Anti-aging bio-based rubber asphalt material as well as preparation method and application thereof
By mixing rubber powder and bio-oil and expanding microwave to form bio-based modified rubber and mixing it with matrix asphalt, the problem of aging of rubber asphalt intensifies at high temperatures is solved, and its anti-aging performance and road service life are significantly improved.
Patent Information
- Application Number
- CN202410998999.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The performance damage of existing rubber asphalt at high temperatures leads to aggravation of aging, affecting the mechanical properties and long-term service performance of asphalt pavement.
Rubber powder and bio-oil are used as raw materials to obtain bio-based modified rubber through microwave expansion, and mixed with matrix asphalt to form anti-aging bio-based rubber asphalt material, improving the self-healing ability and anti-aging properties of rubber asphalt.
It delays the aging process of rubber asphalt, improves its mechanical properties and rheological properties after aging of hot oxygen and ultraviolet rays, reduces the aging index, enhances the strength and moisture resistance of the interface between asphalt and aggregates, and extends the service life of the road surface. .
Smart Images

Figure CN118931213A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of asphalt materials and relates to an anti-aging bio-based rubber asphalt material and a preparation method and application thereof. Background Art
[0002] As an environmentally friendly, economical and high-performance road engineering material, rubber asphalt has received widespread attention in recent years, especially in functional pavements such as drainage, noise reduction and deicing. However, rubber asphalt pavement will gradually age during its service, and during the aging process, it will induce various diseases such as cracking and peeling in the asphalt pavement, resulting in pavement performance. In view of the performance degradation behavior of asphalt and rubber asphalt under the action of environmental factors, it is necessary to modify the asphalt. With reference to the Chinese patent document with application number CN202111145163.5, a modified asphalt mortar based on green composite filler and a preparation method thereof are disclosed, the formula includes: green composite filler, composite modified asphalt, anti-aging agent and co-solvent, and shell powder, coal gangue powder, fly ash and waste brick powder are used in the formula. While improving the high and low temperature performance of asphalt, it also reduces the porosity of asphalt, enhances the adhesion between asphalt and mineral powder, and reduces the pollution of waste materials to the environment.
[0003] Through the analysis and research of the existing asphalt modification technology, it is found that it mainly slows down the aging rate of asphalt materials by shielding ultraviolet light, isolating oxygen or capturing oxygen-containing free radicals, thereby improving the mechanical properties of asphalt pavement. However, these methods have problems such as complex production process, high cost of use, poor compatibility between inorganic materials and asphalt, which leads to damage to the performance of rubber asphalt at high temperature, causing aging to accelerate, greatly affecting the performance of asphalt, and cannot be widely used in pavement. Summary of the invention
[0004] In view of the technical problem in the prior art that the performance of rubber asphalt is damaged at high temperature, resulting in accelerated aging and greatly affecting the performance of asphalt, the present invention provides an anti-aging bio-based rubber asphalt material and a preparation method and application thereof.
[0005] The present invention uses rubber powder and bio-oil as raw materials, obtains bio-based modified rubber by microwave expansion, and further mixes it with base asphalt to obtain anti-aging bio-based rubber asphalt material, thereby improving the self-healing ability of rubber asphalt and avoiding damage, thereby improving the anti-aging ability of base asphalt.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing an anti-aging bio-based rubber asphalt material comprises the following steps:
[0008] S1. Mix rubber powder and bio-oil in a mass ratio of 1:(0.5-1.5), and stir evenly under heating conditions to prepare substance A;
[0009] S2, expanding the substance A in step S1 at room temperature to prepare a bio-based expanded rubber;
[0010] S3, expanding the bio-expanded rubber prepared in step S2 under microwaves to prepare a bio-based modified rubber;
[0011] S4. Add the bio-based modified rubber of step S3 to the base asphalt, wherein the mass of the bio-based modified rubber added is 10% to 20% of the mass of the base asphalt, and then stir and react under heating conditions to obtain an anti-aging bio-based rubber asphalt material.
[0012] It is further defined that in step S1, the main chemical components of the bio-oil are hexanal, methyl heptanoate, methyl hexanoate, methyl octanoate, 1,2,3,4-tetramethylbenzene, 1-pentanol, valeraldehyde, 2-heptanone, methyl salicylate and 1-octene.
[0013] It is further defined that the rubber powder in step S1 is obtained by grinding waste tires into particles using a mechanical grinding method at room temperature, and the particle size of the rubber powder is 0.18 mm to 0.25 mm.
[0014] It is further defined that in step S1, the heating temperature is 100°C to 150°C, and the stirring time is 30min to 60min.
[0015] It is further defined that in step S2, the expansion time is 6 hours to 18 hours.
[0016] It is further defined that in step S3, the power of the microwave is 300W to 500W, the frequency of the microwave is 2000MHz to 3000MHz, and the expansion time is 2min to 8min.
[0017] It is further defined that in step S4, the heating temperature is 150° C. to 200° C., and the stirring time is 10 min to 50 min.
[0018] The anti-aging bio-based rubber asphalt material is prepared by the method for preparing the anti-aging bio-based rubber asphalt material.
[0019] Application of anti-aging bio-based rubber asphalt material in pavement engineering.
[0020] The beneficial effects of the present invention are:
[0021] 1. The present invention uses rubber powder and bio-oil as raw materials, obtains bio-based modified rubber by microwave expansion, and further mixes it with matrix asphalt to obtain anti-aging bio-based rubber asphalt material, thereby improving the self-healing ability of rubber asphalt and avoiding damage, thereby improving the anti-aging ability of matrix asphalt; and further making the ability to resist water damage after aging stronger.
[0022] 2. The bio-based rubber asphalt material formed by the present invention can inhibit the formation of aging products in the asphalt material, thereby reducing the degradation of the mechanical properties of the rubber asphalt after thermal oxidation and ultraviolet aging, and delaying the occurrence and development of pavement diseases; it can also improve the rheological properties of the rubber asphalt after aging and the asphalt-aggregate interface strength, improve the long-term pavement service performance of the rubber asphalt, and ultimately achieve the goal of green development.
[0023] 3. The present invention has found through research that the addition of bio-oil can reduce the formation of carbonyl components in the para phase of the rubber asphalt binder after aging, thereby reducing the chemical aging index by 13%; the bio-oil can also enhance the stability and self-healing ability of the rubber asphalt binder during thermal aging and ultraviolet aging. The softening and deaggregation ability of the bio-oil compensates for the evolution of components in the asphalt binder caused by aging, so that the BMR maintains a 43% lower aggregation index based on the UV-visible absorption spectrum, and the growth of the medium molecular size content is reduced by 22%.
[0024] 4. Compared with ordinary rubber asphalt, the deagglomeration ability of the bio-based rubber asphalt of the present invention makes the modified asphalt material have better cohesion; the bio-based rubber asphalt has higher affinity and stronger moisture resistance, which increases the sensitivity of the road surface to moisture.
[0025] 5. The bio-oil used in the present invention has a stable source, and its main components are hexanal, methyl heptanoate, methyl hexanoate, methyl octanoate, 1,2,3,4-tetramethylbenzene, 1-pentanol, valeraldehyde, 2-heptanone, methyl salicylate and 1-octene. The bio-oil has good compatibility with rubber asphalt, the process is simple, and it has high road performance and road use performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The comparison chart of carbonyl and sulfoxide contents of the bio-based rubber asphalt and rubber asphalt prepared in Example 1 after 40 hours of heat aging or 150 hours of ultraviolet aging, respectively, indicates that the bio-oil inhibits the formation of aging products;
[0027] Figure 2 Comparison of the topographic image and phase image of the bio-based rubber asphalt (BMR) prepared in Example 1, rubber asphalt (CRM), and bio-based asphalt (BOA) before and after aging;
[0028] Figure 3This is a comparison chart of the agglomeration index of the bio-based rubber asphalt and the rubber asphalt prepared in Example 1 under different aging conditions;
[0029] Figure 4 This is a graph of asphalt self-healing performance of bio-based rubber asphalt and rubber asphalt prepared in Example 1 under different aging conditions;
[0030] Figure 5 This is a cross modulus comparison diagram of the bio-based rubber asphalt and the rubber asphalt prepared in Example 1 after heat aging and ultraviolet aging respectively;
[0031] Figure 6 It is a comparison chart of the contact angle moisture sensitivity index of the bio-based rubber asphalt and the rubber asphalt prepared in Example 1 after heat aging and ultraviolet aging respectively;
[0032] Figure 7 This is a comparison chart of the humidity-induced shear thinning index of the bio-based rubber asphalt prepared in Example 1 and the rubber asphalt after thermal aging and ultraviolet aging, respectively. DETAILED DESCRIPTION
[0033] The technical solution protected by the present invention is described in detail below with reference to the accompanying drawings. Although the accompanying drawings show specific embodiments of the present invention, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein.
[0034] The present invention provides a method for preparing an anti-aging bio-based rubber asphalt material, comprising the following steps:
[0035] S1. Rubber powder and bio-oil are mixed in a mass ratio of 1:(0.5-1.5), and stirred evenly under heating conditions to prepare substance A.
[0036] In the present invention, the mass ratio of rubber powder to bio-oil is 1:0.5, 1:0.8, 1:1.0, 1:1.2 or 1:1.5.
[0037] In step S1 of the present invention, the main chemical components of the bio-oil are hexanal, methyl heptanoate, methyl hexanoate, methyl octanoate, 1,2,3,4-tetramethylbenzene, 1-pentanol, valeraldehyde, 2-heptanone, methyl salicylate and 1-octene.
[0038] The contents of the main components of bio-oil are shown in Table 1.
[0039] Table 1 Main components of bio-oil (based on GC-MS)
[0040] chemical composition Chemical formula percentage Molecular weight (amu) <![CDATA[Polarizability (Bohr 3 )]]> Hexanal <![CDATA[C6H 12 The]]> 16.97% 100.089 78.54 Methyl heptanoate <![CDATA[C8H 16 O2]]> 13.31% 144.115 106.71 Methyl hexanoate <![CDATA[C7H 14 O2]]> 9.59% 130.099 94.15 Methyl octanoate <![CDATA[C9H 18 O2]]> 6.75% 158.131 119.33 1,2,3,4-Tetramethylbenzene <![CDATA[C 10 H 14 ]]> 4.87% 134.11 118.38 1-Pentanol <![CDATA[C5H 12 The]]> 4.86% 88.089 69.13 Valeraldehyde <![CDATA[C5H 10 The]]> 4.59% 86.073 66.05 2-Heptanone <![CDATA[C7H 14 The]]> 3.22% 114.104 89.88 Methyl salicylate <![CDATA[C8H8O3]]> 3.11% 152.047 105.31 1-Octene <![CDATA[C8H 16 ]]> 1.85% 112.125 101.76
[0041] The rubber powder in step S1 of the present invention is obtained by grinding waste tires into particles by mechanical grinding at room temperature, and the particle size of the rubber powder is 0.18 mm to 0.25 mm.
[0042] Preferably, the particle size of the rubber powder is 0.18 mm, 0.2 mm or 0.25 mm.
[0043] In step S1 of the present invention, the heating temperature is 100° C. to 150° C., and the stirring time is 30 min to 60 min.
[0044] In the present invention, the heating temperature is 100° C., 110° C., 120° C., 125° C., 130° C., 140° C. or 150° C., and the stirring time is 30 min, 40 min, 45 min, 50 min or 60 min.
[0045] S2. Expand the substance A in step S1 at room temperature to prepare a bio-based expanded rubber.
[0046] In step S2 of the present invention, the expansion time is 6 hours to 18 hours.
[0047] In the present invention, the expansion time is 6h, 7h, 8h, 9h, 10h, 12h, 15h or 18h
[0048] S3, expanding the bioexpanded rubber prepared in step S2 under microwaves to obtain bio-based modified rubber.
[0049] In step S3 of the present invention, the power of the microwave is 300W to 500W, the frequency of the microwave is 2000MHz to 3000MHz, and the expansion time is 2min to 8min.
[0050] In the present invention, the power of the microwave is 300W, 350W, 400W, 450W or 500W, the frequency of the microwave is 2000MHz, 2200MHz, 2400MHz, 2450MHz, 2500MHz, 2600MHz, 2800MHz or 3000MHz, and the expansion time is 2min, 3min, 5min, 6min or 8min.
[0051] S4. Add the bio-based modified rubber of step S3 to the base asphalt, wherein the mass of the bio-based modified rubber added is 10% to 20% of the mass of the base asphalt, and then stir and react under heating conditions to obtain an anti-aging bio-based rubber asphalt material.
[0052] In the present invention, the mass of the bio-based modified rubber added is 10%, 12%, 14%, 15%, 16%, 18% or 20% of the mass of the base asphalt.
[0053] In step S4 of the present invention, the heating temperature is 150° C. to 200° C., and the stirring time is 10 min to 50 min.
[0054] In the present invention, the heating temperature is 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, and the stirring time is 10 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min or 50 min.
[0055] The technical advantages of the anti-aging bio-based rubber asphalt material prepared by the present invention are described below through several groups of implementation methods and performance tests.
[0056] It should be noted that, unless otherwise specified, the reagents, drugs, instruments, etc. used in the following examples are all conventional products in the field purchased from the market.
[0057] Example 1
[0058] The method for preparing the anti-aging bio-based rubber asphalt material provided in this embodiment comprises the following steps:
[0059] S1. Mix rubber powder and bio-oil in a mass ratio of 1:0.5, stir at 150° C. for 30 min, and prepare substance A.
[0060] S2. Expand the substance A prepared in step S1 at room temperature for 12 hours to prepare a bio-based expanded rubber (denoted as BS).
[0061] S3. Expand the bio-expanded rubber in step S2 by microwave at a power of 400 W (frequency of 2450 MHz) for 5 min to prepare bio-based modified rubber (BM).
[0062] S4. Add bio-based modified rubber (BM) into base asphalt at a mass fraction of 15%, stir at 170° C. for 45 minutes to obtain an anti-aging bio-based rubber asphalt material.
[0063] The specific steps are: crush the bio-based modified rubber into small particles, add them to the liquefied base asphalt, mix them at 170°C with a desktop shear mixer at a speed of 3000r / min for 45 minutes, so that the bio-based modified rubber is evenly dispersed in the base asphalt to prepare an anti-aging bio-based rubber asphalt material.
[0064] In this embodiment, the bio-oil is derived from soybean oil collected from the catering service industry, and its performance meets the requirements of Table 1; the rubber powder is obtained by grinding waste tires at room temperature using a mechanical grinding method, and its particle size range is 0.18 mm to 0.25 mm.
[0065] In this embodiment, the base asphalt is No. 70 petroleum asphalt produced in the Middle East.
[0066] Example 2
[0067] The method for preparing the anti-aging bio-based rubber asphalt material provided in this embodiment comprises the following steps:
[0068] S1. Mix rubber powder and bio-oil in a mass ratio of 1:1, stir at 135° C. for 30 min, and prepare substance A.
[0069] S2. Expand the substance A prepared in step S1 at room temperature for 12 hours to prepare a bio-based expanded rubber (denoted as BS).
[0070] S3. Expand the bio-expanded rubber in step S2 by microwave at a power of 400 W (frequency of 2450 MHz) for 4 min to prepare bio-based modified rubber (BM).
[0071] S4. Add bio-based modified rubber (BM) into base asphalt at a mass fraction of 15%, stir at 170° C. for 45 minutes to obtain an anti-aging bio-based rubber asphalt material.
[0072] In this example, the sources and properties of soybean oil, rubber powder and base asphalt are referred to Example 1.
[0073] Example 3
[0074] The method for preparing the anti-aging bio-based rubber asphalt material provided in this embodiment comprises the following steps:
[0075] S1. Mix rubber powder and bio-oil in a mass ratio of 1:1.5, stir at 135° C. for 30 min, and prepare substance A.
[0076] S2. Expand the substance A prepared in step S1 at room temperature for 12 hours to prepare a bio-based expanded rubber (denoted as BS).
[0077] S3. Expand the bio-expanded rubber in step S2 by microwave at a power of 400 W (frequency of 2450 MHz) for 4 min to prepare bio-based modified rubber (BM).
[0078] S4. Add bio-based modified rubber (BM) into base asphalt at a mass fraction of 15%, stir at 170° C. for 45 minutes to obtain an anti-aging bio-based rubber asphalt material.
[0079] In this example, the sources and properties of soybean oil, rubber powder and base asphalt are referred to Example 1.
[0080] Example 4
[0081] The method for preparing the anti-aging bio-based rubber asphalt material provided in this embodiment comprises the following steps:
[0082] S1. Mix rubber powder and bio-oil in a mass ratio of 1:1, stir at 135° C. for 30 min, and prepare substance A.
[0083] S2. Expand the substance A prepared in step S1 at room temperature for 12 hours to prepare a bio-based expanded rubber (denoted as BS).
[0084] S3. Expand the bio-expanded rubber in step S2 by microwave at a power of 400 W (frequency of 2450 MHz) for 4 min to prepare bio-based modified rubber (BM).
[0085] S4. Add bio-based modified rubber (BM) into base asphalt at a mass fraction of 10%, stir at 170° C. for 45 minutes to obtain an anti-aging bio-based rubber asphalt material.
[0086] In this example, the sources and properties of soybean oil, rubber powder and base asphalt are referred to Example 1.
[0087] Example 5
[0088] The method for preparing the anti-aging bio-based rubber asphalt material provided in this embodiment comprises the following steps:
[0089] S1. Mix rubber powder and bio-oil in a mass ratio of 1:1, stir at 135° C. for 30 min, and prepare substance A.
[0090] S2. Expand the substance A prepared in step S1 at room temperature for 12 hours to prepare a bio-based expanded rubber (denoted as BS).
[0091] S3. Expand the bio-expanded rubber in step S2 by microwave at a power of 400 W (frequency of 2450 MHz) for 4 min to prepare bio-based modified rubber (BM).
[0092] S4. Add bio-based modified rubber (BM) into base asphalt at a mass fraction of 20%, stir at 170° C. for 45 minutes to obtain an anti-aging bio-based rubber asphalt material.
[0093] In this example, the sources and properties of soybean oil, rubber powder and base asphalt are referred to Example 1.
[0094] In order to illustrate the performance of the anti-aging bio-based modified rubber asphalt material prepared by the present invention, the following test was conducted.
[0095] It should be noted that in the following tests, rubber asphalt (CRM) was prepared by mixing 15% unmodified rubber with base asphalt using a benchtop shear mixer at 3000 r / min and 180°C for 30 minutes. Bio-based asphalt (BOA) was prepared by mixing 7.5% bio-oil with base asphalt binder using a benchtop shear mixer at 3000 r / min and 180°C for 30 minutes.
[0096] Test 1
[0097] The purpose of this experiment is to optimize the rubber to bio-oil mass ratio and the added mass of bio-based modified rubber through experimental tests.
[0098] 1. Take the anti-aging bio-based modified rubber asphalt materials prepared in Examples 1 to 3 to conduct aging performance tests.
[0099] The specific test method is: three anti-aging bio-based modified rubber asphalt materials are subjected to thermal oxidation aging T40 and ultraviolet aging U150 respectively. Thermal oxidation aging T40 is to pour the sample into a glass jar and place it in an oven at a temperature of 163°C for 85 minutes; then 50g of the sample is placed in a container with high pressure (2070kPa) and high temperature (100°C) for 40h; ultraviolet aging U150 is to place a 30g disc-shaped sample (diameter 140mm) at a distance of 40cm from the ultraviolet lamp, the temperature is 60°C, the ultraviolet lamp power is 300W, the wavelength is 200nm~400nm, and the sample is subjected to ultraviolet irradiation for 150h. The carbonyl (ICO) content and sulfoxide (ISO) content in the aging product are determined for the aged materials, and the results are shown in Table 2.
[0100] Table 2 Comparison of aging products in different embodiments
[0101]
[0102] The experimental results in Table 2 show that the higher the proportion of bio-oil, the fewer aging products are produced after aging. The possible reason is that bio-oil replenishes the components lost by asphalt after aging and enhances the colloidal stability of asphalt during aging. However, adding too much bio-oil will lead to a decrease in the high-temperature performance of asphalt. Therefore, a 1:1 ratio of rubber to bio-oil is more appropriate.
[0103] 2. Take the anti-aging bio-based modified rubber asphalt materials prepared in Example 1, Example 4 and Example 5 to perform composite shear modulus performance test.
[0104] The bio-based rubber asphalt materials obtained under three different mass fractions of bio-based rubber were subjected to short-term aging. The short-term aging was carried out using a rotating thin film oven test (RTFO). Specifically, the samples were poured into a glass jar and placed in an oven at 163°C for 85 minutes. After the short-term aging was completed, the composite shear modulus of the anti-aging bio-based modified rubber asphalt materials before and after short-term aging was measured, and the results are shown in Table 3.
[0105] Table 3 Composite shear modulus of different embodiments before and after aging
[0106]
[0107] It can be seen from Table 3 that rubber absorbs light components in asphalt to expand, thereby improving the high and low temperature capabilities of asphalt; bio-oil can supplement light components for asphalt and improve the low temperature and anti-aging capabilities of asphalt; with the increase of bio-based modified rubber parameters, the content of rubber and bio-oil also increases. When the bio-based modified rubber is less, the rubber in the asphalt is not enough to completely absorb the expansion, and the performance improvement is limited; with the increase of the amount of addition, the performance of bio-based modified rubber asphalt materials is gradually improving, but when the bio-oil content exceeds a certain amount, the rubber is not enough to completely absorb the light components in the asphalt, and the excess bio-oil dissociates in the asphalt system, thereby reducing the stiffness of the asphalt and affecting the high temperature performance of the asphalt. Therefore, a bio-based modified rubber with a mass fraction of 15% is selected to be mixed into the matrix asphalt to ensure that the final asphalt material has excellent performance.
[0108] Test 2
[0109] Sample: the anti-aging bio-based modified rubber asphalt material (denoted as BMR) of Example 2, rubber asphalt (CRM).
[0110] Test method: The aging comparison of the above samples was carried out according to the following method.
[0111] (1) The sample was not subjected to any aging treatment (denoted as Unaged).
[0112] (2) Thermal aging: Short-term aging is carried out using a rotating thin film oven test (RTFO), in which the sample is poured into a glass jar and placed in an oven at 163°C for 85 min. Long-term aging is carried out using a pressure aging test (PAV), in which 50 g of the sample is placed in a container at high pressure (2070 kPa) and high temperature (100°C) for 20 h (denoted as T20) and 40 h (denoted as T40).
[0113] (3) Ultraviolet aging: A 30 g disc-shaped sample (diameter 140 mm) was placed 40 cm away from a UV lamp at a temperature of 60°C. The UV lamp power was 300 W and the wavelength was 200 nm to 400 nm. The sample was subjected to ultraviolet irradiation for 50 h (denoted as U50) and 150 h (denoted as U150).
[0114] The carbonyl content and sulfoxide content in the aged samples were tested respectively. The test results are as follows: Figure 1 As shown, (a) is the comparison result of carbonyl (ICO) content; (b) is the comparison result of sulfoxide (ISO) content.
[0115] See also Figure 1 , after comparing the carbonyl (ICO) content and sulfoxide (ISO) content data after 40h thermal aging or 150h UV aging, it was found that after different aging methods, it can be proved that the aging products of bio-based rubber asphalt are lower than those of ordinary rubber asphalt. And the CRM and BMR after UV aging showed that the ICO and ISO values were larger, indicating that the samples had thermal oxidation aging during UV aging (U50 and U150). When analyzing the aging of U50 and U150, the increase of ICO and ISO of CRM was significantly slowed down, while the ICO and ISO of BMR continued to increase. According to previous studies, when the number of carboxylic acids is stable, the reactive compounds are exhausted during the aging process, followed by the loss and hardening of volatile small molecules. This proves the efficacy of bio-oil in delaying the aging process of BMR exposed to thermal oxidation and UV radiation. At the same time, compared with CRM, the ICO and ISO values of BMR at various stages of thermal aging and UV aging are smaller, indicating that BMR has better resistance to thermal aging and UV aging. After U50 aging, the results of ICO showed that the formation of carbonyl groups during thermal aging was reduced by 36% due to the addition of bio-oil. This may be related to the highly reactive components (BO2, BO3 and BO4) in bio-oil, which are the main targets of oxidative attack and delay the formation of carbonyl groups. At the same time, compared with CRM, the ISO of BMR after thermal aging is 33% lower on average, indicating that the bio-oil in BMR is effective in enhancing resistance to thermal oxidative aging. This indicates that bio-oil inhibits the formation of aging products, and it is found that bio-based rubber asphalt shows a more obvious anti-aging behavior after aging.
[0116] Test 3
[0117] Samples: the anti-aging bio-based modified rubber asphalt material (denoted as BMR) of Example 2, rubber asphalt (CRM), and bio-based asphalt (BOA).
[0118] Test method: Use the method in Test 1 to age the samples separately.
[0119] In this example, mixed aging (ie, TU aging) was also performed, which included short-term aging rotating thin film oven test (RTFOT) and 50 h ultraviolet aging (U50).
[0120] The surface morphology of the materials was obtained by atomic force microscopy (AFM) imaging of the aged samples in each group, and the evolution of the aging factors, the changes in the honeycomb structure, and the changes in the corresponding domains on the phase diagram during the aging process of the three samples were observed, thus proving that BMR has good anti-aging ability. Figure 2 shown.
[0121] See also Figure 2 , the morphology and phase images of bio-based rubber asphalt (BMR), rubber asphalt (CRM), and bio-based asphalt (BOA) before and after aging. When bio-based rubber is added, the stability of BMR after heat aging and UV aging is increased by 70% and 21% respectively compared with rubber asphalt and bio-based asphalt; At the same time, atomic force microscopy-infrared spectroscopy (AFM-IR) observations show that the carbonyl component generation of rubber asphalt is reduced after adding bio-based rubber, thereby reducing the aging index. This shows that bio-based rubber effectively improves the anti-aging ability of rubber asphalt.
[0122] Test 4
[0123] Sample: the anti-aging bio-based modified rubber asphalt material (denoted as BMR) of Example 2, rubber asphalt (CRM).
[0124] Test method: (1) The samples were subjected to heat aging for 20 h (T20), heat aging for 40 h (T40), UV aging for 50 h (U50) and UV aging for 150 h (U150) according to the method of Test 1; (2) The effects of thermal oxidative aging and UV aging on the structural changes of the two materials were evaluated by UV-visible absorption spectroscopy, and the UV-visible absorption spectra in the range of 300 nm-800 nm were collected using a Cary 6000i UV-Vis-NIR spectrophotometer.
[0125] The spectra were obtained after centrifugation of the samples to reduce the influence of rubber crumbs and certain particles in the bio-oil. The visible light (400nm-700nm) and ultraviolet (300nm-400nm) absorption (R' Vis / UV ) to evaluate the aging of the sample; the agglomeration index is calculated using the following formula to indicate resistance to thermal oxidation and ultraviolet aging.
[0126]
[0127] Where: R′ Vis / UV is the ratio of visible light absorption to ultraviolet light absorption under different aging conditions, R Vis / UVis the ratio of visible light absorption to ultraviolet absorption of the unaged sample; the test results are as follows Figure 3 shown.
[0128] See also Figure 3 , the agglomeration index of bio-based rubber asphalt and rubber asphalt under different aging conditions, indicating the effectiveness of bio-oil in resisting the agglomeration behavior of aromatic compounds, proving its anti-aging ability. The test found that the softening and de-agglomeration ability of bio-oil compensated for the evolution of components in the asphalt binder caused by aging, so that BMR maintained a 43% lower aggregation index based on UV-visible absorption spectrum, and the growth of medium molecular size content was reduced by 22%, which shows that bio-based can well resist the aging of rubber asphalt and improve the anti-aging ability of rubber asphalt.
[0129] Test 5
[0130] Sample: the anti-aging bio-based modified rubber asphalt material (denoted as BMR) of Example 2, rubber asphalt (CRM).
[0131] Test method: First, age the sample according to the method of test 1, and then each aged sample is tested for healing using an Anton Parr SmartPave-102 dynamic shear rheometer. At 25°C, an 8mm plate with a 2mm gap is used to evaluate its healing ability at a strain rate of 5% and a frequency of 10Hz. When the complex shear modulus of the specimen drops to 50% of the initial value, loading is stopped. After healing for 900s, loading is resumed to measure the recovered modulus; at least three repeated tests are prepared for each test. The healing index (HI) is calculated using the following formula:
[0132]
[0133] Where: G0 is the initial modulus, Ga is 50% of the initial modulus, and Gb is the modulus after healing for 900s.
[0134] The healing index results of samples after different aging are as follows: Figure 4 shown.
[0135] See also Figure 4 The self-healing properties of asphalt were compared between bio-based rubber asphalt and rubber asphalt under different aging conditions. It was found that the self-healing ability of bio-based rubber asphalt was 84% and 106% higher than that of ordinary rubber after thermal aging and ultraviolet aging, respectively. This shows that bio-based can not only delay the aging rate of rubber asphalt, but also maintain the good self-healing ability of rubber asphalt; it shows that bio-oil also plays a great role in improving the self-healing ability of asphalt.
[0136] Test 6
[0137] Sample: the anti-aging bio-based modified rubber asphalt material (denoted as BMR) of Example 2, rubber asphalt (CRM).
[0138] Test method: First, age the samples according to the method of test 1, and then use a dynamic shear rheometer (SmartPave-102, Anton Parr) to evaluate the cohesive properties of each aged sample. At temperatures of 16°C, 10°C, and 4°C, use an 8mm parallel plate with a gap of 2mm to perform a frequency scan from 0.1rad / s to 100rad / s to obtain the master curves of the storage and loss modulus at the corresponding temperature. The crossover frequency and crossover modulus are obtained at the intersection of the storage modulus G' master curve and the loss modulus G" master curve. These two variables were used to observe the changes in the colloid structure during the thermal oxidation aging and ultraviolet aging process. The results are as follows: Figure 5 As shown, the figure shows the cross modulus of the two modified asphalts; (a) is a comparison of the cross modulus of bio-based rubber asphalt and rubber asphalt after thermal aging; (b) is a comparison of the cross modulus of bio-based rubber asphalt and rubber asphalt after ultraviolet aging.
[0139] See also Figure 5 It was found that compared with ordinary rubber asphalt, the cross-modulus of bio-based rubber asphalt after thermal aging was 393% higher and the cross-modulus after UV aging was 128% higher, indicating that the deaggregation ability of bio-based rubber asphalt led to better cohesion and delayed the aging rate of rubber asphalt.
[0140] Test 7
[0141] Sample: the anti-aging bio-based modified rubber asphalt material (denoted as BMR) of Example 2, rubber asphalt (CRM).
[0142] Test Method: The samples were aged as described in Test 1, and then each aged sample was tested as follows. The specific test process was as follows: Silica glass slides were sterilized in acetone, isopropanol, and water, then sonicated for 10 min each, and then dried with nitrogen; the slides were then placed in UV ozone for 15 min to ensure removal of any monolayer; within one hour after cleaning, 15 mg of each binder was placed on the slide and placed in an oven at 150 ° C for 30 min to ensure proper coating, and then annealed at ambient temperature for 1 h. The prepared specimens were left overnight before measuring the contact angle at ambient temperature. For water conditioning, the samples were placed in a deionized water vial containing 5 mL of water and placed at 80 ° C for 2 h, and then the vial was immersed in a deionized water bath at ambient temperature for 5 min. The vial was then dried with gas. Each sample was then imaged at ambient temperature using an SL200 KS contact angle goniometer. 12 readings were collected for unconditioned (dry) and conditioned (wet) specimens. The contact angle moisture sensitivity index (CAMSI) was calculated using the following formula.
[0143]
[0144] The test results are as follows Figure 6 As shown; (a) is the comparison of CAMSI results after thermal oxidation aging, and (b) is the comparison of CAMSI results after ultraviolet aging.
[0145] See also Figure 6 The contact angle moisture sensitivity index of bio-based rubber asphalt and rubber asphalt after heat aging and UV aging respectively can be found that compared with the contact angle moisture sensitivity index (CAMSI) value of ordinary rubber asphalt, the CAMSI value of bio-based rubber asphalt after heat aging is 88% lower and 69% lower after UV aging, indicating that bio-based rubber asphalt has a higher affinity for the surface of siliceous stone. This shows that after aging, asphalt will reduce adhesion to aggregates, which is manifested as increased contact angle moisture sensitivity; the contact angle of rubber asphalt with added bio-oil increases very little after aging, indicating that bio-oil effectively slows down the aging rate of asphalt.
[0146] Test 8
[0147] Sample: the anti-aging bio-based modified rubber asphalt material (denoted as BMR) of Example 2, rubber asphalt (CRM).
[0148] Test method: First, the samples were aged according to the method of test 1, and then each aged sample was observed by frequency sweep test. The test process is: glass beads (diameter 100μm) and asphalt binder were mixed in a weight ratio of 1:2 to simulate the interface between asphalt binder and aggregate. Then 0.3g of the sample was placed in the 8mm parallel plate of the dynamic shear rheometer and frequency sweep test (0.1rad / s-100rad / s) was performed at various temperatures (the sample test temperatures corresponded to CRM~65℃, CRM-T20~72℃, CRMT40~80℃, CRM-U50~72℃, CRMU150~72℃ and BMR~58℃, BMR-T20~62℃, BMR-T40~65℃, BMR-U50~60℃ and BMR-U150~60℃). After the test, the test temperature was selected to maintain a viscosity of 1 Pa.s of the sample, which is the optimal initial viscosity to observe shear thinning behavior; a power law equation was fitted to the shear thinning region of the viscosity-shear rate curve to calculate the thinning slope.
[0149] During the test, six specimens were prepared for each type of asphalt binder: three specimens were tested without water treatment, and the other three specimens were water treated at 60°C for 24 hours; all specimens were surface dried before the MISTI test; the humidity-induced shear thinning index MISTI and viscosity were calculated using the following two formulas.
[0150]
[0151] The test results are as follows Figure 7 As shown, where: (a) is a comparison of thermal oxygen aging results, and (b) is a comparison of ultraviolet aging results.
[0152] See also Figure 7 , observed the moisture-induced shear thinning index of bio-based rubber asphalt and rubber asphalt after heat aging and UV aging, as well as the adhesion performance of the two asphalts to siliceous aggregates after aging, and found that bio-based rubber asphalt has stronger moisture resistance, which in turn indicates that its adhesion performance is better after aging, effectively proving that bio-oil rubber asphalt has better anti-aging ability; In addition, it was found that UV aging caused the acid value of ordinary rubber asphalt to increase more than that of bio-based rubber asphalt, and the acidic substances weakened the adhesion to the surface of siliceous stone and increased the sensitivity of the road surface to moisture. After UV aging, the moisture-induced shear thinning index (MISTI) of ordinary rubber asphalt increased by 23.19%, while the thinning index (MISTI) of bio-based rubber asphalt only increased by 9.21%, which further indicates that the presence of bio-based can effectively improve the anti-aging ability of rubber asphalt.
[0153] In summary, the bio-based modified rubber asphalt material prepared by the present invention can greatly improve the anti-aging ability of the base asphalt, and the bio-based modified rubber can inhibit the generation of aging products in the asphalt material, thereby reducing the degradation of the mechanical properties of the rubber asphalt after thermal oxidation and ultraviolet aging, and delaying the occurrence and development of pavement diseases; it can also improve the rheological properties and asphalt-aggregate interface strength of the rubber asphalt after aging, and improve the long-term pavement service performance of the rubber asphalt. Through the verification of the present invention, it is found that the bio-based rubber asphalt has a lower aging index than the rubber asphalt after aging, stronger self-healing ability, stronger cohesion, higher affinity with the surface of siliceous stone, and stronger anti-aging ability.
[0154] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing an anti-aging bio-based rubber asphalt material, characterized in that: The following steps are involved: S1. Mix rubber powder and bio-oil in a mass ratio of 1:(0.5-1.5), and stir evenly under heating conditions to prepare substance A; S2, expanding the substance A in step S1 at room temperature to prepare a bio-based expanded rubber; S3, expanding the bio-expanded rubber prepared in step S2 under microwaves to prepare a bio-based modified rubber; S4. Add the bio-based modified rubber of step S3 to the base asphalt, wherein the mass of the bio-based modified rubber added is 10% to 20% of the mass of the base asphalt, and then stir and react under heating conditions to obtain an anti-aging bio-based rubber asphalt material.
2. The method for preparing the anti-aging bio-based rubber asphalt material according to claim 1, characterized in that: In step S1, the main chemical components of the bio-oil are hexanal, methyl heptanoate, methyl hexanoate, methyl octanoate, 1,2,3,4-tetramethylbenzene, 1-pentanol, valeraldehyde, 2-heptanone, methyl salicylate and 1-octene.
3. The method for preparing the anti-aging bio-based rubber asphalt material according to claim 1, characterized in that: The rubber powder in step S1 is obtained by grinding waste tires into particles by mechanical grinding at room temperature, and the particle size of the rubber powder is 0.18 mm to 0.25 mm.
4. The method for preparing the anti-aging bio-based rubber asphalt material according to claim 1, characterized in that: In the step S1, the heating temperature is 100° C. to 150° C., and the stirring time is 30 min to 60 min.
5. The method for preparing the anti-aging bio-based rubber asphalt material according to claim 1, characterized in that: In step S2, the expansion time is 6 hours to 18 hours.
6. The method for preparing the anti-aging bio-based rubber asphalt material according to claim 1, characterized in that: In step S3, the power of the microwave is 300W to 500W, the frequency of the microwave is 2000MHz to 3000MHz, and the expansion time is 2min to 8min.
7. The method for preparing the anti-aging bio-based rubber asphalt material according to claim 1, characterized in that: In the step S4, the heating temperature is 150° C. to 200° C., and the stirring time is 10 min to 50 min.
8. The anti-aging bio-based rubber asphalt material prepared by the method for preparing the anti-aging bio-based rubber asphalt material according to any one of claims 1 to 7.
9. Use of the anti-aging bio-based rubber asphalt material as claimed in claim 8 in pavement engineering.
Citation Information
Cited By
High-dosage bio-oil activated rubber powder modified asphalt as well as preparation method and production system thereof
CN120248639A
A high-content bio-oil activated rubber powder modified asphalt and its preparation method and production system