Composite powder for semiconductor graphite material surface coating and preparation method thereof
The niobium carbide-coated graphite composite powder prepared by ball milling and spray granulation processes solves the problem of poor anti-corrosion coating bonding performance of graphite material surface under plasma spraying method, achieves uniform distribution and excellent bonding performance, and is suitable for semiconductors Field of protective coatings for graphite materials.
Patent Information
- Application Number
- CN202411144756.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to efficiently prepare anti-corrosion composite coatings on the surface of semiconductor graphite materials through plasma spraying, and the coating bonding performance is poor, and the large difference in thermal expansion coefficient leads to the coating being easily shedded.
Ball milling and spray granulation processes are used to prepare niobium carbide-coated graphite composite powder, combined with magnetic stirring and sintering treatment, composite powder with particle size of 30-70μm is produced, which is used for plasma spraying to prepare the surface protective coating of graphite material.
Achieve uniform distribution and good fluidity of composite powder, avoid high-temperature oxidation and decomposition, provide uniform composition performance and excellent binding performance, and is suitable for the anti-corrosion coating of graphite materials in the semiconductor field, reducing the risk of coating peeling .
Smart Images

Figure CN118931234A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor graphite material protection, and more specifically, to a composite powder for semiconductor graphite material surface coating and a preparation method thereof. Background Art
[0002] Graphite materials are widely used in the semiconductor industry, such as in the field of epitaxial growth of semiconductor crystal materials and integrated circuit manufacturing equipment. The operating conditions for manufacturing semiconductor crystal materials and integrated circuit core manufacturing equipment are mostly high temperature, plasma corrosive environments. Graphite in such an environment is prone to corrosion failure and will affect the purity of the prepared semiconductor materials or the quality of the integrated circuits. Therefore, a protective coating needs to be prepared on the surface of the graphite material.
[0003] NbC has excellent high-temperature chemical stability and corrosion resistance, and can protect graphite materials in high-temperature and corrosive environments. Currently, PVD and CVD vapor deposition methods are widely used to prepare a layer of NbC coating on the surface of graphite materials, but the preparation efficiency is not high. The plasma spraying method has high coating preparation efficiency, but since NbC materials are easily decomposed at high temperatures, the coating bonding performance is very poor. Therefore, it is impossible to use the plasma spraying method and pure NbC powder to prepare an effective protective coating. In addition, the thermal expansion coefficients of NbC and graphite differ by half, and the thermal stress is large and the coating is easy to fall off. Therefore, it is necessary to develop a protective composite coating with a small difference in thermal expansion coefficient on the surface of graphite materials that can be efficiently prepared by plasma spraying. However, there is currently no suitable composite powder for plasma spraying on the surface of graphite materials to prepare protective composite coatings.
[0004] Therefore, how to prepare a composite powder suitable for plasma spraying to prepare an anti-corrosion composite coating on the surface of graphite materials used in the semiconductor field has become a technical problem that urgently needs to be solved. Summary of the invention
[0005] In view of the shortcomings of the prior art, the object of the present invention is to provide a composite powder suitable for preparing an anti-corrosion composite coating on the surface of a graphite material for use in the semiconductor field by plasma spraying and a preparation method thereof.
[0006] The above technical objectives of the present invention are achieved through the following technical solutions: A method for preparing composite powder for surface coating of semiconductor graphite material, comprising the following steps:
[0007] (1) adding niobium carbide raw material powder into a planetary ball mill and performing ball milling using niobium carbide abrasive;
[0008] (2) adding graphite powder in an amount of 10wt.% to 50wt.% of the total mass of the composite powder, and adding an organic adhesive, and continuing ball milling;
[0009] (3) using centrifugal spray granulation equipment to make granulated powder from the slurry;
[0010] (4) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 30-60 μm;
[0011] (5) heating and sintering the granulated powder obtained by screening in a heating furnace;
[0012] (6) The sintered powder is vibrated and sieved to obtain a niobium carbide-coated graphite composite powder with a particle size of 20-50 μm;
[0013] (7) adding niobium carbide coated graphite composite powder to niobium powder and an organic adhesive, and using magnetic stirring to prepare a slurry with a solid content of 40 wt.% to 70 wt.%;
[0014] (8) using a centrifugal spray granulation device to prepare a granulated powder from the slurry;
[0015] (9) Screening the granulated powder using a vibrating screen to obtain a granulated powder with a particle size of 40-80 μm;
[0016] (10) heating and sintering the granulated powder obtained by screening in a heating furnace;
[0017] (11) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 30-70 μm for plasma spraying to prepare a surface protective coating of graphite materials for use in the semiconductor field.
[0018] The present invention is further configured as follows: in step (1), the particle size of the niobium carbide raw material powder is 30-50 μm.
[0019] The present invention is further configured as follows: in step (1), the ball milling is carried out in an argon atmosphere for 20-40 hours, and the particle size of the niobium carbide after ball milling is 30-90 nm.
[0020] The present invention is further configured as follows: in step (2), the particle size of the graphite powder is 30-80 μm.
[0021] The present invention is further configured as follows: in step (2), ball milling is performed for 2-5 hours to obtain a slurry with a solid content of 40wt.%-70wt.%.
[0022] The present invention is further configured as follows: in step (3), the spray granulation process parameters are: inlet temperature 200-400°C, outlet temperature 150-200°C, feed pump speed 600-1000r / min, atomizer speed 5000-7000r / min.
[0023] The present invention is further configured as follows: in step (5), the sintering temperature is 200-250°C.
[0024] The present invention is further configured as follows: in step (7), the particle size of the niobium carbide coated graphite composite powder is 20-50 μm, the particle size of the niobium powder is 20-70 nm, and the added amount is 5wt.% to 20wt.% of the total mass of the composite powder.
[0025] The present invention is further configured as follows: in step (8), the spray granulation process parameters include an inlet temperature of 200-300° C., an outlet temperature of 150-200° C., a feed pump speed of 600-1000 r / min, and an atomizer speed of 5000-7000 r / min.
[0026] The present invention also provides a composite powder for semiconductor graphite material surface coating, which is obtained through the above preparation process.
[0027] In summary, the present invention has the following beneficial effects: the present invention uses micron-sized niobium carbide and micron-sized graphite powder as raw materials, prepares precursor powder of a certain particle size by ball milling and spray granulation, and then prepares niobium carbide-coated graphite composite powder by sintering and screening methods; then, the niobium carbide-coated graphite composite powder and nano-sized niobium powder are mixed by magnetic stirring slurrying and spray granulation to prepare precursor powder of a certain particle size, and then prepares composite powders of graphite / niobium carbide / niobium from the inside to the outside by sintering and screening methods. Compared with mechanically mixed powder materials, the composite powder material prepared by the method has uniform distribution of components, suitable bulk density and good fluidity, and can avoid oxidative decomposition of graphite and niobium carbide at high temperature, and can be used for plasma spraying to prepare anti-corrosion composite coatings on the surface of graphite materials for semiconductor fields, and the prepared coating has the advantages of uniform composition performance, excellent bonding performance, small difference in thermal expansion coefficient with the graphite substrate, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a SEM photograph of the appearance of the composite powder obtained by the processing of the present invention. DETAILED DESCRIPTION
[0029] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.
[0030] The object of the present invention is to provide a composite powder suitable for preparing a graphite material surface anti-corrosion composite coating for use in the semiconductor field by plasma spraying and a preparation method thereof.
[0031] The invention uses micron-grade niobium carbide and micron-grade graphite powder as raw materials, prepares precursor powder of a certain particle size by ball milling and spray granulation, and then prepares niobium carbide-coated graphite composite powder by sintering and screening methods; then, the niobium carbide-coated graphite composite powder and nano-grade niobium powder are mixed by magnetic stirring slurrying and spray granulation to prepare precursor powder of a certain particle size, and then prepares composite powder of graphite / niobium carbide / niobium from the inside to the outside by sintering and screening methods. Compared with mechanically mixed powder materials, the composite powder material prepared by the method has uniform distribution of components, suitable bulk density and good fluidity, and can avoid oxidative decomposition of graphite and niobium carbide at high temperature, and can be used for plasma spraying to prepare anti-corrosion composite coating on the surface of graphite material for semiconductor field, and the prepared coating has the advantages of uniform component performance, excellent bonding performance, small difference in thermal expansion coefficient with graphite substrate, and has good application prospect.
[0032] The composite powder provided by the present invention is suitable for preparing the anti-corrosion composite coating on the surface of the graphite material for the semiconductor field by plasma spraying and the preparation method thereof comprises the following steps:
[0033] (1) Add niobium carbide raw material powder (particle size: 30-50 μm) into a planetary ball mill, use niobium carbide abrasive, and ball mill for 20-40 hours in an argon atmosphere. After ball milling, the particle size of niobium carbide is 30-90 nm.
[0034] (2) adding graphite powder (particle size: 30-80 μm) in an amount of 10 wt.%-50 wt.% of the total mass of the powder, and adding an organic adhesive, and continuing ball milling for 2-5 hours to obtain a slurry with a solid content of 40 wt.%-70 wt.%.
[0035] (3) Use centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size.
[0036] Spray granulation process parameters: inlet temperature 200-400℃, outlet temperature 150-200℃, feed pump speed 600-1000r / min, atomizer speed 5000-7000r / min.
[0037] (4) The granulated powder is sieved using a vibrating screen to obtain a granulated powder with a particle size of 30-60 μm.
[0038] (5) The granulated powder obtained by screening is heated and sintered in a heating furnace at a sintering temperature of 200-300°C.
[0039] (6) The sintered powder is vibrated and sieved to obtain niobium carbide-coated graphite composite powder with a particle size of 20-50 μm.
[0040] (7) Niobium carbide coated graphite composite powder (particle size of 20-50 μm) and niobium powder (particle size of 20-70 nm, added in an amount of 5wt.%-20wt.% of the total mass of the powder) are mixed with an organic adhesive and magnetically stirred for 2-5 hours to prepare a slurry with a solid content of 40wt.%-70wt.%.
[0041] (8) Use centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size.
[0042] Spray granulation process parameters: inlet temperature 200-300℃, outlet temperature 150-200℃, feed pump speed 600-1000r / min, atomizer speed 5000-7000r / min.
[0043] (9) The granulated powder is sieved using a vibrating screen to obtain a granulated powder with a particle size of 40-80 μm.
[0044] (10) The granulated powder obtained by screening is heated and sintered in a heating furnace at a sintering temperature of 200-250°C.
[0045] (11) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 30-70 μm for plasma spraying to prepare a graphite material surface protective coating for the semiconductor field.
[0046] As attached Figure 1 The figure shows a SEM photograph (200x) of the appearance of the composite powder obtained in the present invention.
[0047] The following is a detailed description:
[0048] Example 1
[0049] (1) adding niobium carbide raw material powder (particle size: 30 μm) into a planetary ball mill, using niobium carbide abrasive, and ball milling for 40 hours in an argon atmosphere. After ball milling, the particle size of niobium carbide is 30 nm;
[0050] (2) adding graphite powder (particle size: 80 μm) in an amount of 10 wt.% of the total mass of the powder, and adding an organic adhesive, and continuing ball milling for 5 hours to obtain a slurry with a solid content of 40 wt.%;
[0051] (3) using centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size;
[0052] Spray granulation process parameters: inlet temperature 200℃, outlet temperature 150℃, feed pump speed 1000r / min, atomizer speed 5000r / min;
[0053] (4) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 30;
[0054] (5) heating and sintering the granulated powder obtained by screening in a heating furnace at a sintering temperature of 300° C.
[0055] (6) The sintered powder is vibrated and sieved to obtain a niobium carbide-coated graphite composite powder with a particle size of 50 μm;
[0056] (7) adding niobium carbide coated graphite composite powder (particle size of 20 μm) and niobium powder (particle size of 70 nm, added in an amount of 5 wt.% of the total mass of the powder) and an organic adhesive, and stirring by magnetic force for 5 hours to prepare a slurry with a solid content of 70 wt.%;
[0057] (8) Using centrifugal spray granulation equipment to make granulated powder of a certain particle size;
[0058] Spray granulation process parameters: inlet temperature 200℃, outlet temperature 200℃, feed pump speed 600r / min, atomizer speed 7000r / min;
[0059] (9) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 80 μm;
[0060] (10) heating and sintering the granulated powder obtained by screening in a heating furnace at a sintering temperature of 250° C.;
[0061] (11) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 30 μm for plasma spraying to prepare a surface protective coating of graphite materials for use in the semiconductor field.
[0062] Example 2
[0063] (1) adding niobium carbide raw material powder (particle size: 50 μm) into a planetary ball mill, using niobium carbide abrasive, and ball milling for 20 hours in an argon atmosphere. After ball milling, the particle size of niobium carbide was 90 nm;
[0064] (2) adding graphite powder (particle size: 30 μm) in an amount of 50 wt.% of the total mass of the powder, and adding an organic adhesive, and continuing ball milling for 2 hours to obtain a slurry with a solid content of 70 wt.%;
[0065] (3) using centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size;
[0066] Spray granulation process parameters: inlet temperature 400℃, outlet temperature 150℃, feed pump speed 600r / min, atomizer speed 7000r / min;
[0067] (4) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 60 μm;
[0068] (5) using a heating furnace to heat and sinter the granulated powder obtained by screening at a sintering temperature of 200° C.;
[0069] (6) The sintered powder is vibrated and sieved to obtain a niobium carbide-coated graphite composite powder with a particle size of 50 μm;
[0070] (7) adding niobium carbide coated graphite composite powder (particle size of 50 μm) and niobium powder (particle size of 70 nm, added in an amount of 20 wt.% of the total mass of the powder) and an organic adhesive, and stirring by magnetic force for 2 hours to prepare a slurry with a solid content of 40 wt.%;
[0071] (8) Using centrifugal spray granulation equipment to make granulated powder of a certain particle size;
[0072] Spray granulation process parameters: inlet temperature 200℃, outlet temperature 150℃, feed pump speed 1000r / min, atomizer speed 5000r / min;
[0073] (9) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 80 μm;
[0074] (10) heating and sintering the granulated powder obtained by screening in a heating furnace at a sintering temperature of 200° C.;
[0075] (11) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 70 μm for plasma spraying to prepare a surface protective coating of graphite materials for use in the semiconductor field.
[0076] Example 3
[0077] (1) adding niobium carbide raw material powder (particle size: 40 μm) into a planetary ball mill, using niobium carbide abrasive, and ball milling for 30 hours in an argon atmosphere. After ball milling, the particle size of niobium carbide was 60 nm;
[0078] (2) adding graphite powder (particle size: 50 μm) in an amount of 30 wt.% of the total mass of the powder, and adding an organic adhesive, and continuing ball milling for 4 hours to obtain a slurry with a solid content of 60 wt.%;
[0079] (3) using centrifugal spray granulation equipment to make the slurry into granulated powder of a certain particle size;
[0080] Spray granulation process parameters: inlet temperature 300℃, outlet temperature 180℃, feed pump speed 800r / min, atomizer speed 6000r / min;
[0081] (4) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 40 μm;
[0082] (5) using a heating furnace to heat and sinter the granulated powder obtained by screening at a sintering temperature of 250° C.;
[0083] (6) The sintered powder is vibrated and sieved to obtain a niobium carbide-coated graphite composite powder with a particle size of 30 μm;
[0084] (7) adding niobium carbide coated graphite composite powder (particle size of 40 μm) and niobium powder (particle size of 30 nm, added in an amount of 15 wt.% of the total mass of the powder) and an organic adhesive, and stirring by magnetic force for 4 hours to prepare a slurry with a solid content of 50 wt.%;
[0085] (8) Using centrifugal spray granulation equipment to make granulated powder of a certain particle size;
[0086] Spray granulation process parameters: inlet temperature 220℃, outlet temperature 190℃, feed pump speed 900r / min, atomizer speed 5500r / min;
[0087] (9) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 65 μm;
[0088] (10) heating and sintering the granulated powder obtained by screening in a heating furnace at a sintering temperature of 210° C.;
[0089] (11) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 60 μm for plasma spraying to prepare a surface protective coating of graphite materials for use in the semiconductor field.
[0090] The bulk density, fluidity and particle size of the composite powders obtained in Example 1, Example 2 and Example 3 were tested to obtain the results shown in Table 1:
[0091] Table 1: Test results
[0092]
[0093] In summary, the present invention can achieve the following beneficial effects:
[0094] (1) The composite powder of the graphite material surface anti-corrosion composite coating prepared by plasma spraying in the semiconductor field has a spherical appearance, and the structural composition from the inside to the outside is graphite / niobium carbide / niobium, such as Figure 1 As shown in Table 1, it has a suitable bulk density and good fluidity. It can avoid high-temperature oxidation and decomposition of graphite and niobium carbide. The composite coating can be prepared by spraying with plasma spraying equipment, and the continuity and stability of powder feeding can be guaranteed during the spraying process.
[0095] (2) The components of the composite powder of the anti-corrosion composite coating on the surface of graphite material for use in the semiconductor field prepared by plasma spraying are evenly distributed, which can ensure the uniformity of the composition, structure and performance of the coating prepared by plasma spraying.
[0096] (3) The anti-corrosion composite coating prepared on the surface of the graphite material for the semiconductor field by spraying the composite powder prepared by the present invention has excellent thermal shock resistance and excellent bonding performance compared with a single niobium carbide coating, and can effectively prevent the protective coating on the surface of the graphite material from falling off and failing due to thermal stress.
[0097] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing composite powder for surface coating of semiconductor graphite material, characterized in that: The following steps are involved: (1) adding niobium carbide raw material powder into a planetary ball mill and performing ball milling using niobium carbide abrasive; (2) adding graphite powder in an amount of 10wt.% to 50wt.% of the total mass of the composite powder, and adding an organic adhesive, and continuing ball milling; (3) using centrifugal spray granulation equipment to make granulated powder from the slurry; (4) using a vibrating screen to sieve the granulated powder to obtain a granulated powder with a particle size of 30-60 μm; (5) heating and sintering the granulated powder obtained by screening in a heating furnace; (6) The sintered powder is vibrated and sieved to obtain a niobium carbide-coated graphite composite powder with a particle size of 20-50 μm; (7) adding niobium carbide coated graphite composite powder to niobium powder and an organic adhesive, and using magnetic stirring to prepare a slurry with a solid content of 40 wt.% to 70 wt.%; (8) using a centrifugal spray granulation device to prepare a granulated powder from the slurry; (9) Screening the granulated powder using a vibrating screen to obtain a granulated powder with a particle size of 40-80 μm; (10) heating and sintering the granulated powder obtained by screening in a heating furnace; (11) The sintered powder is vibrated and sieved to finally obtain a composite powder with a particle size of 30-70 μm for plasma spraying to prepare a surface protective coating of graphite materials for the semiconductor field.
2. The method for preparing a composite powder for surface coating of a semiconductor graphite material according to claim 1, characterized in that: In step (1), the particle size of the niobium carbide raw material powder is 30-50 μm.
3. The method for preparing a composite powder for surface coating of a semiconductor graphite material according to claim 1 or 2, characterized in that: In step (1), the ball milling is carried out in an argon atmosphere for 20-40 hours, and the particle size of the niobium carbide after ball milling is 30-90 nm.
4. The method for preparing a composite powder for surface coating of a semiconductor graphite material according to claim 1, characterized in that: In step (2), the particle size of the graphite powder is 30-80 μm.
5. The method for preparing a composite powder for surface coating of a semiconductor graphite material according to claim 1 or 4, characterized in that: In step (2), ball milling is performed for 2-5 hours to obtain a slurry with a solid content of 40wt.%-70wt.%.
6. The method for preparing a composite powder for surface coating of a semiconductor graphite material according to claim 1, characterized in that: In step (3), the spray granulation process parameters are: inlet temperature 200-400°C, outlet temperature 150-200°C, feed pump speed 600-1000r / min, atomizer speed 5000-7000r / min.
7. The method for preparing a composite powder for surface coating of a semiconductor graphite material according to claim 1, characterized in that: In step (5), the sintering temperature is 200-250°C.
8. The method for preparing a composite powder for surface coating of a semiconductor graphite material according to claim 1, characterized in that: In step (7), the particle size of the niobium carbide-coated graphite composite powder is 20-50 μm, the particle size of the niobium powder is 20-70 nm, and the added amount is 5 wt.% to 20 wt.% of the total mass of the composite powder.
9. The method for preparing a composite powder for surface coating of a semiconductor graphite material according to claim 1, characterized in that: In step (8), the spray granulation process parameters include inlet temperature 200-300°C, outlet temperature 150-200°C, feed pump speed 600-1000r / min, atomizer speed 5000-7000r / min.
10. A composite powder for surface coating of semiconductor graphite material, characterized in that: The method comprises preparing the product by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Composite powder for anti-corrosion coating of cavity of semiconductor integrated circuit and preparation method of composite powder
CN117820889A
Production of carbon containing refractory
JP1998053454A
Tantalum carbide powder, tantalum carbide-niobium composite powder and their production method