Hydrophobic anti-icing material with lubricating interface as well as preparation method and application of hydrophobic anti-icing material
Through the combination of rheological matrix materials and porous nano-SiO2 and other materials, the interface lubricating surface structure is designed, which solves the fragility and wear of superhydrophobic coatings in low temperature and high humidity environments, and achieves the combination of interface lubricating and durability, which significantly increases the degree of Improves anti-ice coating performance and mechanical and thermal stability of the coating.
Patent Information
- Application Number
- CN202411200709.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
The existing superhydrophobic coatings have problems such as structural fragility, wear failure and easy to be pinned in low temperature and high humidity environments, making it difficult to continuously exert anti-icing performance.
The rheological matrix material is used to prepare the interfacial lubricating surface material. Through the combination of porous nano SiO2 and fluorocarbon resin and other materials, a controllable coating structure is designed to achieve the combination of interface lubrication and durability, and organically modified silicon powder and diluents are used. To improve the mechanical properties and thermal stability of the coating.
The prepared interface lubricated hydrophobic anti-icing material has good self-cleaning characteristics, mechanical properties, thermal stability and anti-icing ability, which significantly improves anti-icing performance and reduces production cost and difficulty.
Smart Images

Figure CN118931268A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of coating materials, and in particular relates to a hydrophobic anti-icing material with interface lubrication, and a preparation method and application thereof. Background Art
[0002] The occurrence and accumulation of ice and ice coating in low temperature and high humidity environment will cause serious damage to industries such as road traffic, power transportation, air transportation, wind power generation, and even endanger life and cause serious property losses. In the power transportation industry, the damage caused by ice coating is particularly significant. The accumulation of ice greatly increases the weight of the wires, which can cause wire breakage, tower bending and even collapse. For surface ice accumulation and ice coating, the traditional deicing method is mainly an active method to treat the symptoms through pneumatic belt (airbag) deicing method, electric pulse deicing method, electric mechanical deicing, etc., but in many cases the operation is difficult and difficult to be applied in practice. Later, the thermal anti-icing / deicing method, that is, the anti-icing / deicing area is continuously heated or periodically heated by the heating element to achieve the purpose of anti-icing / deicing. Although the effect is significant, the energy consumption is very large.
[0003] In recent years, in order to break through the limitations of the above passive anti-icing, anti-icing coating materials based on the concept of active anti-icing have become a research hotspot at home and abroad. Super-hydrophobic surfaces can delay the formation of ice crystals on the surface and are used as anti-icing surfaces. It is expected to achieve the purpose of inhibiting or preventing the formation of surface ice and effectively removing surface ice. The reason is that super-hydrophobic surfaces have a very good repelling effect on water, with a high water contact angle and a low rolling angle, which makes water roll off the surface to prevent water adhesion.
[0004] The super-hydrophobic coatings currently under development have problems such as fragile structure, wear failure, and ice pinning. Considering the delayed icing characteristics of super-hydrophobic coatings, designing and preparing anti-icing coatings that are both hydrophobic and have low ice layer shear force is an effective way to solve the above problems. The traditional conventional method is to use the design idea of doping with modified substances. Although the prepared hydrophobic materials have good hydrophobicity, their wear resistance and easy deicing ability are poor, and the anti-icing performance cannot be continuously exerted. Summary of the invention
[0005] The purpose of the present invention is to develop an anti-icing coating material with good anti-icing performance and practicality for low-temperature application environments. A method is proposed to prepare a rheological matrix material into a functional dominant design interface lubrication surface material, construct a structure-controllable surface design method and a "bottom-up" lubricable composite material preparation strategy, and realize an application based on an interface lubrication with integrated anti-icing performance and durability performance.
[0006] The specific technical solutions are as follows:
[0007] A method for preparing a hydrophobic anti-icing material with interface lubrication comprises the following steps:
[0008] (1) Take a reaction device and add silicone oil, then take silicon micropowder and evenly disperse it in the silicone oil;
[0009] (2) adding the coating resin to the reaction device described in step (1), then adding a diluent and stirring the reaction for 5-10 minutes;
[0010] (3) Then take the curing agent and add it to the reaction device, stir and react for 10-20 minutes;
[0011] (4) The prepared coating is coated on a substrate and dried and cured at 80-100° C. for 1-2 hours to obtain a hydrophobic anti-icing material with a lubricated interface.
[0012] Preferably, the silicon micropowder in step 1) is modified porous nano-SiO2, and the mass ratio of the silicon micropowder in the silicone oil is 10%-80%.
[0013] Preferably, the coating resin in step 2) is a single FEVE type fluorocarbon resin, or a combined mixed resin of a FEVE type fluorocarbon resin and any one or more of PAA, PU and PDMS.
[0014] Preferably, the diluent in step 2) is butyl acetate, and the mass ratio of the coating resin to the diluent is 1:1-2.
[0015] Preferably, the curing agent in step 3) includes one or more of blocked isocyanate, hexamethylene diisocyanate, and elastic polyisocyanate.
[0016] Preferably, the mass ratio of the silicon powder to the coating resin is 1:4-12.
[0017] Preferably, when the coating resin in step 2) is a single FEVE-type fluorocarbon resin, the mass ratio of the FEVE-type fluorocarbon resin to the curing agent is 1:1-3; when the coating resin in step 2) is a combined mixed resin of a FEVE-type fluorocarbon resin and any one or more of PAA, PU and PDMS, the mass ratio of the FEVE-type fluorocarbon resin to the curing agent is 1:1-3, the mass ratio of PAA to the curing agent is 2:1, the mass ratio of PU to the curing agent is 1:1, and the mass ratio of PDMS to the curing agent is 10:1.
[0018] Preferably, the coating method in step (4) is ordinary brush coating, scraper coating or spin coating. If there are many bubbles after the coating is prepared, it needs to be dried under vacuum conditions. The prepared coating is placed in a vacuum drying oven and evacuated for 10 minutes.
[0019] The invention discloses a hydrophobic anti-icing material with interface lubrication obtained by the preparation method.
[0020] The above-mentioned hydrophobic anti-icing material with interface lubrication is applied to a metal surface, an alloy surface, a composite material surface or a non-metallic material surface.
[0021] The beneficial effects of the present invention are as follows: the wear-resistant hydrophobic anti-icing material prepared by the porous microstructure oil immersion method has good self-cleaning properties. The technical solution of the present invention adds modified nano-SiO2 to the resin base to improve the durability of the coating. Butyl acetate is used as a diluent, so that the coating has good high-temperature stability. The present invention adopts organic modified silicon powder, and the sliding of the organic silicon molecular chain promotes the enhancement of the interface slip between ice and the surface, thereby improving the anti-icing performance. By adopting a mixed resin matrix material, the volatilization rate of silicone oil is delayed, and the durability of the coating is improved. By optimizing the preparation process of the fluorocarbon resin-based lubricating coating, optimizing the addition ratio of porous nano-silicon dioxide, silicone oil, and diluent, the anti-icing performance of the prepared lubricating coating is greatly improved. In addition, the coating prepared by the present invention has low production cost and low difficulty. The prepared hydrophobic anti-icing material with interface lubrication has good mechanical properties, thermal stability, self-cleaning ability and anti-icing ability. This coating material with excellent comprehensive performance has taken a key step on the road of application, which is conducive to promoting the development of advanced functional coating technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0023] Figure 1 Schematic diagram of the characteristics of hydrophobic and lipophilic modified silica powder;
[0024] Figure 2 A flow chart showing the preparation of a single fluorocarbon resin-based interface lubricating coating;
[0025] Figure 3 Figures showing the morphological characteristics of silicon micropowder and coating with and without silicone oil. a is the porous surface structure of silicon micropowder without silicone oil, b is the surface structure of Example 1, c is the surface structure of micropowder with silicone oil, and d is the surface structure of Example 2;
[0026] Figure 4 It shows the wettability and self-cleaning process of the lubricating coating in Example 2;
[0027] Figure 5 The anti-icing performance characterization diagram is shown in FIG. a, the ice delay process of the sample in Example 1, and b, the ice delay process of the sample in Example 2;
[0028] Figure 6Indicates the mechanical durability of the coating. a, the surface morphology of the sample in Example 2 after 100 cycles of wear, b, the surface morphology of the sample in Example 2 after being placed at 80°C for 7 days;
[0029] Figure 7 A flow chart showing the preparation of a hybrid resin-based interface lubricating coating. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in combination with comparative examples and examples. It should be understood that the specific examples described herein are only used to explain the present invention and are not intended to limit the present invention.
[0031] In the present technical solution, FEVE represents FEVE type fluorocarbon resin, which is a thermosetting coating resin copolymerized by fluoroolefin and alkyl vinyl ether or alkyl vinyl ester, PAA represents polyacrylic resin, PU represents polyurethane resin, and PDMS represents polydimethylsiloxane resin.
[0032] Preparation of modified porous nano-SiO2: add 8 ml of deionized water and 4 ml of ammonia water to 80 ml of ethanol, and then add 1.2 g of chain silica sol, and stir magnetically for 10 minutes to mix evenly; use a pipette to drop 0.6 ml of tetraethyl orthosilicate and continue to stir magnetically for 20 minutes; use a pipette to slowly drop 0.6 ml of n-octyltriethoxysilane into the above mixture, and stir magnetically for 24 hours in a 50°C water bath to obtain a super-hydrophobic and super-oleophilic solution. Place the above solution in an oven at 80°C and dry it for 12 hours. After grinding and sieving the dried block, you can get super-hydrophobic and super-oleophilic silicon micropowder, that is, modified porous nano-SiO2, for later use. The hydrophobic and oleophilic test results are as follows: Figure 1 shown.
[0033] Example 1
[0034] The preparation process of hydrophobic anti-icing material with single resin-based interface lubrication is as follows: Figure 2 , the specific process is as follows:
[0035] (1) Weigh 1g of silicon powder (modified porous nano-SiO2) and place it in a beaker. At this time, the proportion of silicone oil mixed is 0%;
[0036] (2) Drop 10g of FEVE fluorocarbon resin into the beaker with the oil storage particles prepared, and at the same time drop 10g of butyl acetate, a diluent, in a 1:1 ratio to the total mass of the resin, into the beaker. Then put in a rotor, seal it with plastic wrap, and stir it on a magnetic stirrer for 5-10 minutes.
[0037] (3) Add curing agent isocyanate to the above mixed solution. The mass ratio of the added curing agent to the FEVE type fluorocarbon resin is 1:3, so add about 3.3g of curing agent, seal again, and stir magnetically for more than 10 minutes until the silicon powder is dispersed more evenly.
[0038] (4) After the coating is prepared, the coating is applied to a glass slide using a drop coating method. Each prepared coating is applied to the substrate material. After the coating is smooth, it is placed in a vacuum oven, vacuumed for 10 minutes, set at 80°C, and placed for 2 hours to cure to complete the coating preparation. The anti-icing performance and mechanical properties of the prepared coating material are shown in Table 1.
[0039] Table 1 Anti-icing performance and mechanical properties of the coating in Example 1
[0040]
[0041] Example 2
[0042] The preparation process of hydrophobic anti-icing material with single resin-based interface lubrication is as follows: Figure 2 , the specific process is as follows:
[0043] (1) Weigh 1g of silicon micropowder (modified porous nano-SiO2) and place it in a beaker. The ratio of silicone oil mixed is 10%. Then use a spoon to stir it into the porous silicon micropowder that is not dispersed separately, so that the silicone oil can be fully diffused and adsorbed into the silicon micropowder.
[0044] (2) Drop 10g of FEVE fluorocarbon resin into the beaker with the oil storage particles prepared, and at the same time drop 10g of butyl acetate, a diluent, in a ratio of 1:1 to the total amount of resin, into the beaker. Then put in a rotor, seal it with plastic wrap, and stir it on a magnetic stirrer for 5-10 minutes.
[0045] (3) Add curing agent to the above mixed solution. The ratio of curing agent to FEVE is 1:3, so add about 3.3g of curing agent, seal again, and stir magnetically for more than 10 minutes until the silica powder is dispersed more evenly.
[0046] (4) After the coating is prepared, the coating is applied on a glass slide using a drop coating method. Each prepared coating is applied on a base material. After the coating is flattened, it is placed in an oven at 80°C for 2 hours to cure, completing the preparation of the coating. The anti-icing performance and mechanical properties of the prepared coating material are shown in Table 2.
[0047] Figure 3 for
[0048] Table 2 Anti-icing performance and mechanical properties of the coating in Example 2
[0049]
[0050]
[0051] Figure 3 Figure 3 shows the morphological characteristics of silicon micropowder and coating with and without silicone oil. a is the porous surface structure of silicon micropowder without silicone oil, b is the surface structure of Example 1, c is the surface structure of micropowder with silicone oil, and d is the surface structure of Example 2.
[0052] Figure 4 It shows the wettability and self-cleaning process of the lubricating coating in Example 2;
[0053] Figure 5 The anti-icing performance characterization diagram is shown in FIG. a, the ice delay process of the sample in Example 1, and b, the ice delay process of the sample in Example 2;
[0054] Figure 6 The mechanical durability of the coating is shown in Fig. a. Surface morphology of the sample in Example 2 after 100 cycles of wear, and b. Surface morphology of the sample in Example 2 after being placed at 80°C for 7 days.
[0055] From the test results of the anti-icing performance and mechanical properties of the coatings prepared in Examples 1-2, it can be found that the silicon micropowder is first dissolved in silicone oil before mixing with the fluorocarbon resin. This improves the dispersibility of the silicon micropowder, effectively promotes the coating hardness of the final prepared hydrophobic anti-icing material, increases the contact angle of water droplets on the coating surface, enhances the hydrophobicity of the coating, and can significantly reduce the shear force of the ice layer, which has a good effect on improving the anti-icing performance of the coating.
[0056] Comparative Example 1
[0057] The difference from Example 1 is that the silicon powder used in this example is ordinary unmodified SiO2. The anti-icing performance and mechanical properties of the prepared coating are shown in Table 3.
[0058] Table 3 Comparative Example 1 Anti-icing performance and mechanical properties of the coating
[0059]
[0060] From the test results of the anti-icing performance and mechanical properties of the coatings prepared in Example 1 and Comparative Example 1, it can be found that the modification process of silicon micropowder can effectively increase the contact angle of water droplets on the coating surface, indicating that the hydrophobicity of the coating is enhanced, and it has a promoting effect on reducing the shear force of the ice layer and improving the anti-icing performance of the coating.
[0061] Example 3
[0062] The preparation process of the hybrid resin-based interfacially lubricated hydrophobic anti-icing material is as follows: Figure 7 , the specific process is as follows:
[0063] (1) Weigh 1g of silicon micropowder and place it in a beaker. The ratio of the mixed silicone oil is 40%. Then use a medicine spoon to stir it into the porous silicon micropowder that is not dispersed separately, so that the silicone oil can be fully diffused and adsorbed into the silicon micropowder.
[0064] (2) Add 2.5g of fluorocarbon resin FEVE (A) and 2.5g of PAA (A) to the beaker with the prepared oil storage particles, and at the same time, add 5g of butyl acetate, a diluent, in a ratio of 1:1 to the total amount of resin. Then put in a rotor, seal it with plastic wrap, and stir it on a magnetic stirrer for 5-10 minutes.
[0065] (3) Add curing agent to the above mixed solution. The addition ratio of different resins and their corresponding curing agents is different. The mass ratio of FEVE: curing agent (isocyanate) is 3:1, and the mass ratio of PAA: curing agent (hexamethylene diisocyanate) is 2:1. After adding the curing agent, seal it again and stir it magnetically for more than 10 minutes until the silica powder is dispersed more evenly.
[0066] The coating was applied on a glass slide using a drop coating method. Each prepared coating was applied on the substrate material. After the coating was leveled, it was placed in a vacuum oven, vacuumed for 10 minutes, set at 80°C, and left to cure for 2 hours. The prepared coating had good anti-icing properties and mechanical properties as shown in Table 4.
[0067] Table 4 Anti-icing performance and mechanical properties of the coating in Example 3
[0068]
[0069] Example 4
[0070] The preparation process of the hybrid resin-based interfacially lubricated hydrophobic anti-icing material is as follows: Figure 7 , the specific process is as follows:
[0071] (1) Weigh 1g of silicon micropowder and place it in a beaker. The mass ratio of the mixed silicone oil is 60%. Then use a medicine spoon to stir it into the porous silicon micropowder that is not dispersed separately, so that the silicone oil can be fully diffused and adsorbed into the silicon micropowder.
[0072] (2) Add 2.5g of fluorocarbon resin FEVE (A) and 2.5g of PU (A) to the beaker with the oil storage particles, and at the same time, add 5g of butyl acetate, a diluent, in a ratio of 1:1 to the total amount of resin. Then put in a rotor, seal it with plastic wrap, and stir it on a magnetic stirrer for 5-10 minutes.
[0073] (3) Add curing agent to the above mixed solution. The addition ratio of different resins and their curing agents is different. The mass ratio of FEVE: curing agent (isocyanate) is 3:1, and the mass ratio of PU: curing agent (hexamethylene diisocyanate) is 1:1. After adding the curing agent, seal it again and stir it magnetically for more than 10 minutes until the silicon powder is dispersed more evenly. Use the drop coating method to apply the coating on the glass slide. Each prepared coating is applied on the base material separately. After the coating is flat, put it in an oven, set it to 80℃, and leave it for 2 hours to cure. The prepared coating has good anti-icing performance and mechanical properties as shown in Table 5.
[0074] Table 5 Anti-icing performance and mechanical properties of the coating in Example 4
[0075]
[0076] Example 5
[0077] The preparation process of the hybrid resin-based interfacially lubricated hydrophobic anti-icing material is as follows: Figure 7 , the specific process is as follows:
[0078] (1) Weigh 1g of silicon micropowder and place it in a beaker. The ratio of the mixed silicone oil is 80%. Then use a medicine spoon to stir it into the porous silicon micropowder that is not dispersed separately, so that the silicone oil can be fully diffused and adsorbed into the silicon micropowder.
[0079] (2) Add 2.5g of fluorocarbon resin FEVE (A) and 2.5g of PDMS (A) to the beaker with the prepared oil storage particles, and at the same time, add 5g of butyl acetate, a diluent, in a ratio of 1:1 to the total amount of resin. Then put in a rotor, seal it with plastic wrap, and stir it on a magnetic stirrer for 5-10 minutes.
[0080] (3) Add curing agent to the above mixed solution. The addition ratio of different resins and their curing agents is different. The mass ratio of FEVE: curing agent (isocyanate) is 3:1, and the mass ratio of PDMS: curing agent (elastic polyisocyanate) is 10:1. After adding the curing agent, seal it again and stir it magnetically for more than 10 minutes until the silicon powder is dispersed more evenly. Use the drop coating method to apply the coating on the glass slide. Each prepared coating is applied on the base material separately. After the coating is flat, put it in an oven, set it to 80℃, and leave it for 2 hours to cure. The prepared coating has good anti-icing performance and mechanical properties as shown in Table 6.
[0081] Table 6 Anti-icing performance and mechanical properties of the coating in Example 5
[0082]
[0083] It can be found from Examples 3-5 that the use of a mixed resin matrix material can further slow down the volatilization rate of silicone oil, improve the durability of the coating, further enhance the hydrophobicity of the coating, and further enhance the effect of reducing the shear force of the ice layer and the anti-icing performance of the coating.
Claims
1. A method for preparing a hydrophobic anti-icing material with interface lubrication, characterized in that: The following steps are involved: (1) Take a reaction device and add silicone oil, then take silicon micropowder and evenly disperse it in the silicone oil; (2) adding the coating resin to the reaction device described in step (1), then adding a diluent and stirring the reaction for 5-10 minutes; (3) Then take the curing agent and add it to the reaction device, stir and react for 10-20 minutes; (4) The prepared coating is coated on a substrate and dried and cured at 80-100° C. for 1-2 hours to obtain a hydrophobic anti-icing material with a lubricated interface.
2. The method for preparing a hydrophobic anti-icing material with interface lubrication according to claim 1, characterized in that: Step 1) The silicon micropowder is modified porous nano-SiO2, and the mass ratio of the silicon micropowder in the silicone oil is 10%-80%.
3. The method for preparing a hydrophobic anti-icing material with interface lubrication according to claim 1, characterized in that: Step 2) The coating resin is a single FEVE type fluorocarbon resin, or a combination of a FEVE type fluorocarbon resin and any one or more of PAA, PU and PDMS.
4. The method for preparing a hydrophobic anti-icing material with interface lubrication according to claim 1, characterized in that: Step 2) The diluent is butyl acetate, and the mass ratio of the coating resin to the diluent is 1:1-2.
5. The method for preparing a hydrophobic anti-icing material with interface lubrication according to claim 1, characterized in that: Step 3) The curing agent includes one or more of blocked isocyanate, hexamethylene diisocyanate, and elastic polyisocyanate.
6. The method for preparing a hydrophobic anti-icing material with interface lubrication according to claim 1, characterized in that: The mass ratio of the silicon powder to the coating resin is 1:4-12.
7. The method for preparing a hydrophobic anti-icing material with interface lubrication according to claim 1, characterized in that: When the coating resin in step 2) is a single FEVE type fluorocarbon resin, the mass ratio of the FEVE type fluorocarbon resin to the curing agent is 1:1-3; when the coating resin in step 2) is a combined mixed resin of a FEVE type fluorocarbon resin and any one or more of PAA, PU and PDMS, the mass ratio of the FEVE type fluorocarbon resin to the curing agent is 1:1-3, the mass ratio of PAA to the curing agent is 2:1, the mass ratio of PU to the curing agent is 1:1, and the mass ratio of PDMS to the curing agent is 10:
1.
8. The method for preparing a hydrophobic anti-icing material with interface lubrication according to claim 1, characterized in that: The coating method in step (4) is ordinary brush coating, scraper coating or spin coating. If there are many bubbles after the coating is prepared, it needs to be dried under vacuum conditions. The prepared coating is placed in a vacuum drying oven and evacuated for 10 minutes.
9. A hydrophobic anti-icing material with interface lubrication obtained according to the preparation method of claims 1-8.
10. Application of an interfacially lubricated hydrophobic anti-icing material coated on a metal surface, an alloy surface, a composite material surface or a non-metallic material surface.
Citation Information
Patent Citations
Hydrophobic coating and preparation method thereof
CN104559522A
Long-acting anti-icing coating as well as preparation method and application thereof
CN112341873A
Preparation method of anti-icing durable super-hydrophobic coating layer
CN113980576A