide, 3 parts of N-isopropyl-N'-phenyl-p-phenylenediamine, and 30 parts of molybdenum trioxide, knead and mix for 3 hours, evacuate at 150°C for 1.5 hours, and the vacuum degree is -0.1 MPa. After cooling, add 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea, and cut to obtain a silicone rubber masterbatch; S2. Put the silicone rubber masterbatch into a cold feed extruder at a temperature of 30°C. After extrusion molding, pass through a drying tunnel for 30 minutes at a temperature of 180°C. After cooling, an insulating and sealed cold shrink tube is obtained.
[0025] Example 4 Compared with Example 3, the difference of Example 4 is that 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea are replaced by an equal amount of 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea.
[0026] Example 5 Compared with Example 3, the difference of Example 5 is that 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea are replaced by 1.8 parts of (9CI)-1H-benzimidazole-2-thiourea and 0.6 parts of 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea.
[0027] Example 6 Compared with Example 3, the difference of Example 6 is that 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea are replaced by 1.6 parts of (9CI)-1H-benzimidazole-2-thiourea and 0.8 parts of 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea.
[0028] Example 7 Compared with Example 3, the difference of Example 7 is that 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea are replaced by 1.2 parts of (9CI)-1H-benzimidazole-2-thiourea and 1.2 parts of 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea.
[0029] Example 8 Compared with Example 3, the difference of Example 8 is that 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea are replaced by 0.96 parts of (9CI)-1H-benzimidazole-2-thiourea and 1.44 parts of 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea.
[0030] Example 9 Compared with Example 3, the difference of Example 9 is that 2.4 parts of (9CI)-1H-benzimidazole-2-thiourea are replaced by 0.8 parts of (9CI)-1H-benzimidazole-2-thiourea and 1.6 parts of 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea.
[0031] Example 10 Compared with Example 7, the difference of Example 10 is that 100 parts of methyl vinyl silicone rubber (vinyl content 0.03 mol%~0.06 mol%, model 112-0) are replaced by an equal amount of methyl vinyl silicone rubber (vinyl content 0.13 mol%~0.18 mol%, model 112-2).
[0032] Embodiment 11 Compared with Example 7, the difference of Example 11 is that 100 parts of methyl vinyl silicone rubber (vinyl content 0.03 mol%~0.06 mol%, model 112-0) are replaced by an equal amount of methyl vinyl silicone rubber (vinyl content 0.50 mol%~0.79 mol%, model 112-5).
[0033] Example 12 Compared with Example 7, the difference of Example 12 is that 100 parts of methyl vinyl silicone rubber (vinyl content 0.03 mol%~0.06 mol%, model 112-0) are replaced by an equal amount of methyl vinyl silicone rubber (vinyl content 0.80 mol%~1.79 mol%, model 112-6).
[0034] Embodiment 13 Compared with Example 7, the difference of Example 13 is that 100 parts of methyl vinyl silicone rubber (vinyl content 0.03 mol%~0.06 mol%, model 112-0) are replaced by an equal amount of methyl vinyl silicone rubber (vinyl content 1.80 mol%~5 mol%, model 112-7).
[0035] Comparative Example 1 Compared with Example 3, Comparative Example 1 is different in that (9CI)-1H-benzimidazole-2-thiourea is not added.
[0036] The insulating sealed cold shrink tubes prepared in Examples 1 to 13 and Comparative Example 1 were tested according to the following method: 1. Dielectric constant: According to the test method specified in GB / T 1693-2007 "Determination of dielectric constant and dielectric loss tangent of vulcanized rubber", the dielectric constant of the sample is tested.
[0037] 2. Tensile strength: Test the tensile strength of the sample according to the test method specified in GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber".
[0038] The test results are shown in the following table: Table 1 Performance test results of the insulating sealed cold shrink tubes prepared in Examples 1 to 13 and Comparative Example 1
[0039] Compared with Comparative Example 1, Example 1 adds (9CI)-1H-benzimidazole-2-thiourea, and Example 4 adds 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea. As a result, the dielectric constant and tensile strength of Example 1 and Example 4 are better than those of Comparative Example 1, indicating that the addition of (9CI)-1H-benzimidazole-2-thiourea or 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea can improve the dielectric constant and tensile strength of the cold shrink tube.
[0040] Compared with Examples 1 and 4, Examples 5 to 9 simultaneously added (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea. As a result, the dielectric constants and tensile strengths of Examples 5 to 9 were better than those of Examples 1 and 4, indicating that (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea played a synergistic role, which could further improve the dielectric constant and tensile strength of the cold shrink tube. In Examples 5 to 9, different mass ratios of (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea were added. As a result, the dielectric constant and tensile strength of Examples 6 to 8 were better than those of Examples 5 and 9, indicating that when the mass ratio of (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea was 2:1 to 3, and the preferred ratio was 1:1, the dielectric constant and tensile strength of the obtained cold shrink tube were better.
[0041] Compared with Example 7, Examples 10 to 13 added methyl vinyl silicone rubber with different vinyl contents. As a result, the dielectric constant and tensile strength of Examples 10 to 12 were better than those of Examples 7 and 13, indicating that when the vinyl content was 0.13 mol% to 1.79 mol%, and the preferred range was 0.50 mol% to 0.79 mol%, the dielectric constant and tensile strength of the obtained cold shrink tube were optimal.
[0042] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An insulating sealed cold shrink tube, characterized in that: The composition comprises the following raw materials in parts by weight: 100 parts of methyl vinyl silicone rubber, 30-40 parts of trifluoropropyl methyl vinyl silicone rubber, 2.4 parts of a crosslinking agent, 1-3 parts of a coupling agent, 8-10 parts of a plasticizer, 5-20 parts of a filler, 2-4 parts of a vulcanizing agent, 1-3 parts of an antioxidant, and 10-30 parts of a flame retardant; the crosslinking agent is an imidazole thiourea compound.
2. The insulating sealed cold shrink tube according to claim 1, characterized in that: The imidazolylthiourea compound consists of (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea.
3. The insulating sealed cold shrink tube according to claim 2, characterized in that: The mass ratio of the (9CI)-1H-benzimidazole-2-thiourea and 1-[2-(1H-benzimidazole-2-yl)ethylamino]-3-(2-chlorophenyl)thiourea is 2:1-3.
4. The insulating sealed cold shrink tube according to claim 1, characterized in that: The vinyl content of the methyl vinyl silicone rubber is 0.13 mol % to 1.79 mol %.
5. The insulating sealed cold shrink tube according to claim 1, characterized in that: The plasticizer includes one or more of dioctyl phthalate, dioctyl sebacate, and dioctyl adipate.
6. The insulating sealed cold shrink tube according to claim 1, characterized in that: The coupling agent includes one or more of vinyl triethoxy silane, vinyl trimethoxy silane, and vinyl tri(β-methoxyethoxy) silane.
7. The insulating sealed cold shrink tube according to claim 1, characterized in that: The filler includes one or more of calcium carbonate, talc and kaolin.
8. The insulating sealed cold shrink tube according to claim 1, characterized in that: The vulcanizing agent includes one or more of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, benzoyl peroxide, and diisopropylbenzene peroxide.
9. The insulating sealed cold shrink tube according to claim 1, characterized in that: The antioxidant includes one or two of dibutyl nickel dithiocarbamate and N-isopropyl-N'-phenyl-p-phenylenediamine.
10. The insulating sealed cold shrink tube according to claim 1, characterized in that: The flame retardant includes one or more of aluminum hydroxide, magnesium hydroxide, and molybdenum trioxide.