Preparation method of transparent wood fireproof coating
Through the composite effect of tea polyphenols in the inner coating and all-organic high-refractive index polymers in the outer coating, the problem of insufficient deformation and protection of wood under ultraviolet rays in the prior art is solved, and transparent wood fire-resistant coatings are realized Excellent UV resistance and fire resistance.
Patent Information
- Application Number
- CN202411141615.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-20
AI Technical Summary
Existing wood protective coatings cannot effectively prevent wood from deforming, discoloring and cracking under the action of sun and ultraviolet rays, and lack composite protection effects, making it unable to achieve good UV resistance.
The combination of inner coating and outer coating is adopted. The inner coating contains tea polyphenols, and the outer coating contains all-organic high-refractive index polymers. Through the complex effects of refraction, reflection and absorption, it reduces the damage to wood by ultraviolet rays.
Significantly reduce UV ray penetration through wood, avoid deformation, discoloration and cracking, achieving better UV resistance while maintaining fire resistance.
Abstract
Description
Technical Field
[0001] The invention mainly relates to the technical field of coatings, and in particular to a method for preparing a transparent wood fire retardant coating. Background Art
[0002] Wood is generally used in wooden structures, cultural relics, gardens, architectural decoration and furniture, etc. It has a certain decorative effect, but often lacks fire resistance, resulting in the inability to effectively control fire hazards. This has led to the advent of decorative fire retardant coatings that combine decorative and fire-proof functions. Decorative fire retardant coatings are applied to the surface of combustible substrates such as wood, fiberboard or cardboard. They have fire retardant protection and decorative effects. They usually play a certain decorative role. Once a fire occurs, they can prevent the fire from spreading and achieve the purpose of protecting the combustible substrate.
[0003] In the prior art, a method for preparing a three-component decorative transparent fire-retardant coating is disclosed in a patent with an authorization announcement number of CN 104497782 B, wherein melamine, hydrogen guanidine, urea, formaldehyde, etc. are selected to form component A, APP II and pentaerythritol are selected to form component B, and acetic acid is selected as component C as an auxiliary acid source and also as a diluent. After the three components are evenly mixed, a decorative transparent fire-retardant coating is prepared. However, this coating has the following problems:
[0004] For wooden structures located outdoors, daily sunlight, especially the effects of ultraviolet rays, can cause deformation, discoloration, cracking and other consequences of the wood. The above-mentioned protective coatings do not have the function of mitigating ultraviolet damage. In addition, after the existing wood protective coating forms a coating, each part of the coating plays the same role at the same time, and cannot achieve a sequential composite protection effect, thereby failing to achieve a good anti-ultraviolet effect. Summary of the invention
[0005] The technical solution of the present invention aims at the technical problem that the existing technical solutions are too single, and provides a solution that is significantly different from the existing technology. It mainly provides a method for preparing a transparent wood fire retardant coating, which is used to solve the technical problem that the existing wood protective coating mentioned in the above background technology cannot achieve a good anti-ultraviolet effect.
[0006] The technical solution adopted by the present invention to solve the above technical problems is:
[0007] A method for preparing a transparent wood fire retardant coating, wherein the transparent wood fire retardant coating comprises an inner coating and an outer coating;
[0008] The preparation method of the inner layer coating comprises the following steps:
[0009] A1. Dissolve the flexible flame retardant in water and add tea polyphenol crystals to prepare a flame retardant mixture;
[0010] A2, uniformly mixing the flame retardant mixture with the amino resin to obtain a transparent fireproof inner coating;
[0011] The preparation method of the outer coating comprises the following steps:
[0012] B1, preparing a sulfur-containing all-organic high refractive index polymer by polymerizing brominated alkane and dithiophenol monomers through organic base catalysis;
[0013] B2, dissolving the sulfur-containing all-organic high-refractive index polymer in a transparent organic solvent to obtain a high-refractive index polymer solution;
[0014] B3, grinding ammonium polyphosphate and pentaerythritol and mixing them evenly with polysiloxane emulsion to obtain a fireproof mixture;
[0015] B4. Add high refractive index polymer solution, film-forming aid and amino resin into the fire-retardant mixture and mix them evenly to obtain a transparent fire-retardant outer coating.
[0016] Specifically, in step A1, the preparation method of the flexible flame retardant is:
[0017] A1-1, mixing a phosphorus source and a carbon source and heating them to obtain a phosphate ester; the mass ratio of the phosphorus source to the carbon source is 1:(0.3-0.5), the heating temperature is 100-120°C, and the time is 4-6h; the phosphorus source is selected from any one of phosphoric acid, polyphosphoric acid amine, phosphorus oxychloride, chloroethanol phosphate, chlorinated phosphate ester and polyphosphoric acid; the carbon source is selected from any one of pentaerythritol, starch, triazine compounds, neopentyl glycol and diethanolamine;
[0018] A1-2, mixing the phosphate ester and the halloysite nanotubes in a mass ratio of 1:(0.01-0.1), and then heating at 50° C. for 30 minutes to obtain the modified phosphate ester;
[0019] A1-3. Mix the modified phosphate ester and polyethylene glycol in a mass ratio of 1:(0.2-0.5), heat at 50°C for 1 hour, and then heat at 120°C for 4 hours to obtain a flexible flame retardant.
[0020] Furthermore, in step A1, after the flexible flame retardant is dissolved in water, the mass fraction of the flexible flame retardant aqueous solution obtained is 40-60wt%, and the amount of the tea polyphenol crystals added is 4-10% of the weight of the flexible flame retardant aqueous solution.
[0021] Furthermore, in step A2, the mass ratio of the flame retardant mixture to the amino resin is 1:(1.0-1.5).
[0022] Furthermore, in step B1, the reaction temperature is 80° C., the monomer concentration is 0.2 M, the solvent is dimethyl sulfoxide (DMSO), and the reaction time is 4 hours.
[0023] Furthermore, in step B2, the organic solvent is dimethylformamide or dichloromethane.
[0024] Specifically, step B3 includes:
[0025] B3-1, add deionized water, defoamer, dispersant, ammonium polyphosphate and pentaerythritol into a stirring device in sequence, stir at 1500-2000 r / min for 20-30 min, and then grind in a three-roll grinder for 2-3 h to obtain a preliminary mixture;
[0026] B3-2. Place the preliminary mixture into a disperser and disperse it at a speed of 1500-2000 r / min. At the same time, add the polysiloxane emulsion to mix well.
[0027] Furthermore, in step B3-1, the mass ratio of the deionized water, defoamer, dispersant, ammonium polyphosphate and pentaerythritol is 1:0.1:0.3:25:15; in step B3-2, the amount of the polysiloxane emulsion added is 7 / 25 of the weight of the ammonium polyphosphate.
[0028] Furthermore, step B4 is specifically as follows: reducing the speed of the disperser containing the fire-retardant mixture to 500-800 r / min, adding a film-forming aid, an amino resin, a defoaming agent, a thickener, a leveling agent, a light stabilizer and a high refractive index polymer solution, and mixing them evenly to obtain a transparent fire-retardant outer coating.
[0029] Furthermore, the mass ratio of the membrane auxiliary agent, amino resin, defoamer, thickener, leveling agent, light stabilizer and high refractive index polymer solution is 0.3:50:0.2:0.3:0.3:0.3:0.3, and the ratio of the amino resin to the polysiloxane emulsion is 50:7.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The present invention includes an inner coating and an outer coating, wherein the outer coating contains an all-organic high-refractive index polymer, and the inner coating contains tea polyphenols. When used, sunlight first irradiates the outer coating, and the high refractive index and high reflectivity of the all-organic high-refractive index polymer are utilized to achieve a good anti-ultraviolet effect, significantly reducing the ultraviolet rays passing through the outer coating; then the inner coating absorbs part of the ultraviolet rays through the ultraviolet absorption capacity of tea polyphenols, further reducing the ultraviolet rays contacting the wood structure. The present invention achieves a good anti-ultraviolet effect through the refraction, reflection, and absorption of ultraviolet rays by the inner coating and the outer coating, and can effectively prevent the deformation, discoloration, and cracking of wood due to the action of ultraviolet rays.
[0032] (2) The present invention includes an inner coating and an outer coating, and both the inner coating and the outer coating have transparent, flame retardant and certain UV resistance properties. For wooden structures in an environment with weak UV intensity, the inner coating and the outer coating in the present invention can be selected and applied alone.
[0033] The present invention will be explained in detail below through specific embodiments. DETAILED DESCRIPTION
[0034] To facilitate understanding of the present invention, the present invention will be described in more detail below. The present invention can be implemented in different forms and is not limited to the embodiments described in the text. On the contrary, these embodiments are provided to make the content disclosed in the present invention more thorough and comprehensive.
[0035] Embodiment 1: A transparent wood fire retardant coating comprises an inner coating and an outer coating.
[0036] The preparation method of the inner coating comprises the following steps:
[0037] A1. Mix a phosphorus source and a carbon source and heat them to obtain a phosphate ester; the mass ratio of the phosphorus source to the carbon source is 1:0.5, the heating temperature is 100°C, and the heating time is 6 hours; the phosphorus source is polyphosphoamine, and the carbon source is pentaerythritol;
[0038] A2, mixing the phosphate ester and the halloysite nanotubes in a mass ratio of 1:0.01, and then heating at 50° C. for 30 minutes to obtain the modified phosphate ester;
[0039] A3. The modified phosphate ester and polyethylene glycol were mixed in a mass ratio of 1:0.3, first heated at 50°C for 1 hour, and then heated at 120°C for 4 hours to obtain a flexible flame retardant;
[0040] A4, dissolving the flexible flame retardant in water to obtain a flexible flame retardant aqueous solution with a mass fraction of 40-60wt%, and then adding tea polyphenol crystals to prepare a flame retardant mixture, wherein the amount of the tea polyphenol crystals added is 4% by weight of the flexible flame retardant aqueous solution;
[0041] A5. Evenly mix the flame retardant mixture and the amino resin to obtain a transparent fireproof inner coating. The mass ratio of the flame retardant mixture to the amino resin is 1:1.0.
[0042] The preparation method of the outer coating comprises the following steps:
[0043] B1, preparing a sulfur-containing all-organic high-refractive index polymer by polymerizing brominated alkane and dithiophenol monomers through organic base catalysis, the reaction temperature is 80°C, the monomer concentration is 0.2M, the solvent is dimethyl sulfoxide (DMSO), and the reaction time is 4 hours;
[0044] B2, dissolving the sulfur-containing all-organic high-refractive index polymer in a transparent organic solvent to obtain a high-refractive index polymer solution, wherein the organic solvent is dimethylamide;
[0045] B3, grinding ammonium polyphosphate and pentaerythritol and mixing them evenly with polysiloxane emulsion to obtain a fireproof mixture;
[0046] B3-1, deionized water, defoamer A203E, dispersant SP-762, ammonium polyphosphate and pentaerythritol were added to a stirring device in sequence, stirred at 1500 r / min for 30 min, and then ground in a three-roll mill for 2 h to obtain a preliminary mixture; the mass ratio of deionized water, defoamer A203E, dispersant SP-762, ammonium polyphosphate and pentaerythritol was 1:0.1:0.3:25:15;
[0047] B3-2, put the preliminary mixture into a disperser and disperse it at a speed of 1500r / min, and add the polysiloxane emulsion to mix evenly; the amount of the polysiloxane emulsion added is 7 / 25 of the weight of the ammonium polyphosphate;
[0048] B4. Reduce the speed of the disperser containing the fire-retardant mixture to 500r / min, add film-forming aid PPH, amino resin, defoamer A203E, thickener XS-167, leveling agent XS-12, light stabilizer UV1130 and high refractive index polymer solution, mix well to obtain a transparent fire-retardant outer coating; the mass ratio of film-forming aid PPH, amino resin, defoamer A203E, thickener XS-167, leveling agent XS-12, light stabilizer UV1130 and high refractive index polymer solution is 0.3:50:0.2:0.3:0.3:0.3:0.3, and the ratio of the amino resin to the aforementioned polysiloxane emulsion is 50:7.
[0049] The sulfur-containing all-organic high-refractive-index polymer in the outer coating has a refractive index of up to 1.8433 at 589 nanometers, and has good optical transparency in the visual and RI regions and even within the range of 100 microns. The high refractive index gives it good reflectivity, thereby being able to exert an anti-UV effect.
[0050] The absorption spectrum of tea polyphenols shows an absorption peak in the ultraviolet light region. The absorption peak of tea polyphenols is usually in the range of 200-400 nanometers, so tea polyphenols have the effect of absorbing ultraviolet rays.
[0051] When used, sunlight first shines on the outer layer of paint, using the high refractive index and high reflectivity of the all-organic high-refractive index polymer to achieve a better anti-UV effect, significantly reducing the ultraviolet rays passing through the outer layer of paint; then the inner layer of paint absorbs part of the ultraviolet rays through the ultraviolet light absorption ability of tea polyphenols, further reducing the ultraviolet rays contacting the wooden structure, thereby achieving a better anti-UV effect, which can effectively prevent the wood from deformation, discoloration, cracking, etc. due to the action of ultraviolet rays.
[0052] The outer coating is compounded with polysiloxane emulsion, ammonium polyphosphate and pentaerythritol. The unique polysiloxane side chains and multi-functional group structure of the polysiloxane emulsion make it have good compatibility with the amino resin. At the same time, the contact angle of the multi-functional group makes the ammonium polyphosphate and pentaerythritol have better dispersibility, so that the transparent fire-retardant coating for wooden buildings of the present invention has good fireproof performance, the coating is transparent, the original appearance of the material can be maintained, it is not easy to crack, and it has good weather resistance.
[0053] The flexible flame retardant in the inner coating has good flame retardant properties, which significantly reduces the fire hazard of wooden structures.
[0054] Embodiment 2: This embodiment differs from Embodiment 1 in that:
[0055] The preparation method of the inner coating comprises the following steps:
[0056] A1. Mix a phosphorus source and a carbon source and heat them to obtain a phosphate ester; the mass ratio of the phosphorus source to the carbon source is 1:0.3, the heating temperature is 110°C, and the heating time is 5 hours; the phosphorus source is chloroethanol phosphoric acid, and the carbon source is starch;
[0057] A2, mixing the phosphate ester and the halloysite nanotubes in a mass ratio of 1:0.05, and then heating at 50° C. for 30 minutes to obtain the modified phosphate ester;
[0058] A3. The modified phosphate ester and polyethylene glycol were mixed in a mass ratio of 1:0.5, first heated at 50°C for 1 hour, and then heated at 120°C for 4 hours to obtain a flexible flame retardant;
[0059] A4, dissolving the flexible flame retardant in water to obtain a flexible flame retardant aqueous solution with a mass fraction of 40-60wt%, and then adding tea polyphenol crystals to prepare a flame retardant mixture, wherein the amount of the tea polyphenol crystals added is 7% by weight of the flexible flame retardant aqueous solution;
[0060] A5. Evenly mix the flame retardant mixture and the amino resin to obtain a transparent fireproof inner coating. The mass ratio of the flame retardant mixture to the amino resin is 1:1.5.
[0061] The preparation method of the outer coating comprises the following steps:
[0062] B1, preparing a sulfur-containing all-organic high-refractive index polymer by polymerizing brominated alkane and dithiophenol monomers through organic base catalysis, the reaction temperature is 80°C, the monomer concentration is 0.2M, the solvent is dimethyl sulfoxide (DMSO), and the reaction time is 4 hours;
[0063] B2, dissolving the sulfur-containing all-organic high-refractive index polymer in a transparent organic solvent to obtain a high-refractive index polymer solution, wherein the organic solvent is dichloromethane;
[0064] B3, grinding ammonium polyphosphate and pentaerythritol and mixing them evenly with polysiloxane emulsion to obtain a fireproof mixture;
[0065] B3-1, deionized water, defoamer A203E, dispersant SP-762, ammonium polyphosphate and pentaerythritol were added to a stirring device in sequence, stirred at 2000 r / min for 20 min, and then ground in a three-roll mill for 3 h to obtain a preliminary mixture; the mass ratio of the deionized water, defoamer A203E, dispersant SP-762, ammonium polyphosphate and pentaerythritol was 1:0.1:0.3:25:15;
[0066] B3-2, put the preliminary mixture into a disperser and disperse it at a speed of 2000r / min, and add the polysiloxane emulsion to mix evenly; the amount of the polysiloxane emulsion added is 7 / 25 of the weight of the ammonium polyphosphate;
[0067] B4. Reduce the speed of the disperser containing the fire-retardant mixture to 800r / min, add film-forming aid PPH, amino resin, defoamer A203E, thickener XS-167, leveling agent XS-12, light stabilizer UV1130 and high refractive index polymer solution, mix evenly to obtain a transparent fire-retardant outer coating; the mass ratio of film-forming aid PPH, amino resin, defoamer A203E, thickener XS-167, leveling agent XS-12, light stabilizer UV1130 and high refractive index polymer solution is 0.3:50:0.2:0.3:0.3:0.3:0.3, and the ratio of the amino resin to the aforementioned polysiloxane emulsion is 50:7.
[0068] The rest is the same as the first embodiment.
[0069] Embodiment 3: This embodiment differs from Embodiment 1 in that:
[0070] The preparation method of the inner coating comprises the following steps:
[0071] A1. Mix a phosphorus source and a carbon source and heat them to obtain a phosphate ester; the mass ratio of the phosphorus source to the carbon source is 1:0.4, the heating temperature is 120°C, and the heating time is 4 hours; the phosphorus source is phosphoric acid, and the carbon source is diethanolamine;
[0072] A2, mixing the phosphate ester and the halloysite nanotubes in a mass ratio of 1:0.1, and then heating at 50° C. for 30 minutes to obtain the modified phosphate ester;
[0073] A3. The modified phosphate ester and polyethylene glycol were mixed in a mass ratio of 1:0.2, first heated at 50°C for 1 hour, and then heated at 120°C for 4 hours to obtain a flexible flame retardant;
[0074] A4, dissolving the flexible flame retardant in water to obtain a flexible flame retardant aqueous solution with a mass fraction of 40-60wt%, and then adding tea polyphenol crystals to prepare a flame retardant mixture, wherein the amount of the tea polyphenol crystals added is 10% by weight of the flexible flame retardant aqueous solution;
[0075] A5. Evenly mix the flame retardant mixture and the amino resin to obtain a transparent fireproof inner coating. The mass ratio of the flame retardant mixture to the amino resin is 1:1.3.
[0076] The preparation method of the outer coating comprises the following steps:
[0077] B1, preparing a sulfur-containing all-organic high-refractive index polymer by polymerizing brominated alkane and dithiophenol monomers through organic base catalysis, the reaction temperature is 80°C, the monomer concentration is 0.2M, the solvent is dimethyl sulfoxide (DMSO), and the reaction time is 4 hours;
[0078] B2, dissolving the sulfur-containing all-organic high-refractive index polymer in a transparent organic solvent to obtain a high-refractive index polymer solution, wherein the organic solvent is dimethylamide;
[0079] B3, grinding ammonium polyphosphate and pentaerythritol and mixing them evenly with polysiloxane emulsion to obtain a fireproof mixture;
[0080] B3-1, deionized water, defoamer A203E, dispersant SP-762, ammonium polyphosphate and pentaerythritol were added to a stirring device in sequence, stirred at 1500 r / min for 25 min, and then ground in a three-roll mill for 2.5 h to obtain a preliminary mixture; the mass ratio of the deionized water, defoamer A203E, dispersant SP-762, ammonium polyphosphate and pentaerythritol was 1:0.1:0.3:25:15;
[0081] B3-2, put the preliminary mixture into a disperser and disperse it at a speed of 1500r / min, and add the polysiloxane emulsion to mix evenly; the amount of the polysiloxane emulsion added is 7 / 25 of the weight of the ammonium polyphosphate;
[0082] B4. Reduce the speed of the disperser containing the fire-retardant mixture to 500r / min, add film-forming aid PPH, amino resin, defoamer A203E, thickener XS-167, leveling agent XS-12, light stabilizer UV1130 and high refractive index polymer solution, mix well to obtain a transparent fire-retardant outer coating; the mass ratio of film-forming aid PPH, amino resin, defoamer A203E, thickener XS-167, leveling agent XS-12, light stabilizer UV1130 and high refractive index polymer solution is 0.3:50:0.2:0.3:0.3:0.3:0.3, and the ratio of the amino resin to the aforementioned polysiloxane emulsion is 50:7.
[0083] The rest is the same as the first embodiment.
[0084] The transparent wood fire retardant coating obtained by the present invention was subjected to sample preparation and performance testing, as follows:
[0085] (1) Small sample combustion performance test:
[0086] The test substrate is made of ordinary solid wood with a size of 200mm×200mm×10mm. Before painting the sample, the sample is fully polished with 300-mesh fine sand to ensure that the surface of the sample is flat and smooth. The sample is painted with the transparent wood fire retardant coating prepared by the present invention, and the wet coating amount is 800g / m 2 The samples were subjected to a combustion test. The test results showed that the sample expanded and foamed rapidly after being heated, forming a honeycomb-shaped dense carbon layer with an expansion ratio of 150-200 times, which effectively blocked the spread of flames and heat and protected the substrate from damage.
[0087] (2) Anti-ultraviolet performance test:
[0088] The sample coating was applied on a glass slide with a size of 60 mm × 60 mm × 0.5 mm using an applicator, and the coated sample was dried in a constant temperature drying oven at 60°C. The light transmittance of the sample was measured at 300 nm, 360 nm and 560 nm using an ultraviolet spectrophotometer, and the same slide without coating was set as a reference sample. The test results are shown in Table 1.
[0089] Table 1 Anti-ultraviolet performance test results
[0090] Experimental protocol 300nm transmittance% 360nm transmittance% 560nm transmittance% Example 1 2.4 3.5 5.1 Example 2 4.7 6.3 9.0 Example 3 3.6 5.4 8.8 Reference sample 40.4 50.1 55.6
[0091] It can be seen from Table 1 that the ultraviolet transmittance of the transparent wood fire retardant coating prepared in Examples 1-3 is only less than 16.2% of that of the reference sample, so the transparent wood fire retardant coating prepared by the present invention has significant anti-ultraviolet performance.
[0092] It can be seen from the above content that the transparent wood fire retardant coating prepared by the present invention has excellent flame retardant and fireproof properties and excellent anti-ultraviolet performance.
[0093] The above content provides an exemplary description of the present invention. Obviously, the specific implementation of the present invention is not limited to the above-mentioned method. As long as such non-substantial improvements are made by adopting the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for preparing a transparent wood fire retardant coating, characterized in that: The transparent wood fireproof coating comprises an inner coating and an outer coating; The preparation method of the inner layer coating comprises the following steps: A1. Dissolve the flexible flame retardant in water and add tea polyphenol crystals to prepare a flame retardant mixture; A2, uniformly mixing the flame retardant mixture with the amino resin to obtain a transparent fireproof inner coating; The preparation method of the outer coating comprises the following steps: B1, preparing a sulfur-containing all-organic high refractive index polymer by polymerizing brominated alkane and dithiophenol monomers through organic base catalysis; B2, dissolving the sulfur-containing all-organic high-refractive index polymer in a transparent organic solvent to obtain a high-refractive index polymer solution; B3, grinding ammonium polyphosphate and pentaerythritol and mixing them evenly with polysiloxane emulsion to obtain a fireproof mixture; B4. Add high refractive index polymer solution, film-forming aid and amino resin into the fire-retardant mixture and mix them evenly to obtain a transparent fire-retardant outer coating.
2. The method for preparing a transparent wood fire retardant coating according to claim 1, characterized in that: In step A1, the preparation method of the flexible flame retardant is: A1-1, mixing a phosphorus source and a carbon source and heating them to obtain a phosphate ester; the mass ratio of the phosphorus source to the carbon source is 1:(0.3-0.5), the heating temperature is 100-120°C, and the time is 4-6h; the phosphorus source is selected from any one of phosphoric acid, polyphosphoric acid amine, phosphorus oxychloride, chloroethanol phosphate, chlorinated phosphate ester and polyphosphoric acid; the carbon source is selected from any one of pentaerythritol, starch, triazine compounds, neopentyl glycol and diethanolamine; A1-2, mixing the phosphate ester and the halloysite nanotubes in a mass ratio of 1:(0.01-0.1), and then heating at 50° C. for 30 minutes to obtain the modified phosphate ester; A1-3. Mix the modified phosphate ester and polyethylene glycol in a mass ratio of 1:(0.2-0.5), heat at 50°C for 1 hour, and then heat at 120°C for 4 hours to obtain a flexible flame retardant.
3. The method for preparing a transparent wood fire retardant coating according to claim 1, characterized in that: In step A1, after the flexible flame retardant is dissolved in water, the mass fraction of the obtained flexible flame retardant aqueous solution is 40-60wt%, and the added amount of the tea polyphenol crystals is 4-10% of the weight of the flexible flame retardant aqueous solution.
4. The method for preparing a transparent wood fire retardant coating according to claim 1, characterized in that: In step A2, the mass ratio of the flame retardant mixture to the amino resin is 1:(1.0-1.5).
5. The method for preparing a transparent wood fire retardant coating according to claim 1, characterized in that: In step B1, the reaction temperature is 80° C., the monomer concentration is 0.2 M, the solvent is dimethyl sulfoxide, and the reaction time is 4 hours.
6. The method for preparing a transparent wood fire retardant coating according to claim 1, characterized in that: In step B2, the organic solvent is dimethylformamide or dichloromethane.
7. The method for preparing a transparent wood fire retardant coating according to claim 1, characterized in that: Step B3 includes: B3-1, add deionized water, defoamer, dispersant, ammonium polyphosphate and pentaerythritol into a stirring device in sequence, stir at 1500-2000 r / min for 20-30 min, and then grind in a three-roll grinder for 2-3 h to obtain a preliminary mixture; B3-2. Place the preliminary mixture into a disperser and disperse it at a speed of 1500-2000 r / min. At the same time, add the polysiloxane emulsion to mix well.
8. The method for preparing a transparent wood fire retardant coating according to claim 7, characterized in that: In step B3-1, the mass ratio of deionized water, defoamer, dispersant, ammonium polyphosphate and pentaerythritol is 1:0.1:0.3:25:15; in step B3-2, the amount of polysiloxane emulsion added is 7 / 25 of the weight of ammonium polyphosphate.
9. The method for preparing a transparent wood fire retardant coating according to claim 7, characterized in that: Step B4 is specifically as follows: reducing the speed of the disperser containing the fire-retardant mixture to 500-800 r / min, adding film-forming aid, amino resin, defoamer, thickener, leveling agent, light stabilizer and high refractive index polymer solution, and mixing evenly to obtain a transparent fire-retardant outer coating.
10. The method for preparing a transparent wood fire retardant coating according to claim 9, characterized in that: The mass ratio of the membrane auxiliary agent, amino resin, defoamer, thickener, leveling agent, light stabilizer and high refractive index polymer solution is 0.3:50:0.2:0.3:0.3:0.3:0.3, and the ratio of the amino resin to the polysiloxane emulsion is 50:7.
Citation Information
Patent Citations
Phosphorus-containing nano flame retardant and preparation method thereof
CN109971037A
Flame retardant
WO2011121001A1