Modified graphene oxide and polyurea anticorrosive coating composition and method for preparing polyurea anticorrosive coating
By using modified graphene oxide and bisphenol F epoxy resin, the adhesion between the polyurea coating and the metal substrate and its barrier ability against corrosive media are improved, solving the problems of weak bonding strength and insufficient barrier ability of the polyurea coating, and achieving better protective effect.
Patent Information
- Application Number
- CN202310533329.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-11
AI Technical Summary
The weak bonding strength between the polyurea coating and the substrate, as well as its poor barrier function against highly corrosive media, result in the coating being prone to peeling and detachment, and insufficient protective effect.
A modified graphene oxide and polyurea anti-corrosion coating composition was used. The graphene oxide was modified by isocyanate-based silane, and bisphenol F epoxy resin and a stabilizing rust-removing agent were added to the coating to improve the adhesion between the coating and the metal substrate and the barrier ability against corrosive media.
It improves the adhesion between polyurea anti-corrosion coating and metal substrate, enhances the barrier performance against corrosive media, extends the service life of the coating, and reduces the difficulty and cycle of construction.
Smart Images

Figure CN118931250A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurea anti-corrosion coatings, and in particular to a modified graphene oxide and polyurea anti-corrosion coating composition and a method for preparing the polyurea anti-corrosion coating. Background Art
[0002] Coating anti-corrosion technology is an important means to mitigate the corrosion problem of metal-based materials. Common anti-corrosion coating products such as epoxy resin paint, polyurethane paint, and fluorocarbon paint rely on the barrier and shielding effect of their own dense structure to inhibit the invasion and penetration of corrosive media into the substrate, thereby producing a good substrate protection effect.
[0003] As an important branch of polyurethane coatings, polyurea anticorrosive coatings are usually prepared by the reaction of prepolymers generated by the reaction of polyisocyanates and hydroxyl polyethers with terminal amino or terminal hydroxyl compounds. They have broad application prospects in the research fields of waterproof and anti-penetration, wear-resistant and scratch-resistant, and explosion-resistant and impact-resistant materials. Compared with traditional epoxy resin-based anticorrosive coatings, polyurea coatings have a higher solid content, which reduces the release of VOCs and avoids environmental pollution during the construction process. In addition, polyurea coatings can complete cross-linking and curing in a short time, and the resulting coating is dense and has fewer pinhole defects. While effectively shortening the construction period, it ensures that the mechanical strength, flexibility and barrier capacity of the coating meet the requirements of metal protection performance. For example, patent CN201910739886.4 discloses a rigid high-temperature resistant polyurea anti-corrosion coating and a preparation method thereof, in which super-tough polyetheramine is added to the coating to enhance the toughness of the coating and make it suitable for anti-corrosion operations in high-temperature (160°C) environments; patent CN201810940993.9 discloses a high-performance, environmentally friendly modified polyurea anti-corrosion coating and a preparation method thereof, in which a cobalt cyclohexane acid catalyst is added to improve the degree of cross-linking inside the coating.
[0004] However, based on a large number of actual on-site applications of coatings, the hydrogen atoms in the urea bonds and carbamate bonds in the polyurea structure have weak interactions with the metal surface, and the coating has high viscosity and lacks wetting and spreading ability, making it difficult to penetrate into the surface of the metal substrate that has not been thoroughly rusted. This results in weak bonding strength between the polyurea coating and the substrate, and it is prone to peeling and other failure phenomena during service. It usually requires complex and detailed substrate surface pretreatment and use with a primer, which increases the difficulty and cycle of construction. In addition, the coating's barrier ability to highly corrosive media needs to be further improved so that it can be applied to different protection scenarios. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of weak bonding strength between the polyurea coating and the substrate and weak barrier ability of the coating to highly corrosive media in the prior art, and to provide a modified graphene oxide and polyurea anticorrosive coating composition and a method for preparing the polyurea anticorrosive coating. The coating formed after spraying the polyurea anticorrosive coating composition provided by the present invention has strong adhesion to the metal substrate and can improve the barrier and corrosion resistance to corrosive media.
[0006] In order to achieve the above-mentioned object, the present invention provides a modified graphene oxide on the one hand, wherein the modified graphene oxide is obtained by modifying graphene oxide with isocyanate silane.
[0007] Preferably, the isocyanate silane is 3-isocyanate propyl triethoxy silane and / or 3-isocyanate propyl trimethoxy silane.
[0008] Preferably, the weight ratio of the graphene oxide to the isocyanate silane is 1:20-50, preferably 1:25-40.
[0009] A second aspect of the present invention provides a method for preparing modified graphene oxide, the method comprising the following steps:
[0010] (1) mixing graphene oxide with an organic solvent and subjecting it to ultrasonic treatment;
[0011] (2) Under the protection of an inert atmosphere, the solution obtained in step (1) is mixed with isocyanate silane for reaction, and the solid-liquid separation is performed to obtain modified graphene oxide.
[0012] Preferably, in step (1), the weight ratio of the graphene oxide to the organic solvent is 1:40 to 105, preferably 1:50 to 99.
[0013] Preferably, the organic solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N,N-diethylformamide.
[0014] Preferably, in step (1), the ultrasonic conditions include: ultrasonic temperature of 15-30°C, ultrasonic time of 30-60 min, and ultrasonic frequency of 20-35 kHz.
[0015] Preferably, the weight ratio of the graphene oxide to the isocyanate silane is 1:20-50, preferably 1:25-40.
[0016] Preferably, in step (2), the reaction conditions include: reaction temperature of 60 to 100° C., and reaction time of 12 to 48 h.
[0017] The third aspect of the present invention provides a polyurea anticorrosive coating composition, which contains a polyurea anticorrosive coating component A and a polyurea anticorrosive coating component B, wherein the polyurea anticorrosive coating component A and the polyurea anticorrosive coating component B are stored independently.
[0018] The polyurea anticorrosive coating component A is prepared from raw materials containing aliphatic diisocyanate, aromatic diisocyanate, polyether polyol, bisphenol F epoxy resin, stable rust-reducing agent, ester viscosity reducer and modified graphene oxide, wherein the modified graphene oxide is the modified graphene oxide described in the first aspect above or the modified graphene oxide prepared by the method described in the second aspect above;
[0019] The polyurea anticorrosive coating component B is prepared from raw materials containing polyether polyamine, terminal amino chain extender, light stabilizer hindered amine, ultraviolet absorber and silane coupling agent.
[0020] Preferably, the weight ratio of the aliphatic diisocyanate, the aromatic diisocyanate, the polyether polyol, the bisphenol F epoxy resin, the stable rust remover, the ester viscosity reducer and the modified graphene oxide is 30:28-44:24-38:5-10:6-15:1-2:0.5-2.
[0021] Preferably, the weight ratio of the polyether polyamine, the amino-terminated chain extender, the light stabilizer hindered amine, the ultraviolet absorber and the silane coupling agent is 55:25-40:1-3:1-2:10-20.
[0022] Preferably, the aliphatic diisocyanate is selected from one or more of hexamethylene diisocyanate, hexamethylene diisocyanate trimer, methyl formate pentamethylene diisocyanate and 2,2,4-trimethylhexane diisocyanate.
[0023] Preferably, the aromatic diisocyanate is selected from one or more of 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, p-phenylene diisocyanate, methylcyclohexyl diisocyanate, p-phenylene diisocyanate, diphenylmethane-4,4'-diisocyanate, 3,3'-dimethoxy-4,4'-diphenyl diisocyanate and hydrogenated phenylmethane diisocyanate.
[0024] Preferably, the molecular weight of the polyether polyol is 200-3000.
[0025] Preferably, the polyether polyol is selected from one or more of polyoxypropylene ether glycol, polytetramethylene ether glycol, polyoxypropylene-oxyethylene glycol and tetramethylene ether glycol-oxypropylene copolymer glycol.
[0026] Preferably, the epoxy equivalent of the bisphenol F epoxy resin is 140 to 200 g / eq, preferably 150 to 190 g / eq.
[0027] Preferably, the stabilizing rust-removing agent is selected from one or more of zinc phosphate, zinc chromate and aluminum dihydrogen tripolyphosphate.
[0028] Preferably, the ester viscosity reducer is selected from one or more of dioctyl phthalate, dibutyl phthalate, ethyl carbonate, propylene carbonate, propane sultone, 2-dimethylaminoethyl acetate, 2-chloroethyl ester and dimethylaminoethyl acrylate.
[0029] Preferably, the molecular weight of the polyether polyamine is 100-3000, preferably 200-2000.
[0030] Preferably, the amino-terminated chain extender is selected from one or more of dimethylthiotoluenediamine, N,N'-di-sec-butyl-p-phenylenediamine, N,N'-dialkylphenylenediamine, N,N'-dialkylmethyldiamine, bis(p-aminobenzoic acid)propylene glycol ester, diethyltoluenediamine and methyldiethanolamine.
[0031] Preferably, the light stabilizer hindered amine is bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and / or 4-benzoyloxy-2,2,6,6-tetramethylpiperidine.
[0032] Preferably, the ultraviolet absorber is selected from one or more of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P), 2-(5-chloro-2-benzotriazolyl)-6-tert-butyl-p-cresol (UV-326), 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole (UV-327) and 2-hydroxy-4-n-octylbenzophenone (UV-531).
[0033] Preferably, the silane coupling agent is selected from one or more of γ-diethylenetriaminopropylmethyldimethoxysilane (KH-103), γ-aminopropyltriethoxysilane (KH-550), γ-(2,3-epoxypropyloxy)propyltrimethoxysilane (KH-560), N-aminoethyl-3-aminopropylmethyldimethoxysilane (KH-602) and γ-aminoethylaminopropyltrimethoxysilane (KH-792).
[0034] Preferably, the preparation method of the polyurea anticorrosive coating component A comprises:
[0035] S1, dehydrating the polyether polyol;
[0036] S2. Under normal pressure and inert atmosphere, the product obtained in step S1 is mixed with aliphatic diisocyanate, aromatic diisocyanate, bisphenol F epoxy resin, stable rust-reducing agent, ester viscosity reducer and modified graphene oxide for reaction.
[0037] Preferably, in step S1, the conditions for the dehydration treatment include: a pressure of -0.05 to -0.15 MPa, a temperature of 100 to 120°C, and a time of 2 to 3 hours.
[0038] Preferably, in step S2, the reaction conditions include: reaction temperature of 70 to 100° C., preferably 80 to 90° C.; reaction time of 1 to 6 h, preferably 2 to 4 h.
[0039] Preferably, the preparation method of the polyurea anticorrosive coating component B comprises:
[0040] 1) mixing the polyether polyamine and the amino-terminated chain extender and performing a dehydration treatment;
[0041] 2) Under normal pressure and inert atmosphere, the product obtained in step 1) is mixed with a light stabilizer hindered amine, a UV absorber and a silane coupling agent to react.
[0042] Preferably, in step 1), the conditions for the dehydration treatment include: a pressure of -0.05 to -0.15 MPa, a temperature of 90 to 110° C., and a time of 2 to 3 hours.
[0043] Preferably, in step 2), the reaction conditions include: reaction temperature of 50 to 80° C., preferably 60 to 75° C.; reaction time of 0.5 to 4 h, preferably 1 to 2 h.
[0044] The fourth aspect of the present invention provides a method for preparing a polyurea anti-corrosion coating, which comprises: mixing the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B, spraying the mixture on the surface of a metal substrate, and performing curing to obtain a polyurea anti-corrosion coating.
[0045] Preferably, the weight ratio of the polyurea anticorrosive coating component A to the polyurea anticorrosive coating component B is 1-1.2:1, preferably 1.05-1.15:1.
[0046] Preferably, the spraying conditions include: a spraying temperature of 60 to 80° C. and a spraying pressure of 14 to 16 MPa.
[0047] Preferably, the curing conditions include: a curing temperature of 15 to 30° C. and a curing time of 5 to 9 days.
[0048] Preferably, the metal substrate is carbon steel material of the outer wall of the storage tank.
[0049] The present invention adopts a specific modifier to carry out graft modification on graphene oxide, and the surface of the obtained modified graphene oxide is modified with rich isocyanate functional groups and imine groups; in the process of preparing a polyurea anti-corrosion coating component A, the modified graphene oxide is used as a filler, which not only has good compatibility and dispersibility in the polyurea anti-corrosion coating component A, but also after the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are sprayed on a metal substrate, the mechanical properties of the polyurea anti-corrosion coating, the barrier shielding and corrosion resistance to corrosive media are significantly improved, the durability and protective effect of the polyurea anti-corrosion coating in a corrosive environment are improved, and the service life of the polyurea anti-corrosion coating is extended.
[0050] In the process of preparing the polyurea anticorrosive coating component A, the present invention modifies the polyurea anticorrosive coating by compounding bisphenol F epoxy resin and a stable rust-removing agent, so that the polyurea anticorrosive coating can form a strong adhesion with the metal substrate and the rusty metal surface, improve the adhesion between the polyurea anticorrosive coating and the metal substrate, reduce the requirements for the surface pretreatment of the polyurea anticorrosive coating, and make the polyurea anticorrosive coating applicable to the rusty metal surface without primer coating, thereby reducing the possibility of peeling failure during service. At the same time, the modified graphene oxide uniformly dispersed in the coating can increase its barrier capacity, improve the durability and protective effect of the coating in a corrosive environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 It is the FTIR spectrum of the graphene oxide and modified graphene oxide described in Example 1. DETAILED DESCRIPTION
[0052] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0053] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0054] A first aspect of the present invention provides a modified graphene oxide, wherein the modified graphene oxide is obtained by modifying graphene oxide with isocyanate silane.
[0055] Modifying graphene oxide with isocyanate silane can graft isocyanate groups and imine groups on the surface of graphene oxide. The obtained modified graphene oxide can be used as a filler for polyurea anti-corrosion coatings. It can form hydrogen bonds with the coating matrix to achieve uniform dispersion of graphene oxide in the coating. It can give full play to the physical and chemical properties of the two-dimensional sheet structure of graphene oxide, extend the diffusion path of corrosive media, and improve the comprehensive performance of polyurea anti-corrosion coatings.
[0056] According to the present invention, preferably, the isocyanate silane is 3-isocyanate propyl triethoxy silane and / or 3-isocyanate propyl trimethoxy silane.
[0057] In the present invention, in order to make the graphene oxide grafted with abundant isocyanate groups and imine groups, and the obtained modified graphene oxide has good compatibility and dispersibility in the polyurea anticorrosive coating component A, the amount of the graphene oxide and the isocyanate silane should be appropriate. In a specific embodiment, the weight ratio of the amount of the graphene oxide to the isocyanate silane can be 1:20 to 50, preferably 1:25 to 40, for example 1:25, 1:26, 1:27, 1:28, 1:29, 1:30, 1:31, 1:32, 1:33, 1:34, 1:35, 1:36, 1:37, 1:38, 1:39 or 1:40.
[0058] A second aspect of the present invention provides a method for preparing modified graphene oxide, the method comprising the following steps:
[0059] (1) mixing graphene oxide with an organic solvent and subjecting it to ultrasonic treatment;
[0060] (2) Under the protection of an inert atmosphere, the solution obtained in step (1) is mixed with isocyanate silane for reaction, and the solid-liquid separation is performed to obtain modified graphene oxide.
[0061] According to the present invention, the organic solvent can be any conventional choice in the art, as long as it can dissolve graphene oxide. In a specific embodiment, the organic solvent can be selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N,N-diethylformamide, preferably N,N-dimethylformamide.
[0062] In the present invention, there is no particular restriction on the usage ratio of the graphene oxide to the organic solvent. Specifically, in step (1), the weight ratio of the graphene oxide to the organic solvent can be 1:40 to 105, preferably 1:50 to 99, for example 1:50, 1:55, 1:60, 1:65, 1:70, 1:75, 1:80, 1:85, 1:90, 1:95 or 1:99.
[0063] In a specific embodiment, in step (1), the ultrasonic temperature of the ultrasound can be 15-30°C, for example, 15°C, 20°C, 25°C or 30°C; the ultrasonic time of the ultrasound can be 30-60min, for example, 30min, 35min, 40min, 45min, 50min, 55min or 60min; the ultrasonic frequency of the ultrasound can be 20-35kHz, for example, 20kHz, 25kHz, 30kHz or 35kHz.
[0064] In the present invention, in order to make the graphene oxide grafted with abundant isocyanate groups and imine groups, and the obtained modified graphene oxide has good compatibility and dispersibility in the polyurea anticorrosive coating component A, the amount of the graphene oxide and the isocyanate silane should be appropriate. In a specific embodiment, the weight ratio of the amount of the graphene oxide to the isocyanate silane can be 1:20 to 50, preferably 1:25 to 40, for example 1:25, 1:26, 1:27, 1:28, 1:29, 1:30, 1:31, 1:32, 1:33, 1:34, 1:35, 1:36, 1:37, 1:38, 1:39 or 1:40.
[0065] In a preferred embodiment, in step (2), the reaction temperature of the reaction can be 60-100°C, for example 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C; the reaction time of the reaction can be 12-48h, for example 12h, 15h, 18h, 20h, 25h, 30h, 35h, 40h, 45h or 48h.
[0066] According to the present invention, specifically, in step (2), the reaction is carried out under stirring conditions. Preferably, the stirring speed is 800-1200 r / min.
[0067] According to the present invention, specifically, in step (2), the solid-liquid separation is carried out by centrifugation; after the solid-liquid separation, the obtained precipitate is repeatedly washed with dichloromethane to obtain modified graphene oxide.
[0068] The third aspect of the present invention provides a polyurea anticorrosive coating composition, which contains a polyurea anticorrosive coating component A and a polyurea anticorrosive coating component B, wherein the polyurea anticorrosive coating component A and the polyurea anticorrosive coating component B are stored independently. In the present invention, the polyurea anticorrosive coating component A and the polyurea anticorrosive coating component B are stored independently before spraying, and the polyurea anticorrosive coating component A and the polyurea anticorrosive coating component B are mixed when spraying onto the surface of the metal substrate.
[0069] According to the present invention, the polyurea anti-corrosion coating component A is prepared from raw materials containing aliphatic diisocyanate, aromatic diisocyanate, polyether polyol, bisphenol F epoxy resin, stable rust inhibitor, ester viscosity reducer and modified graphene oxide, wherein the modified graphene oxide is the modified graphene oxide described in the first aspect above or the modified graphene oxide prepared by the method described in the second aspect above.
[0070] The modified graphene oxide provided by the present invention, which is grafted with isocyanate groups and imine groups on the surface, can be used as a filler for preparing component A of a polyurea anticorrosive coating to form hydrogen bonds with the coating matrix, thereby achieving uniform dispersion of the graphene oxide in the coating, giving full play to the physical and chemical property advantages of the two-dimensional sheet structure of the graphene oxide, extending the diffusion path of the corrosive medium, enhancing the corrosion resistance and mechanical strength of the polyurea anticorrosive coating, extending the service life of the coating, and improving the comprehensive performance of the polyurea anticorrosive coating.
[0071] The raw materials for preparing component A of the polyurea anticorrosive coating of the present invention are compounded with low-viscosity bisphenol F epoxy resin, and the adhesion of the coating is improved by utilizing the interaction between the hydroxyl group and the ether bond on the structure of the bisphenol F epoxy resin and the metal surface. At the same time, a stabilizing rust-converting agent is added to the coating, which can convert the rust on the surface of the metal substrate into a heteropolyacid complex passivation layer with strong adhesion performance, and has a good rust-stabilizing effect, so that it can be applied to the surface of rusty metal equipment.
[0072] According to the present invention, the polyurea anticorrosive coating component B is prepared from raw materials containing polyether polyamine, amino-terminated chain extender, light stabilizer hindered amine, ultraviolet absorber and silane coupling agent.
[0073] In the present invention, in order to obtain a polyurea anticorrosive coating with excellent comprehensive performance, it is necessary to limit the usage ratio of each raw material for preparing component A of the polyurea anticorrosive coating to an appropriate range.
[0074] In a specific embodiment, the weight ratio of the aliphatic diisocyanate, the aromatic diisocyanate, the polyether polyol, the bisphenol F epoxy resin, the stable rust remover, the ester viscosity reducer and the modified graphene oxide can be 30:28-44:24-38:5-10:6-15:1-2:0.5-2.
[0075] In the present invention, in order to obtain a polyurea anticorrosive coating with excellent comprehensive performance, it is necessary to limit the usage ratio of each raw material for preparing component B of the polyurea anticorrosive coating to an appropriate range.
[0076] In a specific embodiment, the weight ratio of the polyether polyamine, the amino-terminated chain extender, the light stabilizer hindered amine, the ultraviolet absorber and the silane coupling agent is 55:25-40:1-3:1-2:10-20.
[0077] According to the present invention, the aliphatic diisocyanate used to prepare the polyurea anticorrosive coating component A can be a conventional choice in the art. In a preferred embodiment, the aliphatic diisocyanate can be selected from one or more of hexamethylene diisocyanate, hexamethylene diisocyanate trimer, methyl formate pentamethylene diisocyanate and 2,2,4-trimethylhexane diisocyanate.
[0078] According to the present invention, the aromatic diisocyanate used to prepare the polyurea anticorrosive coating component A can be a conventional choice in the art. In a preferred embodiment, the aromatic diisocyanate is selected from one or more of 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, p-phenylene diisocyanate, methylcyclohexyl diisocyanate, p-phenylene diisocyanate, diphenylmethane-4,4'-diisocyanate, 3,3'-dimethoxy-4,4'-diphenyl diisocyanate and hydrogenated phenylmethane diisocyanate.
[0079] In the present invention, in a specific embodiment, the molecular weight of the polyether polyol can be 200 to 3000, for example, 200, 400, 650, 800, 1000, 1500, 2000, 2500 or 3000.
[0080] In a preferred embodiment, the polyether polyol is selected from one or more of polyoxypropylene ether glycol, polytetramethylene ether glycol, polyoxypropylene-oxyethylene glycol and tetramethylene ether glycol.
[0081] According to the present invention, the bisphenol F epoxy resin may be any of various options known to those skilled in the art, as long as it can provide hydroxyl groups and ether bonds.
[0082] In a specific embodiment, the epoxy equivalent of the bisphenol F epoxy resin is 140 to 200 g / eq, preferably 150 to 190 g / eq; the source of the bisphenol F epoxy resin is not limited, and it can be various commercially available products or homemade. In a preferred embodiment, the bisphenol F epoxy resin can be selected from one or more of NPEF-170, EPON-862, REF-170, DER-321, DER-354 and PY-306.
[0083] According to the present invention, in order to convert the rust on the surface of the metal substrate into a heteropolyacid complex passivation layer with strong adhesion properties and play a good rust stabilization role, in a preferred embodiment, the stable rust-converting agent can be selected from one or more of zinc phosphate, zinc chromate and dihydrogen aluminum tripolyphosphate.
[0084] In the present invention, the type of the lipid viscosity reducer is not limited. In a preferred embodiment, the ester viscosity reducer can be selected from one or more of dioctyl phthalate, dibutyl phthalate, ethyl carbonate, propylene carbonate, propane sultone, 2-dimethylaminoethyl acetate, 2-chloroethyl ester and dimethylaminoethyl acrylate.
[0085] According to the present invention, the molecular weight of the polyether polyamine is 100 to 3000, preferably 200 to 2000; the source of the polyether polyamine is not limited, and it can be various commercially available products or homemade. In a preferred embodiment, the polyether polyamine is selected from one or more of polyetheramine T-403, polyetheramine T-430, polyetheramine T-1000, polyetheramine T-2000, polyetheramine D-230, polyetheramine D-400, polyetheramine D-2000, polyetheramine FL-1000 and polyetheramine ED-600.
[0086] In the present invention, the amino-terminated chain extender can be various choices well known to those skilled in the art. In a preferred embodiment, the amino-terminated chain extender is selected from one or more of dimethylthiotoluenediamine, N,N'-di-sec-butyl-p-phenylenediamine, N,N'-dialkylphenylenediamine, N,N'-dialkylmethyldiamine, bis(p-aminobenzoic acid)propylene glycol ester, diethyltoluenediamine and methyldiethanolamine.
[0087] In the present invention, the light stabilizer hindered amine can be a conventional choice in the art. In a preferred embodiment, the light stabilizer hindered amine can be bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and / or 4-benzoyloxy-2,2,6,6-tetramethylpiperidine.
[0088] According to the present invention, the ultraviolet absorber can be various choices well known to those skilled in the art. In a preferred embodiment, the ultraviolet absorber can be selected from one or more of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P), 2-(5-chloro-2-benzotriazolyl)-6-tert-butyl-p-cresol (UV-326), 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole (UV-327) and 2-hydroxy-4-n-octylbenzophenone (UV-531).
[0089] In the present invention, the silane coupling agent can be a conventional choice in the art. In a preferred embodiment, the silane coupling agent can be selected from one or more of γ-diethylenetriaminopropylmethyldimethoxysilane (KH-103), γ-aminopropyltriethoxysilane (KH-550), γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH-560), N-aminoethyl-3-aminopropylmethyldimethoxysilane (KH-602) and γ-aminoethylaminopropyltrimethoxysilane (KH-792).
[0090] Furthermore, the present invention provides a method for preparing a polyurea anticorrosive coating component A. In a preferred embodiment, the method for preparing the polyurea anticorrosive coating component A comprises:
[0091] S1, dehydrating the polyether polyol;
[0092] S2. Under normal pressure and inert atmosphere, the product obtained in step S1 is mixed with aliphatic diisocyanate, aromatic diisocyanate, bisphenol F epoxy resin, stable rust-reducing agent, ester viscosity reducer and modified graphene oxide for reaction.
[0093] In a specific embodiment, in step S1, the pressure of the dehydration treatment can be -0.05 to -0.15 MPa, for example, -0.05 MPa, -0.06 MPa, -0.07 MPa, -0.08 MPa, -0.09 MPa, -0.1 MPa, -0.11 MPa, -0.12 MPa, -0.13 MPa, -0.14 MPa or -0.15 MPa; the temperature can be 100 to 120°C, for example, 100°C, 105°C, 110°C, 115°C or 120°C; the time can be 2 to 3 h, for example, 2 h, 2.2 h, 2.5 h, 2.8 h or 3 h.
[0094] In a more specific embodiment, step S1 comprises: placing the polyether polyol in a reaction kettle under a pressure of -0.05 to -0.15 MPa, heating to 100 to 120° C. with stirring, and maintaining the temperature for 2 to 3 hours.
[0095] According to the present invention, in step S2, the reaction temperature of the reaction can be 70-100°C, preferably 80-90°C, for example 80°C, 82°C, 85°C, 88°C or 90°C; the reaction time of the reaction can be 1-6h, preferably 2-4h, for example 2h, 2.5h, 3h, 3.5h or 4h.
[0096] In a specific embodiment, step S2 comprises: under normal pressure and inert atmosphere protection, lowering the temperature of the reaction system of step (1) to 50-60°C, then adding aliphatic diisocyanate, aromatic diisocyanate, bisphenol F epoxy resin, stable rust remover, ester viscosity reducer and modified graphene oxide, heating to 80-90°C, stirring and reacting for 2-4h, after the reaction is completed, waiting for the system to cool to 20-30°C, filtering, and obtaining polyurea anticorrosive coating component A.
[0097] Furthermore, the present invention provides a method for preparing a polyurea anticorrosive coating component B. In a preferred embodiment, the method for preparing the polyurea anticorrosive coating component B comprises:
[0098] 1) mixing the polyether polyamine and the amino-terminated chain extender and performing a dehydration treatment;
[0099] 2) Under normal pressure and inert atmosphere, the product obtained in step 1) is mixed with a light stabilizer hindered amine, a UV absorber and a silane coupling agent to react.
[0100] In a specific embodiment, in step 1), the pressure of the dehydration treatment can be -0.05 to -0.15 MPa, for example, -0.05 MPa, -0.06 MPa, -0.07 MPa, -0.08 MPa, -0.09 MPa, -0.1 MPa, -0.11 MPa, -0.12 MPa, -0.13 MPa, -0.14 MPa or -0.15 MPa; the temperature can be 90 to 110°C, for example, 90°C, 95°C, 100°C, 105°C, 110°C or 120°C; the time can be 2 to 3 h, for example, 2 h, 2.2 h, 2.5 h, 2.8 h or 3 h.
[0101] In a more specific embodiment, step 1) comprises: mixing the polyether polyamine and the amino-terminated chain extender under a pressure of -0.05 to -0.15 MPa, stirring and heating to 90 to 110° C., and maintaining the mixture for 2 to 3 hours for dehydration treatment.
[0102] In a specific embodiment, in step 2), the reaction temperature of the reaction can be 50-80°C, preferably 60-75°C, for example 60°C, 62°C, 65°C, 68°C, 70°C, 72°C or 75°C; the reaction time can be 0.5-4h, preferably 1-2h, for example 1h, 1.5h or 2h.
[0103] In a more specific embodiment, step 2) includes: under normal pressure and inert atmosphere protection, lowering the temperature of the reaction system of step 1) to 50-60°C, then adding light stabilizer hindered amine, ultraviolet absorber and silane coupling agent, heating to 50-80°C, stirring and reacting for 0.5-4h, after the reaction is completed, waiting for the system to cool to 20-30°C, filtering, and obtaining polyurea anticorrosive coating component B.
[0104] The fourth aspect of the present invention provides a method for preparing a polyurea anti-corrosion coating, which comprises: mixing the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B, spraying the mixture on the surface of a metal substrate, and performing curing to obtain a polyurea anti-corrosion coating.
[0105] In the present invention, the metal substrate may be pre-treated before spraying. In a specific embodiment, acetone and / or ethanol are used to remove grease on the surface of the metal substrate, and then the surface of the metal substrate is treated to St 2 or Sa 2.5 by manual polishing and / or spraying to remove rust.
[0106] According to the present invention, the polyurea anticorrosive coating component A and the polyurea anticorrosive coating component B are mixed and sprayed on the surface of the metal substrate to form a polyurea anticorrosive coating on the surface of the metal substrate. Specifically, the weight ratio of the polyurea anticorrosive coating component A to the polyurea anticorrosive coating component B can be 1-1.2:1, preferably 1.05-1.15:1, such as 1.05:1, 1.06:1, 1.07:1, 1.08:1, 1.09:1, 1.1:1, 1.11:1, 1.12:1, 1.13:1, 1.14:1 or 1.15:1.
[0107] In a specific embodiment, the spraying conditions include: the spraying temperature can be 60-80°C, such as 60°C, 65°C, 70°C, 75°C or 80°C; the spraying pressure can be 14-16MPa, such as 14MPa, 14.5MPa, 15MPa, 15.5MPa or 16MPa.
[0108] According to the present invention, the curing conditions can be conventionally selected in the art. In a specific embodiment, the curing conditions include: the curing temperature can be 15 to 30°C, such as 15°C, 20°C, 25°C or 30°C; the curing time can be 5 to 9 days, such as 5 days, 6 days, 7 days, 8 days or 9 days.
[0109] The polyurea anticorrosion coating prepared by the present invention can be applied to equipment external anticorrosion projects in complex corrosive environments, which has important practical significance for ensuring the safety of oil and gas storage and transportation, and has a strong application prospect. In a specific embodiment, the metal substrate is a carbon steel material for the outer wall of the storage tank.
[0110] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.
[0111] Example 1
[0112] The raw materials for preparing component A of the polyurea anti-corrosion coating include: 30 parts by weight of hexamethylene diisocyanate (Yantai Wanhua), 28 parts by weight of p-phenylene diisocyanate (Dexin Chemical), 36 parts by weight of polyoxypropylene ether glycol PPG-1000 (Mitsui Chemicals, molecular weight 1000), 8 parts by weight of NPEF-170 (Nan Ya, epoxy equivalent of 160-180 g / eq), 12 parts by weight of dihydrogen aluminum tripolyphosphate (McLean), 1 part by weight of dioctyl phthalate (Shandong Xincheng), and 2 parts by weight of modified graphene oxide.
[0113] The raw materials for preparing component B of the polyurea anti-corrosion coating include: 55 parts by weight of polyetheramine T-403 (BASF, molecular weight 403), 30 parts by weight of N,N'-dialkylphenylenediamine (Nanjing Kaitian), 1 part by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (Chongqing Ruiya), 1 part by weight of UV-326 (Guangzhou Yinuo), and 12 parts by weight of KH-560 (Aldrich).
[0114] S1. Preparation process of modified graphene oxide
[0115] 1 part by weight of graphene oxide powder (Xianfeng Nano) was mixed with 50 parts by weight of N,N-dimethylformamide (Aldrich), and ultrasonically dispersed at 25°C for 45 minutes with the ultrasonic frequency set to 20 kHz; the obtained mixed solution was placed in a nitrogen environment, and 32 parts by weight of 3-isocyanatepropyltriethoxysilane (Hengchang Chemical) were added, the reaction system was heated to 80°C, and stirred at a speed of 1000 r / min for 24 hours; after the reaction system was naturally cooled to room temperature, the obtained black suspension was centrifuged and the lower precipitate was removed, and then the lower precipitate was repeatedly washed with dichloromethane (Jinan Xichuan) to obtain modified graphene oxide.
[0116] S2. Preparation process of polyurea anticorrosive coating component A
[0117] Add polyoxypropylene ether diol PPG-1000 into the reactor, stir and heat to 100°C under a pressure of -0.1MPa, and maintain dehydration treatment for 2.5h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 50°C, add hexamethylene diisocyanate, p-phenylene diisocyanate, NPEF-170, aluminum dihydrogen triphosphate, dioctyl phthalate and modified graphene oxide prepared in step S1 according to the above ratio, then raise the temperature to 80°C, stir and react for 2h; after the reaction is completed, cool the reaction system to 30°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0118] S3. Preparation process of polyurea anticorrosive coating component B
[0119] Add polyetheramine T-403 and N,N'-dialkylphenylenediamine into the reaction kettle according to the above ratio, stir and heat to 90°C under -0.1MPa pressure, and maintain dehydration for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 55°C, add bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, UV-326 and KH-560 according to the above ratio, then raise the temperature to 70°C, stir and react for 1.5h; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0120] S4. Preparation process of polyurea anticorrosion coating
[0121] First, acetone and ethanol are used to remove grease on the surface of the metal substrate, and then the surface of the metal substrate is treated to Sa 2.5 level by spraying rust removal. Using a special spraying device for polyurea coating, polyurea anti-corrosion coating component A and polyurea anti-corrosion coating component B are mixed and sprayed onto the surface of the metal substrate in a weight ratio of 1.13:1. The spraying temperature is set to 70°C and the spraying pressure is 14MPa. After curing for 7 days at 25°C, the polyurea anti-corrosion coating can be obtained.
[0122] Example 2
[0123] The raw materials for preparing component A of the polyurea anticorrosive coating include: 30 parts by weight of hexamethylene diisocyanate trimer (Yantai Wanhua), 38 parts by weight of diphenylmethane-4,4′-diisocyanate (Huntsman), 24 parts by weight of polyoxypropylene ether glycol PPG-2000 (Nantong Ruhr, molecular weight 2000), 10 parts by weight of EPON-862 (HEXION, epoxy equivalent of 165-173 g / eq), 8 parts by weight of zinc phosphate (Sinopharm Reagent), 1 part by weight of propylene carbonate (Jinan Pulai), and 1 part by weight of modified graphene oxide.
[0124] The raw materials for preparing component B of the polyurea anti-corrosion coating include: 55 parts by weight of polyetheramine T-1000 (BASF, molecular weight 1000), 25 parts by weight of diethyltoluenediamine (Shandong Chuangyu), 2 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl)sebacate (Chongqing Ruiya), 1 part by weight of UV-P (Nanjing Milan), and 16 parts by weight of KH-550 (Aldrich).
[0125] S1. Preparation process of modified graphene oxide
[0126] 1 part by weight of graphene oxide powder (prepared by the conventional Hummers method) was mixed with 99 parts by weight of N,N-dimethylformamide (Aldrich), and ultrasonically dispersed at 25°C for 50 minutes with the ultrasonic frequency set to 25kHz; the obtained mixed solution was placed in a nitrogen environment, and 25 parts by weight of 3-isocyanatepropyltrimethoxysilane (Yishun Chemical) were added, the reaction system was heated to 80°C, and stirred at a speed of 800r / min for 30 hours; after the reaction system was naturally cooled to room temperature, the obtained black suspension was centrifuged to remove the lower precipitate, and the lower precipitate was repeatedly washed with dichloromethane (Jinan Xichuan) to obtain modified graphene oxide.
[0127] S2. Preparation process of polyurea anticorrosive coating component A
[0128] Add polyoxypropylene ether diol PPG-2000 into the reactor, stir and heat to 100°C under a pressure of -0.1MPa, and maintain dehydration treatment for 3 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 55°C, add hexamethylene diisocyanate trimer, diphenylmethane-4,4′-diisocyanate, EPON-862, zinc phosphate, propylene carbonate and modified graphene oxide prepared in step S1 according to the above ratio, then heat to 80°C, stir and react for 3 hours; after the reaction is completed, cool the reaction system to 30°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0129] S3. Preparation process of polyurea anticorrosive coating component B
[0130] Add polyetheramine T-1000 and diethyltoluenediamine into the reaction kettle according to the above-mentioned ratio, stir and heat to 100°C under -0.1MPa pressure, and maintain dehydration treatment for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 50°C, add bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, UV-P and KH-550 according to the above-mentioned ratio, then raise the temperature to 75°C, stir and react for 2h; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0131] S4. Preparation process of polyurea anticorrosion coating
[0132] First, acetone and ethanol are used to remove grease on the surface of the metal substrate, and then the surface is treated to Sa 2.5 level by spraying to remove rust. Using a special spraying device for polyurea coating, the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are mixed and sprayed onto the surface of the metal substrate in a weight ratio of 1.05:1. The spraying temperature is set to 70°C and the spraying pressure is 15MPa. After curing for 7 days at 25°C, the polyurea anti-corrosion coating can be obtained.
[0133] Example 3
[0134] The raw materials for preparing component A of the polyurea anti-corrosion coating include: 30 parts by weight of methyl methyl pentamethylene diisocyanate (Xi'an Kangnuo), 32 parts by weight of hydrogenated phenylmethane diisocyanate (Yantai Wanhua), 32 parts by weight of polyoxypropylene ether glycol PPG-1000 (BASF, molecular weight 1000), 5 parts by weight of DER-321 (DOW, epoxy equivalent of 180-188 g / eq), 10 parts by weight of zinc phosphate (Sinopharm Reagent), 1.5 parts by weight of propane sultone (Jinan Zhenda), and 0.5 parts by weight of modified graphene oxide.
[0135] The raw materials for preparing component B of the polyurea anticorrosive coating include: 55 parts by weight of polyetheramine D-230 (BASF, molecular weight 230), 25 parts by weight of dimethylthiotoluene diamine (Jiangsu Runfeng), 1 part by weight of 4-benzoyloxy-2,2,6,6-tetramethylpiperidine (Shanghai Jizhi), 1 part by weight of UV-327 (Nanjing Milan), and 12 parts by weight of KH-602 (Nanjing Quanxi).
[0136] S1. Preparation process of modified graphene oxide
[0137] 1 part by weight of graphene oxide powder (Aldrich) was mixed with 50 parts by weight of N,N-dimethylacetamide (Aldrich), and ultrasonically dispersed at 25°C for 60 min, with the ultrasonic frequency set to 30 kHz; the obtained mixed solution was placed in a nitrogen environment, and 35 parts by weight of 3-isocyanatepropyltriethoxysilane (Hengchang Chemical) were added, the reaction system was heated to 80°C, and stirred at a speed of 1000 r / min for 20 h; after the reaction system was naturally cooled to room temperature, the obtained black suspension was centrifuged and the lower precipitate was removed, and the lower precipitate was repeatedly washed with dichloromethane (Jinan Xichuan) to obtain modified graphene oxide.
[0138] S2. Preparation process of polyurea anticorrosive coating component A
[0139] Add polyoxypropylene ether diol PPG-1000 into the reactor, stir and heat to 110°C under a pressure of -0.1 MPa, and maintain dehydration treatment for 2 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add methyl methyl pentamethylene diisocyanate, hydrogenated phenylmethane diisocyanate, DER-321, zinc phosphate, propane sultone and modified graphene oxide prepared in step S1 according to the above ratio, then raise the temperature to 90°C, stir and react for 3.5 hours; after the reaction is completed, cool the reaction system to 30°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0140] S3. Preparation process of polyurea anticorrosive coating component B
[0141] Add polyetheramine D-230 and dimethylthiotoluene diamine into the reaction kettle according to the above ratio, stir and heat to 100°C under -0.1MPa pressure, and maintain dehydration treatment for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 55°C, add 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, UV-327 and KH-602 according to the above ratio, then raise the temperature to 60°C, stir and react for 1h; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0142] S4. Preparation process of polyurea anticorrosion coating
[0143] First, acetone and ethanol are used to remove grease on the surface of the metal substrate, and then the surface is treated to St 2 grade by manual polishing. Using a special polyurea coating spraying device, the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are mixed in a weight ratio of 1.1:1 and sprayed onto the surface of the metal substrate. The spraying temperature is set to 70°C and the spraying pressure is 14MPa. After curing for 7 days at 25°C, the polyurea anti-corrosion coating can be obtained.
[0144] Example 4
[0145] The raw materials for preparing component A of the polyurea anticorrosive coating include: 30 parts by weight of 2,2,4-trimethylhexane diisocyanate (Desmodur), 44 parts by weight of 3,3'-dimethoxy-4,4'-diphenyl diisocyanate (Hunan Jinjinle), 26 parts by weight of polytetramethylene ether polyol PTMG-650 (Korea PTG, molecular weight 650), 6 parts by weight of DER-321 (DOW, epoxy equivalent of 180-188 g / eq), 10 parts by weight of zinc phosphate (Sinopharm Reagent), 1 part by weight of dibutyl phthalate (Aldrich), and 1 part by weight of modified graphene oxide.
[0146] The raw materials for preparing component B of the polyurea anticorrosive coating include: 55 parts by weight of polyetheramine D-400 (BASF, molecular weight 400), 40 parts by weight of methyldiethanolamine (Shandong Yousheng), 1 part by weight of 4-benzoyloxy-2,2,6,6-tetramethylpiperidine (Shanghai Jizhi), 3 parts by weight of UV-327 (Nanjing Milan), and 10 parts by weight of KH-560 (Aldrich).
[0147] S1. Preparation process of modified graphene oxide
[0148] 1 part by weight of graphene oxide powder (Aldrich) was mixed with 60 parts by weight of N,N-dimethylformamide (Aldrich), and ultrasonically dispersed at 25°C for 40 minutes with the ultrasonic frequency set to 35kHz; the obtained mixed solution was placed in a nitrogen environment, and 40 parts by weight of 3-isocyanatepropyltriethoxysilane (Hengchang Chemical) was added, the reaction system was heated to 80°C, and stirred at a speed of 1200r / min for 25 hours; after the reaction system was naturally cooled to room temperature, the black suspension was centrifuged and the lower precipitate was removed, and the lower precipitate was repeatedly washed with dichloromethane (Aldrich) to obtain modified graphene oxide.
[0149] S2. Preparation process of polyurea anticorrosive coating component A
[0150] Add polytetramethylene glycol PTMG-650 into the reaction kettle, stir and heat to 100°C under a pressure of -0.1MPa, and maintain dehydration for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 50°C, add 2,2,4-trimethylhexane diisocyanate, 3,3'-dimethoxy-4,4'-diphenyl diisocyanate, DER-321, zinc phosphate, dibutyl phthalate and modified graphene oxide according to the above ratio, then raise the temperature to 85°C, stir and react for 2h; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0151] S3. Preparation process of polyurea anticorrosive coating component B
[0152] Add polyetheramine D-400 and methyldiethanolamine in the reaction kettle according to the above ratio, stir and heat to 90°C under -0.1MPa pressure, and maintain dehydration treatment for 3 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 50°C, add 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, UV-327 and KH-560 according to the above ratio, then raise the temperature to 75°C, stir and react for 1.5 hours; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0153] S4. Preparation process of polyurea anticorrosion coating
[0154] First, acetone and ethanol are used to remove grease on the surface of the metal substrate, and then the surface is treated to Sa 2.5 level by spraying to remove rust. Using a special spraying device for polyurea coating, the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are mixed and sprayed onto the surface of the metal substrate in a weight ratio of 1.15:1. The spraying temperature is set to 70°C and the spraying pressure is 16MPa. After curing for 7 days at 25°C, the polyurea anti-corrosion coating can be obtained.
[0155] Example 5
[0156] The raw materials for preparing component A of the polyurea anti-corrosion coating include: 30 parts by weight of hexamethylene diisocyanate (Yantai Wanhua), 30 parts by weight of methyl cyclohexyl diisocyanate (Dexin Chemical), 29 parts by weight of polyoxypropylene ether glycol PPG-3000 (DU PONT, molecular weight 3000), 5 parts by weight of PY-306 (DOW, epoxy equivalent of 156-167 g / eq), 6 parts by weight of zinc chromate (Aldrich), 1 part by weight of 2-chloroethyl ester (Jinan Yongchen), and 0.5 parts by weight of modified graphene oxide.
[0157] The raw materials for preparing component B of the polyurea anti-corrosion coating include: 55 parts by weight of polyetheramine ED-600 (Huntsman, molecular weight 600), 32 parts by weight of propylene glycol bis(p-aminobenzoic acid) ester (Ningbo Yinuo), 2 parts by weight of 4-benzoyloxy-2,2,6,6-tetramethylpiperidine (Shanghai Jizhi), 1.5 parts by weight of UV-531 (Shandong Maofa), and 16 parts by weight of KH-792 (Qingdao Hengda).
[0158] S1. Preparation process of modified graphene oxide
[0159] 1 part by weight of graphene oxide powder (prepared by the conventional Hummers method) was mixed with 99 parts by weight of N,N-dimethylacetamide (Aldrich), and ultrasonically dispersed at 25°C for 55 minutes, with the ultrasonic frequency set to 25 kHz; the obtained mixed solution was placed in a nitrogen environment, and 28 parts by weight of 3-isocyanatepropyltriethoxysilane (Hubei Jiufenglong) were added, the reaction system was heated to 80°C, and stirred at a speed of 900 r / min for 26 hours; after the reaction system was naturally cooled to room temperature, the obtained black suspension was centrifuged and the lower precipitate was removed, and the lower precipitate was repeatedly washed with dichloromethane (Aldrich) to obtain modified graphene oxide.
[0160] S2. Preparation process of polyurea anticorrosive coating component A
[0161] Add tetrahydrofuran-propylene oxide copolymer glycol POM-111P into the reaction kettle, stir and heat to 110°C under a pressure of -0.1MPa, and maintain dehydration treatment for 3 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add hexamethylene diisocyanate, methylcyclohexyl diisocyanate, PY-306, zinc chromate, 2-chloroethyl ester and modified graphene oxide according to the above ratio, then raise the temperature to 90°C, stir and react for 2 hours; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0162] S3. Preparation process of polyurea anticorrosive coating component B
[0163] Add polyetheramine ED-600 and propylene glycol bis(p-aminobenzoic acid) into the reaction kettle according to the above ratio, heat to 100°C with stirring under a pressure of -0.1MPa, and maintain dehydration treatment for 2 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, UV-531 and KH-792 according to the above ratio, then raise the temperature to 70°C, stir and react for 2 hours; after the reaction is completed, reduce the reaction system to 30°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0164] S4. Preparation process of polyurea anticorrosive coating
[0165] First, acetone and ethanol are used to remove grease on the surface of the metal substrate, and then the surface is treated to Sa 2.5 level by spraying to remove rust. Using a special spraying device for polyurea coating, the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are mixed and sprayed onto the surface of the metal substrate in a weight ratio of 1.08:1. The spraying temperature is set to 70°C and the spraying pressure is 15MPa. After curing for 7 days at 25°C, the polyurea anti-corrosion coating can be obtained.
[0166] Example 6
[0167] The raw materials for preparing component A of the polyurea anti-corrosion coating include: 30 parts by weight of methyl formate pentamethylene diisocyanate (Xi'an Kangnuo), 35 parts by weight of terephthalate diisocyanate (Tesco Chemical), 27 parts by weight of polyoxypropylene ether glycol PPG-400 (Lianji Chemical, molecular weight 400), 10 parts by weight of NPEF-170 (Nanya, epoxy equivalent of 160-180 g / eq), 12 parts by weight of zinc chromate (Aldrich), 1 part by weight of ethyl carbonate (Sinopharm Reagent), and 1.8 parts by weight of modified graphene oxide.
[0168] The raw materials for preparing component B of the polyurea anti-corrosion coating include: 55 parts by weight of polyetheramine D-230 (Huntsman, molecular weight 230), 38 parts by weight of N,N'-dialkylphenylenediamine (Nanjing Kaitian), 3 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (Chongqing Ruiya), 1 part by weight of UV-326 (Guangzhou Yinuo), and 16 parts by weight of KH-602 (Rongguang Chemical).
[0169] S1. Preparation process of modified graphene oxide
[0170] 1 part by weight of graphene oxide powder (Aldrich) was mixed with 85 parts by weight of N,N-diethylformamide (Aldrich), and ultrasonically dispersed at 30°C for 30 minutes with the ultrasonic frequency set to 35kHz; the obtained mixed solution was placed in a nitrogen environment, and 39 parts by weight of 3-isocyanatepropyltrimethoxysilane (Yishun Chemical) were added, the reaction system was heated to 85°C, and stirred at a speed of 1200r / min for 25h; after the reaction system was naturally cooled to room temperature, the obtained black suspension was centrifuged and the lower precipitate was removed, and then the lower precipitate was repeatedly washed with dichloromethane (Jinan Xichuan) to obtain modified graphene oxide.
[0171] S2. Preparation process of polyurea anticorrosive coating component A
[0172] Add polyoxypropylene ether glycol PPG-400 into the reactor, stir and heat to 100°C under a pressure of -0.13 MPa, and maintain dehydration treatment for 2.5 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 55°C, add methyl formate pentamethylene diisocyanate, p-tert-butylene diisocyanate, NPEF-170, zinc chromate, ethyl carbonate and modified graphene oxide prepared in step S1 according to the above ratio, then raise the temperature to 80°C, stir and react for 2.5 hours; after the reaction is completed, cool the reaction system to 25°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0173] S3. Preparation process of polyurea anticorrosive coating component B
[0174] Add polyetheramine D-230 and N,N'-dialkylphenylenediamine into the reaction kettle according to the above ratio, stir and heat to 100°C under -0.1MPa pressure, and maintain dehydration for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, UV-326 and KH-602 according to the above ratio, then raise the temperature to 75°C, stir and react for 2h; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0175] S4. Preparation process of polyurea anticorrosion coating
[0176] First, acetone is used to remove grease on the surface of the metal substrate, and then the surface of the metal substrate is treated to Sa 2.5 level by spraying to remove rust. Using a special spraying device for polyurea coating, the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are mixed in a weight ratio of 1.15:1 and sprayed onto the surface of the metal substrate. The spraying temperature is set to 80°C and the spraying pressure is 14.5MPa. After curing for 8 days at 25°C, the polyurea anti-corrosion coating can be obtained.
[0177] Example 7
[0178] The raw materials for preparing component A of the polyurea anti-corrosion coating include: 30 parts by weight of 2,2,4-trimethylhexane diisocyanate (Desmodur), 40 parts by weight of methyl cyclohexyl diisocyanate (Desin Chemical), 29 parts by weight of polyether polyol 1000D (Shenghe Weiye, molecular weight of 1000), 7 parts by weight of REF-170 (Huite Chemical, epoxy equivalent of 160-180 g / eq), 6 parts by weight of dialuminum tripolyphosphate (Aldrich), 1 part by weight of 2-dimethylaminoethyl acetate (Hengchang Chemical), and 0.5 parts by weight of modified graphene oxide.
[0179] The raw materials for preparing component B of the polyurea anti-corrosion coating include: 55 parts by weight of polyetheramine ED-600 (Huntsman, molecular weight 600), 39 parts by weight of diethyltoluenediamine (Shandong Chuangyu), 3 parts by weight of 4-benzoyloxy-2,2,6,6-tetramethylpiperidine (Shanghai Jizhi), 2 parts by weight of UV-531 (Shandong Maofa), and 18 parts by weight of KH-103 (Jingtianwei Chemical).
[0180] S1. Preparation process of modified graphene oxide
[0181] 1 part by weight of graphene oxide powder (prepared by conventional Hummers method) was mixed with 95 parts by weight of N,N-dimethylacetamide (Aldrich), and ultrasonically dispersed at 25°C for 50 min, with the ultrasonic frequency set to 20 kHz; the obtained mixed solution was placed in a nitrogen environment, and 28 parts by weight of 3-isocyanatepropyltrimethoxysilane (Yishun Chemical) was added, the reaction system was heated to 60°C, and stirred at a speed of 900 r / min for 20 hours; after the reaction system was naturally cooled to room temperature, the obtained black suspension was centrifuged and the lower precipitate was removed, and the lower precipitate was repeatedly washed with dichloromethane (Aldrich) to obtain modified graphene oxide.
[0182] S2. Preparation process of polyurea anticorrosive coating component A
[0183] Add polyether polyol 1000D into the reactor, stir and heat to 100°C under a pressure of -0.1MPa, and maintain dehydration treatment for 3 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add 2,2,4-trimethylhexane diisocyanate, methylcyclohexyl diisocyanate, REF-170, aluminum dihydrogen tripolyphosphate, 2-dimethylaminoethyl acetate and modified graphene oxide according to the above ratio, then heat to 90°C, stir and react for 2 hours; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0184] S3. Preparation process of polyurea anticorrosive coating component B
[0185] Add polyetheramine ED-600 and diethyltoluenediamine into the reaction kettle according to the above-mentioned ratio, heat to 105°C under -0.1MPa pressure, and maintain dehydration for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, UV-531 and KH-103 according to the above-mentioned ratio, then raise the temperature to 75°C, stir and react for 2h; after the reaction is completed, reduce the reaction system to 25°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0186] S4. Preparation process of polyurea anticorrosive coating
[0187] First, acetone and ethanol are used to remove grease on the surface of the metal substrate, and then the surface is treated to St 2 grade by manual polishing. Using a special polyurea coating spraying device, the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are mixed and sprayed onto the surface of the metal substrate in a weight ratio of 1.05:1. The spraying temperature is set to 70°C and the spraying pressure is 16MPa. After curing for 5 days at 30°C, the polyurea anti-corrosion coating can be obtained.
[0188] Example 8
[0189] The raw materials for preparing component A of the polyurea anticorrosive coating include: 30 parts by weight of hexamethylene diisocyanate trimer (Yantai Wanhua), 33 parts by weight of 3,3'-dimethoxy-4,4'-diphenyl diisocyanate (Hunan Jinjinle), 36 parts by weight of polytetramethylene ether polyol PTMG-650 (Korea PTG, molecular weight 650), 6 parts by weight of EPON-862 (HEXION, epoxy equivalent of 165-173 g / eq), 6 parts by weight of zinc phosphate (Sinopharm Reagent), 1.5 parts by weight of propane sultone (Tosoh Chemical), and 0.5 parts by weight of modified graphene oxide.
[0190] The raw materials for preparing component B of the polyurea anticorrosive coating include: 55 parts by weight of polyetheramine D-400 (BASF, molecular weight 400), 30 parts by weight of diethyltoluenediamine (Shandong Chuangyu), 3 parts by weight of 4-benzoyloxy-2,2,6,6-tetramethylpiperidine (Shanghai Jizhi), 3 parts by weight of UV-531 (Shandong Maofa), and 12 parts by weight of KH-560 (Aldrich).
[0191] S1. Preparation process of modified graphene oxide
[0192] 1 part by weight of graphene oxide powder (Xianfeng Nano) was mixed with 90 parts by weight of N,N-dimethylformamide (Aldrich), and ultrasonically dispersed at 20°C for 40 minutes with the ultrasonic frequency set to 35kHz; the obtained mixed solution was placed in a nitrogen environment, and 34 parts by weight of 3-isocyanatepropyltriethoxysilane (Hengchang Chemical) were added, the reaction system was heated to 75°C, and stirred at a speed of 1200r / min for 35h; after the reaction system was naturally cooled to room temperature, the black suspension was centrifuged and the lower precipitate was removed, and the lower precipitate was repeatedly washed with dichloromethane (Aldrich) to obtain modified graphene oxide.
[0193] S2. Preparation process of polyurea anticorrosive coating component A
[0194] Add polytetramethylene glycol PTMG-650 into the reaction kettle, stir and heat to 110°C under a pressure of -0.1MPa, and maintain dehydration for 2.2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 50°C, add 2,2,4-trimethylhexane diisocyanate, 3,3'-dimethoxy-4,4'-diphenyl diisocyanate, DER-321, zinc phosphate, dibutyl phthalate and modified graphene oxide according to the above ratio, then raise the temperature to 85°C, stir and react for 2h; after the reaction is completed, wait for the reaction system to cool to 25°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0195] S3. Preparation process of polyurea anticorrosive coating component B
[0196] Add polyetheramine D-400 and diethyltoluenediamine into the reaction kettle according to the above ratio, stir and heat to 90°C under -0.1MPa pressure, and maintain dehydration treatment for 3 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 50°C, add 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, UV-531 and KH-560 according to the above ratio, then raise the temperature to 65°C, stir and react for 2 hours; after the reaction is completed, wait for the reaction system to cool to 20°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0197] S4. Preparation process of polyurea anticorrosive coating
[0198] First, ethanol is used to remove grease on the surface of the metal substrate, and then the surface is treated to Sa2.5 grade by spraying to remove rust. Using a special spraying device for polyurea coating, the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are mixed in a weight ratio of 1.15:1 and sprayed onto the surface of the metal substrate. The spraying temperature is set to 80°C and the spraying pressure is 14MPa. After curing for 9 days at 30°C, the polyurea anti-corrosion coating can be obtained.
[0199] Example 9
[0200] The raw materials for preparing component A of the polyurea anti-corrosion coating include: 30 parts by weight of methyl methyl pentamethylene diisocyanate (Xi'an Kangnuo), 37 parts by weight of p-phenylene diisocyanate (Dexin Chemical), 37 parts by weight of polyoxypropylene ether glycol PPG-1000 (BASF, molecular weight 1000), 8 parts by weight of DER-354 (DOW, epoxy equivalent of 167-174 g / eq), 10 parts by weight of zinc chromate (Aldrich), 1 part by weight of propane sultone (Jinan Zhenda), and 2 parts by weight of modified graphene oxide.
[0201] The raw materials for preparing component B of the polyurea anti-corrosion coating include: 55 parts by weight of polyetheramine FL-1000 (Huntsman, molecular weight 1000), 26 parts by weight of dimethylthiotoluene diamine (Jiangsu Runfeng), 1 part by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (Chongqing Ruiya), 1.5 parts by weight of UV-327 (Nanjing Milan), and 18 parts by weight of KH-602 (Nanjing Quanxi).
[0202] S1. Preparation process of modified graphene oxide
[0203] 1 part by weight of graphene oxide powder (Aldrich) was mixed with 75 parts by weight of N,N-dimethylacetamide (Aldrich), and ultrasonically dispersed at 30°C for 55 min, with the ultrasonic frequency set to 30 kHz; the obtained mixed solution was placed in a nitrogen environment, and 34 parts by weight of 3-isocyanatepropyltriethoxysilane (Hengchang Chemical) were added, the reaction system was heated to 80°C, and stirred at a speed of 1000 r / min for 48 hours; after the reaction system was naturally cooled to room temperature, the obtained black suspension was centrifuged and the lower precipitate was removed, and the lower precipitate was repeatedly washed with dichloromethane (Jinan Xichuan) to obtain modified graphene oxide.
[0204] S2. Preparation process of polyurea anticorrosive coating component A
[0205] Add polyoxypropylene ether glycol PPG-1000 into the reactor, stir and heat to 100°C under a pressure of -0.15MPa, and maintain dehydration treatment for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add methyl methyl pentamethylene diisocyanate, hydrogenated phenylmethane diisocyanate, DER-354, zinc chromate, propane sultone and modified graphene oxide prepared in step S1 according to the above ratio, then raise the temperature to 80°C, stir and react for 3.5h; after the reaction is completed, cool the reaction system to 30°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0206] S3. Preparation process of polyurea anticorrosive coating component B
[0207] Add polyetheramine FL-1000 and dimethylthiotoluene diamine into the reaction kettle according to the above ratio, stir and heat to 105°C under -0.1MPa pressure, and maintain dehydration treatment for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, UV-327 and KH-602 according to the above ratio, then raise the temperature to 60°C, stir and react for 1.5h; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0208] S4. Preparation process of polyurea anticorrosion coating
[0209] First, acetone and ethanol are used to remove grease on the surface of the metal substrate, and then the surface is treated to Sa 2.5 level by spraying to remove rust. Using a special spraying device for polyurea coating, the polyurea anti-corrosion coating component A and the polyurea anti-corrosion coating component B are mixed in a weight ratio of 1.1:1 and sprayed onto the surface of the metal substrate. The spraying temperature is set to 70°C and the spraying pressure is 15.5MPa. After curing for 7 days at 25°C, the polyurea anti-corrosion coating can be obtained.
[0210] Example 10
[0211] The raw materials for preparing component A of the polyurea anti-corrosion coating include: 30 parts by weight of hexamethylene diisocyanate (Yantai Wanhua), 39 parts by weight of p-phenylene diisocyanate (Dexin Chemical), 24 parts by weight of polyoxypropylene ether glycol PPG-1500 (Daixu Chemical, molecular weight of 1500), 8 parts by weight of DER-321 (DOW, epoxy equivalent of 180-188 g / eq), 15 parts by weight of dialuminum tripolyphosphate (McLean), 1 part by weight of 2-dimethylaminoethyl acetate (Hengchang Chemical), and 1 part by weight of modified graphene oxide.
[0212] The raw materials for preparing component B of the polyurea anti-corrosion coating include: 55 parts by weight of polyetheramine T-430 (BASF, molecular weight 430), 36 parts by weight of N,N'-dialkylphenylenediamine (Nanjing Kaitian), 2.5 parts by weight of bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (Chongqing Ruiya), 1 part by weight of UV-P (Jianchu Biological), and 12 parts by weight of KH-550 (Aldrich).
[0213] S1. Preparation process of modified graphene oxide
[0214] 1 part by weight of graphene oxide powder (prepared by the conventional Hummers method) was mixed with 50 parts by weight of N,N-dimethylformamide (Aldrich), and ultrasonically dispersed at 25°C for 60 minutes with the ultrasonic frequency set to 30 kHz; the obtained mixed solution was placed in a nitrogen environment, and 26 parts by weight of 3-isocyanatepropyltrimethoxysilane (Yishun Chemical) were added, the reaction system was heated to 80°C, and stirred at a speed of 1200 r / min for 25 hours; after the reaction system was naturally cooled to room temperature, the obtained black suspension was centrifuged and the lower precipitate was removed, and then the lower precipitate was repeatedly washed with dichloromethane (Jinan Xichuan) to obtain modified graphene oxide.
[0215] S2. Preparation process of polyurea anticorrosive coating component A
[0216] Add polyoxypropylene ether diol PPG-1500 into the reactor, stir and heat to 115°C under a pressure of -0.11 MPa, and maintain dehydration treatment for 2.5 hours; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 60°C, add hexamethylene diisocyanate, p-phenylene diisocyanate, DER-321, aluminum dihydrogen tripolyphosphate, 2-dimethylaminoethyl acetate and modified graphene oxide prepared in step S1 according to the above ratio, then heat to 88°C, stir and react for 2 hours; after the reaction is completed, cool the reaction system to 30°C, filter, and obtain polyurea anticorrosive coating component A for standby use.
[0217] S3. Preparation process of polyurea anticorrosive coating component B
[0218] Add polyetheramine T-403 and N,N'-dialkylphenylenediamine into the reaction kettle according to the above ratio, stir and heat to 95°C under -0.1MPa pressure, and maintain dehydration for 2h; adjust the reaction system to normal pressure and nitrogen environment, reduce the temperature to 55°C, add bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, UV-P and KH-550 according to the above ratio, then raise the temperature to 70°C, stir and react for 2h; after the reaction is completed, wait for the reaction system to cool to 30°C, filter, and obtain polyurea anticorrosive coating component B for standby use.
[0219] S4. Preparation process of polyurea anticorrosive coating
[0220] First, acetone and ethanol are used to remove grease on the surface of the metal substrate, and then the surface of the metal substrate is treated to Sa 2.5 level by spraying rust removal. Using a special spraying device for polyurea coating, polyurea anti-corrosion coating component A and polyurea anti-corrosion coating component B are mixed in a weight ratio of 1.15:1 and sprayed onto the surface of the metal substrate. The spraying temperature is set to 80°C and the spraying pressure is 16MPa. After curing for 6 days at 20°C, the polyurea anti-corrosion coating can be obtained.
[0221] Comparative Example 1
[0222] The method of Example 1 is followed, except that NPEF-170 is not added in step S2, that is, bisphenol F epoxy resin is not added during the preparation of component A of the polyurea anticorrosive coating.
[0223] Comparative Example 2
[0224] The method of Example 1 is followed, except that no aluminum dihydrogen tripolyphosphate is added in step S2, that is, no stable rust-inhibiting agent is added during the preparation of component A of the polyurea anticorrosive coating.
[0225] Comparative Example 3
[0226] The method of Example 1 is followed, except that NPEF-170 and aluminum dihydrogen tripolyphosphate are not added in step S2, that is, bisphenol F epoxy resin and stable rust-removing agent are not added in the process of preparing component A of the polyurea anticorrosive coating.
[0227] Comparative Example 4
[0228] The method of Example 1 is followed, except that step S1 is not performed and modified graphene oxide is not added in step S2, that is, modified graphene oxide is not added during the preparation of component A of the polyurea anticorrosive coating.
[0229] Comparative Example 5
[0230] The method of Example 1 was followed, except that step S1 was not performed and graphene oxide (Xianfeng Nano) was directly added in step S2, that is, unmodified graphene oxide was added during the preparation of component A of the polyurea anticorrosive coating.
[0231] Test Example 1
[0232] The FTIR spectra of the graphene oxide and the modified graphene oxide described in step S1 of Example 1 were measured using an ATR-FTIR infrared spectrometer (ThermoFisher), with the scanning range set to 400-4000 cm -1 .
[0233] Depend on Figure 1 The infrared spectrum shows that graphene oxide has a peak at 3428 cm -1 、1730cm -1 and 1655cm -1 The stretching vibration characteristic peaks of OH, C=O and C=C were observed at 3422 cm -1 、1735cm -1 and 1655cm -1 In addition, the modified graphene oxide 2258cm -1 and 1735cm -1 Absorption peaks corresponding to NC=O and CN=C appeared at the surface of graphene oxide modified with 3-isocyanatepropyltriethoxysilane, proving that isocyanate groups and imide bonds were successfully grafted onto the surface.
[0234] Test Example 2
[0235] The polyurea anticorrosive coatings prepared in Examples 1-10 and Comparative Examples 1-5 were tested for mechanical properties and corrosion resistance, and the test results are shown in Tables 1 and 2. The mechanical properties test method is as follows: adhesion refers to the method described in the standard GB / T5210-2006, tensile strength and elongation at break refer to the method described in the standard GB / T 2567-2021, and hardness refers to the method described in the standard GB / T 2411-2008; the corrosion resistance test method is as follows: neutral salt spray resistance refers to the method described in the standard GB / T1771-2007, and resistance to 3wt% NaCl solution, 5wt% NaOH solution, and 5wt% H2SO4 solution refers to the method described in the standard GB / T9274-1988.
[0236] Table 1
[0237]
[0238] It can be seen from Table 1 that the adhesion, tensile strength, elongation at break and hardness of the polyurea anti-corrosion coating prepared in the embodiment of the present invention are better than those in the comparative example.
[0239] Table 2
[0240]
[0241]
[0242] It can be seen from Table 2 that the corrosion resistance of the polyurea anti-corrosion coating prepared in the embodiment of the present invention in neutral salt spray, 3wt% NaCl solution, 5wt% NaOH solution, and 5wt% H2SO4 solution is significantly better than that of the comparative example.
[0243] From the test data in Table 1 and Table 2 above, we can see that:
[0244] (1) By comparing the test results of Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3, it is found that the addition of bisphenol F epoxy resin and a stable rust-removing agent in the process of preparing the polyurea anti-corrosion coating component A of the present invention can enhance the adhesion of the coating by interacting with the surface of the metal substrate; at the same time, the service life of the prepared coating in a corrosive environment is extended, and failure phenomena such as detachment from the substrate and loss of adhesion during long-term corrosion are avoided.
[0245] (2) By comparing the test results of Example 1, Comparative Example 4, and Comparative Example 5, it is found that the addition of the modified graphene oxide in the process of preparing the polyurea anticorrosive coating component A of the present invention helps to improve the tensile strength, elongation at break, hardness and corrosion resistance of the coating, mainly due to the excellent impermeability, mechanical strength and stability of the two-dimensional layered structure of graphene. In addition, since the uniform dispersion of graphene oxide in the coating is an important prerequisite for exerting its various characteristics, the compatibility and dispersibility of the modified graphene oxide with the coating are significantly improved, and the reinforcement effect on the coating performance is more significant.
[0246] Test Example 3
[0247] The method described in Examples 1-10 and Comparative Examples 1-5 is implemented, except that the surface pretreatment of the metal substrate in step S4 is performed according to the following operations:
[0248] Surface pretreatment of metal substrate: place the metal substrate in a 3.5wt% NaCl solution and immerse and corrode it at 25°C for 14 days to make the surface of the metal substrate rusty. After taking out the rusty metal substrate, use acetone and ethanol to remove the surface grease, and then use 200 mesh and 400 mesh sandpaper to simply polish it.
[0249] With reference to the method described in standard GB / T 5210-2006, the bonding strength (adhesion) between each polyurea anti-corrosion coating and the rusted metal substrate was tested, and the results are shown in Table 3.
[0250] Table 3
[0251] Adhesion / MPa Example 1 15.7 Example 2 14.9 Example 3 15.3 Example 4 15.2 Example 5 15.0 Example 6 15.1 Example 7 15.5 Example 8 15.7 Example 9 15.2 Example 10 15.1 Comparative Example 1 13.5 Comparative Example 2 7.6 Comparative Example 3 6.2 Comparative Example 4 13.4 Comparative Example 5 12.9
[0252] From the test results in Table 3, it can be seen that the polyurea anticorrosive coating of the present invention still has good adhesion on the rusted metal surface. Among them, the stable rust-removing agent is the main functional filler, which can decompose at the interface to generate phosphate and chromate ions and metal rust to generate a heteropolyacid complex passivation layer with strong adhesion, enhance the combination of the polyurea coating and the base metal, so that it can be applied to the surface of rusted metal equipment.
[0253] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A modified graphene oxide, characterized in that: The modified graphene oxide is obtained by modifying graphene oxide with isocyanate silane.
2. The modified graphene oxide according to claim 1, characterized in that The isocyanate silane is 3-isocyanate propyl triethoxy silane and / or 3-isocyanate propyl trimethoxy silane.
3. The modified graphene oxide according to claim 1 or 2, characterized in that: The weight ratio of the graphene oxide to the isocyanate silane is 1:20 to 50, preferably 1:25 to 40.
4. A method for preparing the modified graphene oxide according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: (1) mixing graphene oxide with an organic solvent and subjecting it to ultrasonic treatment; (2) Under the protection of an inert atmosphere, the solution obtained in step (1) is mixed with isocyanate silane for reaction, and the solid-liquid separation is performed to obtain modified graphene oxide.
5. The method according to claim 4, characterized in that In step (1), the weight ratio of the graphene oxide to the organic solvent is 1:40 to 105, preferably 1:50 to 99; Preferably, the organic solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide and N,N-diethylformamide.
6. The method according to claim 4 or 5, characterized in that: In step (1), the ultrasonic conditions include: ultrasonic temperature of 15-30°C, ultrasonic time of 30-60 min, and ultrasonic frequency of 20-35 kHz.
7. The method according to any one of claims 4 to 6, characterized in that: The weight ratio of the graphene oxide to the isocyanate silane is 1:20 to 50, preferably 1:25 to 40.
8. The method according to any one of claims 4 to 7, characterized in that: In step (2), the reaction conditions include: reaction temperature of 60 to 100° C., and reaction time of 12 to 48 h.
9. A polyurea anticorrosive coating composition, characterized in that: The polyurea anticorrosive coating composition comprises a polyurea anticorrosive coating component A and a polyurea anticorrosive coating component B, wherein the polyurea anticorrosive coating component A and the polyurea anticorrosive coating component B are stored independently. The polyurea anticorrosive coating component A is prepared from raw materials containing aliphatic diisocyanate, aromatic diisocyanate, polyether polyol, bisphenol F epoxy resin, stable rust-reducing agent, ester viscosity reducer and modified graphene oxide, wherein the modified graphene oxide is the modified graphene oxide described in any one of claims 1 to 3 or the modified graphene oxide prepared by the method described in any one of claims 4 to 8; The polyurea anticorrosive coating component B is prepared from raw materials containing polyether polyamine, terminal amino chain extender, light stabilizer hindered amine, ultraviolet absorber and silane coupling agent.
10. The polyurea anticorrosive coating composition according to claim 9, characterized in that: The weight ratio of the aliphatic diisocyanate, the aromatic diisocyanate, the polyether polyol, the bisphenol F epoxy resin, the stable rust remover, the ester viscosity reducer and the modified graphene oxide is 30:28-44:24-38:5-10:6-15:1-2:0.5-2.
11. The polyurea anticorrosive coating composition according to claim 9 or 10, characterized in that: The weight ratio of the polyether polyamine, the amino-terminated chain extender, the light stabilizer hindered amine, the ultraviolet absorber and the silane coupling agent is 55:25-40:1-3:1-2:10-20.
12. The polyurea anticorrosive coating composition according to any one of claims 9 to 11, characterized in that: The aliphatic diisocyanate is one or more selected from the group consisting of hexamethylene diisocyanate, hexamethylene diisocyanate trimer, methyl formate pentamethylene diisocyanate and 2,2,4-trimethylhexane diisocyanate.
13. The polyurea anticorrosive coating composition according to any one of claims 9 to 12, characterized in that: The aromatic diisocyanate is selected from one or more of 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, p-phenylene diisocyanate, methylcyclohexyl diisocyanate, p-phenylene diisocyanate, diphenylmethane-4,4'-diisocyanate, 3,3'-dimethoxy-4,4'-diphenyl diisocyanate and hydrogenated phenylmethane diisocyanate.
14. The polyurea anticorrosive coating composition according to any one of claims 9 to 13, characterized in that: The molecular weight of the polyether polyol is 200 to 3000; Preferably, the polyether polyol is selected from one or more of polyoxypropylene ether glycol, polytetramethylene ether glycol, polyoxypropylene-oxyethylene glycol and tetramethylene ether glycol-oxypropylene copolymer glycol.
15. The polyurea anticorrosive coating composition according to any one of claims 9 to 14, characterized in that: The epoxy equivalent of the bisphenol F epoxy resin is 140 to 200 g / eq, preferably 150 to 190 g / eq.
16. The polyurea anticorrosive coating composition according to any one of claims 9 to 15, characterized in that: The stable rust-removing agent is selected from one or more of zinc phosphate, zinc chromate and aluminum dihydrogen tripolyphosphate.
17. The polyurea anticorrosive coating composition according to any one of claims 9 to 16, characterized in that: The ester viscosity reducer is selected from one or more of dioctyl phthalate, dibutyl phthalate, ethyl carbonate, propylene carbonate, propane sultone, 2-dimethylaminoethyl acetate, 2-chloroethyl ester and dimethylaminoethyl acrylate.
18. The polyurea anticorrosive coating composition according to any one of claims 9 to 17, characterized in that: The molecular weight of the polyether polyamine is 100-3000, preferably 200-2000.
19. The polyurea anticorrosive coating composition according to any one of claims 9 to 18, characterized in that: The terminal amino chain extender is selected from one or more of dimethylthiotoluenediamine, N,N'-di-sec-butyl-p-phenylenediamine, N,N'-dialkylphenylenediamine, N,N'-dialkylmethyldiamine, bis(p-aminobenzoic acid)propylene glycol ester, diethyltoluenediamine and methyldiethanolamine.
20. The polyurea anticorrosive coating composition according to any one of claims 9 to 19, characterized in that: The light stabilizer hindered amine is bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate and / or 4-benzoyloxy-2,2,6,6-tetramethylpiperidine.
21. The polyurea anticorrosive coating composition according to any one of claims 9 to 20, characterized in that: The ultraviolet absorber is selected from one or more of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(5-chloro-2-benzotriazolyl)-6-tert-butyl-p-cresol, 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole and 2-hydroxy-4-n-octylbenzophenone.
22. The polyurea anticorrosive coating composition according to any one of claims 9 to 21, characterized in that: The silane coupling agent is selected from one or more of γ-diethylenetriaminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, N-aminoethyl-3-aminopropylmethyldimethoxysilane and γ-aminoethylaminopropyltrimethoxysilane.
23. The polyurea anticorrosive coating composition according to any one of claims 9 to 22, characterized in that: The preparation method of the polyurea anticorrosive coating component A comprises: S1, dehydrating the polyether polyol; S2. Under normal pressure and inert atmosphere, the product obtained in step S1 is mixed with aliphatic diisocyanate, aromatic diisocyanate, bisphenol F epoxy resin, stable rust-reducing agent, ester viscosity reducer and modified graphene oxide for reaction.
24. The polyurea anticorrosive coating composition according to claim 23, characterized in that: In step S1, the conditions of the dehydration treatment include: pressure of -0.05 to -0.15 MPa, temperature of 100 to 120°C, and time of 2 to 3 hours.
25. The polyurea anticorrosive coating composition according to claim 24, characterized in that: In step S2, the reaction conditions include: reaction temperature of 70 to 100° C., preferably 80 to 90° C.; reaction time of 1 to 6 hours, preferably 2 to 4 hours.
26. The polyurea anticorrosive coating composition according to any one of claims 9 to 25, characterized in that: The preparation method of the polyurea anticorrosive coating component B comprises: 1) mixing the polyether polyamine and the amino-terminated chain extender and performing a dehydration treatment; 2) Under normal pressure and inert atmosphere, the product obtained in step 1) is mixed with a light stabilizer hindered amine, a UV absorber and a silane coupling agent to react.
27. The polyurea anticorrosive coating composition according to claim 26, characterized in that: In step 1), the conditions of the dehydration treatment include: pressure of -0.05 to -0.15 MPa, temperature of 90 to 110° C., and time of 2 to 3 hours.
28. The polyurea anticorrosive coating composition according to claim 26 or 27, characterized in that: In step 2), the reaction conditions include: reaction temperature of 50 to 80° C., preferably 60 to 75° C.; reaction time of 0.5 to 4 h, preferably 1 to 2 h.
29. A method for preparing a polyurea anticorrosive coating, characterized in that: The method comprises: mixing the polyurea anticorrosion coating component A and the polyurea anticorrosion coating component B, spraying the mixture on the surface of a metal substrate, and performing curing to obtain a polyurea anticorrosion coating.
30. The method according to claim 29, characterized in that The weight ratio of the polyurea anticorrosive coating component A to the polyurea anticorrosive coating component B is 1-1.2:1, preferably 1.05-1.15:
1.
31. The method according to claim 29 or 30, characterized in that The spraying conditions include: a spraying temperature of 60 to 80° C. and a spraying pressure of 14 to 16 MPa.
32. The method according to any one of claims 29 to 31, characterized in that: The curing conditions include: a curing temperature of 15 to 30° C. and a curing time of 5 to 9 days.
33. The method according to any one of claims 29 to 32, characterized in that: The metal substrate is carbon steel material for the outer wall of the storage tank.
Citation Information
Patent Citations
Preparation method of anticorrosive polyurea coating
CN102786870A
Epoxy-modified spray polyurea anticorrosive paint for surface of steel structure and preparation and using method of paint
CN102993929A
Solvent-free anticorrosive coating based on polyurea elastomer and preparation method of solvent-free anticorrosive coating
CN106928426A
Water-based two-component conversion type rusty anticorrosive paint and preparation method thereof
CN111393956A
Amino functionalized graphene modified polyurea long-acting anticorrosive coating layer and preparation method thereof
CN111500170A
Cited By
Polyurea heavy anti-corrosion coating
CN121592240A
High-strength corrosion-resistant coating, preparation method thereof and application of high-strength corrosion-resistant coating in automobile brake disc
CN121825378A