Liquid resin composition

By using the film formed by the liquid resin composition, the existing thermal insulation film oxidation corrosion and residual glue problems are solved, and efficient infrared and ultraviolet light barriers are achieved, high visible light penetration and flexibility are maintained, and the service life of the article is extended. Provides surface protection.

CN118931276APending Publication Date: 2024-11-12SWANSON TECH CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410318314.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-08-28
Filing Date
2024-03-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing thermal insulation films are prone to oxidation or corrosion after use for a period of time, resulting in poor thermal insulation effect and may leave residual glue during tearing or cause damage to the surface of the article.

Method used

A liquid resin composition containing 20 to 80 wt% of self-crosslinked acrylic or polyurethane resin, 1 to 10 wt% of heat insulating particles and 5 to 25 wt% of aqueous solvent, forming a film that is easy to tear off, the film is It has high visible light penetration and flexibility after drying, and no residual glue remains after tearing.

Benefits of technology

The film can effectively block infrared and ultraviolet light, while maintaining high visible light penetration, with good flexibility and easy to tear off, extending the service life of the item and providing surface protection, while not during construction and tear off. Left residual glue, achieving natural indoor cooling and energy saving and carbon reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931276A_ABST
    Figure CN118931276A_ABST
Patent Text Reader

Abstract

The present invention provides a liquid resin composition comprising (a) 20 to 80 wt% of a resin selected from a group consisting of a self-crosslinking acrylic resin and a polyurethane resin, the resin having a Tg of-20 to 25 DEG C, (b) 1 to 10 wt% of heat-insulating particles, and (c) 5 to 25 wt% of an aqueous solvent. The liquid resin composition can be further coated on a substrate and dried to form a film. The film formed by the liquid resin composition can block infrared light and ultraviolet light and maintain high visible light penetration rate, so that the film has visual transparency and can block radiant heat energy of sunlight and the effect of ultraviolet light; therefore, the purposes of naturally cooling indoors, saving energy, reducing carbon, prolonging the service life of articles, providing a surface protection effect and the like can be achieved. In addition, the film provided by the invention is convenient in construction and tearing operation, and no residual glue is formed on the surface of a coated object.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid resin composition, which can be formed into an easily removable film, particularly a liquid heat-insulating film; however, the present invention is not limited thereto. [Background technology]

[0002] Nowadays, many buildings use glass doors and windows, which are not only beautiful but also allow sunlight to penetrate into the room, making the environment bright. However, too much light exposure will accelerate the aging of items in the building, such as furniture, decorations, and carpets, thereby shortening the service life of the items. This situation is also quite common in cars, and when sunlight shines into the car, it may cause dazzle when driving, and high temperature may cause the car windows to burst.

[0003] Therefore, a layer of thermal insulation film is usually pasted on the windows of buildings or vehicles for heat insulation and UV protection. Generally, thermal insulation film is a metal film made of metal compounds, which can effectively produce functions such as heat insulation, infrared or UV resistance, etc. However, after a period of use, the metal film is prone to oxidation or corrosion, resulting in poor thermal insulation effect; in addition, the subsequent replacement of the thermal insulation film may also produce residual glue or damage the surface of the object due to its inconvenience in tearing off. [Summary of the invention]

[0004] In view of the shortcomings of the prior art, the present invention provides a liquid resin composition that can be applied to the surface of an object and formed into a film after drying, and then arranged into various multi-layer structures. The film can not only effectively block infrared light and ultraviolet light while maintaining high visible light transmittance, but also has high flexibility and is easy to tear off; furthermore, the film of the present invention will not form residual glue on the surface, and can also clean the surface of the object after being torn off.

[0005] Accordingly, the present invention provides a liquid resin composition on one hand, which comprises: (a) 20 to 80 wt % of a resin selected from the group consisting of a cross-linked acrylic resin and a polyurethane resin, and the Tg of the resin is -20 to 25°C, (b) 1 to 10 wt % of thermal insulation particles and (c) 5 to 25 wt % of an aqueous solvent.

[0006] According to at least one embodiment of the present invention, the thermal insulation particles are cesium tungsten oxide.

[0007] According to at least one embodiment of the present invention, the aqueous solvent is selected from the group consisting of water, short-chain esters, ethers, and alcohols.

[0008] According to at least one embodiment of the present invention, the composition further comprises an auxiliary agent selected from the group consisting of a UV absorber, a UV stabilizer, a thickener, a leveling agent, a rheological agent and a defoaming agent.

[0009] According to at least one embodiment of the present invention, the auxiliary agent is a UV absorber or a UV stabilizer, and accounts for 1 to 3 wt % of the liquid resin composition.

[0010] According to at least one embodiment of the present invention, the auxiliary agent is a leveling agent, and accounts for 0.01 to 7 wt % of the liquid resin composition.

[0011] According to at least one embodiment of the present invention, the auxiliary agent is a rheological agent, and accounts for 0.1 to 5 wt % of the liquid resin composition.

[0012] According to at least one embodiment of the present invention, the auxiliary agent is a defoaming agent, and the auxiliary agent accounts for 0.05 to 3 wt % of the liquid resin composition.

[0013] Another aspect of the present invention provides a film that can be torn off on a substrate, wherein the film is formed by coating the above-mentioned liquid resin composition on the substrate and drying it.

[0014] According to at least one embodiment of the present invention, the substrate is glass, polycarbonate or acrylic resin.

[0015] According to at least one embodiment of the present invention, the film has a thickness of 10 to 50 μm.

[0016] According to at least one embodiment of the present invention, the film has a visible light transmittance of 70 to 90%.

[0017] According to at least one embodiment of the present invention, the film has an infrared light blocking rate of 60 to 99%.

[0018] According to at least one embodiment of the present invention, the film has an ultraviolet light blocking rate of 45 to 95%.

[0019] According to at least one embodiment of the present invention, the film has a solar total transmittance (SHGC) of 0.4 to 0.67.

[0020] In another aspect, the present invention provides a multilayer structure comprising the above-mentioned film, wherein the multilayer structure is a wall material, a roof material, a window of a building or structure, or a window of a vehicle.

[0021] The film formed by the liquid resin composition of the present invention can block infrared light and ultraviolet light, while maintaining a high visible light transmittance, thus having visual transparency and being able to block the radiant heat energy and ultraviolet light of sunlight; thereby, the present invention can achieve the purposes of natural indoor cooling, energy saving and carbon reduction, extending the service life of articles, and providing surface protection effects. In addition, the film of the present invention is convenient in construction and removal operations, and no residual glue will be formed on the surface of the coated object, and after removal, it has the additional effect of making the surface of the object clean.

Brief Description of the Drawings

[0022] Embodiments of the present invention will now be described by way of example only with reference to the accompanying drawings, in which:

[0023] Figure 1 is a photograph of a film formed by a liquid resin composition according to an embodiment of the present invention;

[0024] Figure 2 is a schematic diagram of a continuous sunlight device according to an embodiment of the present invention;

[0025] Figure 3 is the continuous sunshine cooling capacity result of the membrane according to one embodiment of the present invention;

[0026] Figures 4A to 4C is the cooling capacity result of different film thicknesses according to an embodiment of the present invention;

[0027] It should be understood that aspects of the present invention are not limited to the configurations, instrumentalities, and characteristics shown in the drawings. [Specific implementation method]

[0028] According to the usual working method, the various features and components in the figure are not drawn according to the actual scale, and the drawing method is to present the specific features and components related to the present invention in the best way. In addition, the same or similar component symbols are used to refer to similar components and parts between different figures.

[0029] The following embodiments should not be considered to unduly limit the present invention. A person with ordinary knowledge in the technical field to which the present invention belongs may modify and change the embodiments discussed herein without departing from the spirit or scope of the present invention, and still fall within the scope of the present invention.

[0030] In this document, unless the context otherwise states, the terms "comprise", "include", "have" or "contain" are inclusive or open, and do not exclude other undescribed elements or method steps; the terms "a" and "the" can be interpreted as singular or plural; the term "one or more" means "at least one", and thus can include a single feature or a mixture / combination. In addition, in this specification and the attached patent scope, unless otherwise stated, "disposed on something" can be regarded as directly or indirectly contacting the surface of something by attachment or other forms, and the definition of the surface should be judged according to the context / paragraph meaning of the specification content and the common knowledge in the field to which the specification belongs.

[0031] The present invention provides a liquid resin composition, which comprises: (a) 20 to 80 wt% of a resin selected from a group consisting of a self-crosslinking acrylic resin and a polyurethane resin, and the Tg (glass transition temperature, hereinafter referred to as Tg) of the resin is -20 to 25°C, (b) 1 to 10 wt% of thermal insulation particles and (c) 5 to 25 wt% of an aqueous solvent.

[0032] Specifically, the (a) 20 to 80 wt% of the resin is, for example but not limited to, between any two of the following values: 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt%, 70 wt%, 75 wt% or 80 wt%; and the Tg of the resin is -20 to 25°C, for example but not limited to, between any two of the following values: -20°C, -19°C, -18°C, -17°C, -16°C, -15°C, -14°C, -13°C, -12°C, -11°C, -10°C, -9°C, -8°C, -7°C, -6°C, -5°C, -4°C, -3°C, -2°C, -1°C, 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C and 25°C.

[0033] Specifically, the (b) 1 to 10 wt% of heat-insulating particles may be, for example but not limited to, between any two of the following values: 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt%. In addition, the (c) 5 to 25 wt% of aqueous solvent may be, for example but not limited to, between any two of the following values: 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt% and 25 wt%.

[0034] According to an embodiment of the present invention, the resin can be selected from a variety of polymer resins, including polyester, acrylic resin, modified acrylic resin, epoxy resin, silicone resin, polyurethane resin, fluorine-containing resin, starch, cellulose, or copolymers or mixtures thereof. In a preferred embodiment, the resin is selected from the group consisting of self-crosslinking acrylic resin and polyurethane resin; more preferably, the resin is polyurethane resin, so as to have more ideal material compatibility, optical transparency, removability and fingerprint resistance.

[0035] According to one embodiment of the present invention, the thermal insulation particles include titanium dioxide (TiO2), mica, indium tin oxide (ITO), antimony tin oxide (ATO), tungsten oxide or cesium tungsten oxide. In a preferred embodiment, the thermal insulation particles are cesium tungsten oxide to have more ideal optical blocking and visible light transmittance. According to one embodiment of the present invention, the particle size of the thermal insulation particles is 10 to 50 nm, for example but not limited to any two of the following values: 10 nm, 13 nm, 15 nm, 18 nm, 20 nm, 22 nm, 24 nm, 25 nm, 27 nm, 30 nm, 31 nm, 34 nm, 35 nm, 36 nm, 39 nm, 40 nm, 42 nm, 43 nm, 45 nm, 46 nm, 47 nm, 48 nm, 49 nm and 50 nm.

[0036] The "aqueous solvent" described herein refers to any solvent that is inactive to other components of the present invention, and it meets the requirements of environmental protection and safety and non-toxicity, and can be used in an indoor air circulation environment. According to one embodiment of the present invention, the aqueous solvent is selected from a group consisting of water, short carbon chain esters, ethers and alcohols, such as but not limited to: esters, alcohols, glycol dimethyl ether, propylene glycol monomethyl ether and propylene glycol mono-tert-butyl ether, ketones and mixtures thereof. In some embodiments, water includes deionized water and / or distilled water. In some embodiments, the solvent is propylene glycol monomethyl ether (PGME), methanol, ethanol, glycol ether (e.g., diethyl, tert-butyl ether, cyclic ether), glycol, ketone (e.g., acetone) or a mixture thereof. In some embodiments, the aqueous solvent contains almost no volatile organic solvents such as aliphatic hydrocarbons, ethyl acetate, glycol ethers and acetone (e.g., less than 1000ppm, less than 100ppm, less than 10ppm, less than 1ppm).

[0037] According to one embodiment of the present invention, the composition further comprises an auxiliary agent, which is selected from the group consisting of UV absorbers, UV stabilizers, thickeners, leveling agents, rheological agents and defoamers. Among them, without being limited by a specific theory, the UV absorber or UV stabilizer can enhance the ultraviolet light blocking ability of the liquid window film; in addition, without being limited by a specific theory, the thickener, leveling agent, rheological agent and defoamer can improve the stability of the coating film.

[0038] According to one embodiment of the present invention, the auxiliary agent comprises a UV absorber or a UV stabilizer, and the UV absorber or the UV stabilizer accounts for 1 to 3wt% of the liquid resin composition, for example but not limited to between any two of the following values: 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt% and 3wt%.

[0039] According to one embodiment of the present invention, the auxiliary agent comprises a leveling agent, and the leveling agent accounts for 0.01 to 7wt% of the liquid resin composition, for example but not limited to any two of the following values: 0.01wt%, 0.05wt%, 0.1wt%, 0.3wt%, 0.5wt%, 0.7wt%, 0.9wt%, 1wt%, 1.3wt%, 1.5wt%, 1.7wt%, 1.9wt%, 2wt%, 2.1wt%, 2.3wt%, 2.5wt% %, 2.5wt%, 2.7wt%, 3wt%, 3.1wt%, 3.3wt%, 3.5wt%, 3.7wt%, 3.9wt%, 4.1wt%, 4.3wt%, 4.5wt%, 4.7wt%, 4.9wt%, 5.1wt%, 5.3wt%, 5.5wt%, 5.7wt%, 5.9wt%, 6wt%, 6.1wt%, 6.3wt%, 6.5wt%, 6.7wt%, 6.9wt% and 7wt%. According to a preferred embodiment of the present invention, the leveling agent accounts for 0.05 to 6.5wt% of the liquid resin composition.

[0040] As used herein, a "rheological agent" is a compound or composition added to adjust the rheology of a formulation. For example, the rheological agent can improve the sagging resistance of the coating by providing a rapid but controlled increase in viscosity after application, and improve the transportability and storage of the coating by helping to prevent the settling of pigments or other solids in the formulation. In some embodiments, the rheological agent can be inorganic, such as clay, fumed silica, and specialty clays (e.g., sepiolite, attapulgite, and smectite). In some embodiments, the rheological agent can be organic, such as cellulosic materials and synthetic materials (e.g., hydrophobically modified polyurethanes, hydrophobically modified polyethers, alkali-swellable emulsions, and castor oil thixotropes). According to one embodiment of the present invention, the auxiliary agent comprises a rheological agent, and the rheological agent accounts for 0.1 to 5wt% of the liquid resin composition, for example but not limited to any two of the following values: 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, 2.1wt% %, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt%, 3wt%, 3.1wt%, 3.2wt%, 3.3wt%, 3.4wt%, 3.5wt%, 3.6wt%, 3.7wt%, 3.8wt%, 3.9wt%, 4wt%, 4.1wt%, 4.2wt%, 4.3wt%, 4.4wt%, 4.5wt%, 4.6wt%, 4.7wt%, 4.8wt%, 4.9wt% or 5wt%. According to a preferred embodiment of the present invention, the rheological agent accounts for 0.2 to 4.5wt% of the liquid resin composition.

[0041] The "defoaming agent" described herein refers to a chemical additive that reduces and hinders the formation of foam. The additive can be one or more compound formulations. According to one embodiment of the present invention, the auxiliary agent includes a defoaming agent, and the defoaming agent accounts for 0.05 to 3wt% of the liquid resin composition, such as but not limited to any two of the following values: 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, 1wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt%, 2wt%, 2.1wt%, 2.2wt%, 2.3wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.7wt%, 2.8wt%, 2.9wt% or 3wt%. According to a preferred embodiment of the present invention, the defoaming agent accounts for 1 to 1.5wt% of the liquid resin composition.

[0042] Another aspect of the present invention provides a film that can be peeled off from a substrate, wherein the film is formed by coating the above-mentioned liquid resin composition on a substrate and drying it. Figure 1 According to one embodiment of the present invention, the coating method is, for example, roller coating, brush coating, or spray coating; in a preferred embodiment, the coating method is spray coating, so as to achieve a uniform and flat film surface; in a preferred embodiment, the film of the present invention is formed by natural drying in an environment at room temperature.

[0043] According to one embodiment of the present invention, the substrate comprises glass, polycarbonate (PC), polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polyvinyl chloride (PVC), polypropylene (PP), polyethylene (PE), nylon or acrylic resin. In a preferred embodiment, the substrate is glass, polycarbonate or acrylic resin.

[0044] According to one embodiment of the present invention, the film has a thickness of 10 to 50 μm, for example but not limited to any two of the following values: 10 μm, 12 μm, 14 μm, 15 μm, 18 μm, 20 μm, 23 μm, 25 μm, 27 μm, 29 μm, 30 μm, 31 μm, 33 μm, 35 μm, 38 μm, 40 μm, 43 μm, 45 μm, 46 μm, 48 μm, 49 μm or 50 μm. According to some embodiments of the present invention, the film thickness is measured by a digital thousand-gauge scale, more specifically, the present invention adopts a Mitutoyo digital thousand-gauge scale 543-706B for measurement.

[0045] The film formed by the present invention can block infrared light and ultraviolet light, and at the same time maintain a high visible light transmittance, so it has visual transparency and can block the radiant heat energy of sunlight and the effect of ultraviolet light. According to one embodiment of the present invention, the film has a visible light transmittance of 70 to 90%, for example but not limited to any two of the following values: 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89% or 90%.

[0046] According to one embodiment of the present invention, the film has an infrared light blocking rate of 60 to 99%, for example but not limited to between any two of the following values: 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%. According to one embodiment of the present invention, the film has a UV blocking rate of 45 to 95%, for example but not limited to any two of the following values: 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94% or 95%.

[0047] According to one embodiment of the present invention, the film has a total solar energy transmittance (SHGC) of 0.4 to 0.67, for example but not limited to between any two of the following values: 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66 or 0.67. As used herein, "Total Solar Energy Transmittance (hereinafter referred to as SHGC)" may also be referred to as Total Solar Energy Transmittance, solar factor or g-value, which refers to the ratio of the solar radiation portion that becomes indoor heat gain through glass doors and windows or glass curtain walls within the wavelength range of 300 to 2500nm to the solar radiation illuminance projected onto the glass, doors and windows or glass curtain wall components. Specifically, the solar radiation portion of indoor heat gain includes: the heat gain of solar radiation through radiation or transmission, and the heat gain of solar radiation absorbed by components and then transmitted into the room (secondary heat transfer). The total solar energy transmittance can represent the heat gain capacity of glass. When the total solar energy transmittance is smaller (for example, less than or equal to 0.6), it means that its thermal insulation performance is better.

[0048] Another aspect of the present invention provides a multilayer structure comprising the above-mentioned film, wherein the multilayer structure is a wall material, roof material, window or vehicle window of a building or structure, etc., which needs to be used for heat insulation, infrared light or ultraviolet light blocking. Example

[0049] Hereinafter, the present invention will be further described with detailed description and examples. However, it should be understood that these examples are only used to help the present invention to be more easily understood and are not used to limit the scope of the present invention.

[0050] Selecting and evaluating resins

[0051] Here, the present invention selects various water-soluble resins with different Tg, and uses the specific concentrations of the water-soluble resins to measure the spraying performance, film transparency, hand touch and removability of the heat-insulating particles. The results are listed in Table 1. The sample is obtained by mixing the specific concentration of resin, 5wt% heat-insulating particles and water, and then filtering the mixed product. In detail, the material of the heat-insulating particles selected here is cesium tungsten oxide.

[0052] The "spraying performance" is to use a pressure spray can to coat the sample on the glass, and evaluate the quality of the film by naked eyes and actual operation. The specific inspection content includes whether there is blockage in the spraying process, whether there are defects in the appearance, and whether the formed film is obviously uneven. Among them, if the formed film does not have the above defects, it is represented by "O"; if it has any of the above defects, it is represented by "X".

[0053] The “film transparency” is determined by measuring the light transmittance (T%) and haze (Haze) using a haze meter (BYK-Gardner haze-gard plus4725); if the haze value is less than 3%, it is represented as “O”; if the haze value is greater than or equal to 3%, it is represented as “X”.

[0054] The "touch feeling" is to touch the film surface with your fingers and visually confirm whether there is any sticking, fingerprints, etc.; the more serious these phenomena are, the larger the value will be; in practice, it is best if this value is less than 2.

[0055] The “removability” refers to the ability to remove the film by sticking a regular tape to the corner of the film after the film has dried. If the film can be easily removed, it is indicated as “O”; if the film cannot be easily removed, it is indicated as “X”.

[0056] Table 1

[0057] As can be seen from Table 1, only when self-crosslinking acrylic resin or polyurethane resin is used and Tg falls within the range of -20 to 25°C, the film produced can have better removability and a more ideal touch performance. On the contrary, when silicone acrylic resin, silicone acrylic resin or fluororesin is used, the touch and removability of the film are not good; moreover, even if a self-crosslinking acrylic resin is used, if its Tg is not within the above range, the touch and removability of the film are still not good.

[0058] Preparation of liquid resin composition and film

[0059] In view of the above results, the present invention mixes 5% cesium tungsten oxide solution, 15wt% aqueous solvent, and 10wt% auxiliary agent, and then adds them into 70wt% aqueous polyurethane resin for mixing and stirring to obtain the liquid resin composition of this embodiment. Furthermore, the above liquid resin composition is used as a coating for liquid window film, and the coating is applied to 3mm thick glass by brushing, and after drying at room temperature for two hours, a transparent heat insulation film is formed on the glass.

[0060] Sunlight cooling capacity test

[0061] Please refer to Figure 2The present invention tests the cooling ability of the membrane by simulating continuous sunlight. Figure 2 To simulate the continuous sunlight device 100, a halogen lamp 110 is used to simultaneously illuminate the bare glass 120 and the sample 130 (i.e., the glass covered with the film of the present invention), and a thermocouple meter 140 is used to monitor the temperature change in the space. The temperature change is calculated as follows: ΔT (°C) = sample (T f )–blank(T f ). Specifically, the preparation method of the sample 130 is similar to the above content, except that it is prepared with a formula of 25% aqueous solvent and 60% aqueous polyurethane resin, and the other solvent types and their proportions remain unchanged. After the sample 130 is prepared, it is coated on the glass and allowed to dry and form; wherein the film thickness coated on the glass is about 20 to 25 μm.

[0062] The experimental results are as follows Figure 3 As shown. The thermal insulation effect of the sample remained stable after 4 hours of continuous sunlight exposure for 8 hours, with a ΔT of about -6.4°C, indicating that the thermal insulation effect of the film sample reached a constant thermal insulation after about 4 hours. It can be seen that the film of the present invention can maintain a stable cooling effect for at least 8 hours under continuous exposure to fixed sunlight, reducing the entry of radiant heat energy.

[0063] Film property testing at different thicknesses

[0064] In this embodiment, samples with film thicknesses of 10, 20, 30.2, 31.6 and 40 μm were prepared in the above manner, and the cooling capacity (measurement method as described above), ultraviolet light blocking rate, infrared light blocking rate, visible light transmittance and SHGC of these samples were measured, while 3 mm thick bare glass was used as a control; the results are shown in Tables 2, 3 and Figures 4A to 4C shown.

[0065] The ultraviolet light blocking rate, infrared light blocking rate and visible light transmittance can be measured by a spectrophotometer (UV-Visspectrophotometer Lambda 750 (PerkinElmer, USA)) or LS182 optical transmittance measuring instrument. Specifically, the calculation range of visible light transmittance is 380 to 780nm; the calculation range of infrared light transmittance is 780 to 2500nm or fixed wavelength at 940 or 1400nm; the calculation of ultraviolet light transmittance is fixed wavelength at 365nm. Furthermore, the infrared light blocking rate is the percentage of infrared light that cannot pass through the transparent thermal insulation film structure, and the formula is infrared light blocking rate = (100%-infrared light transmittance); and the ultraviolet light blocking rate is the percentage of ultraviolet light that cannot pass through the transparent thermal insulation film structure, and the formula is ultraviolet light blocking rate = (100%-ultraviolet light transmittance).

[0066] Regarding SHGC, it is a ratio value that represents the ratio of solar radiation heat that can penetrate. SHGC is a reference data obtained by the instrument LS182 optical transmittance meter (solar film tester). The evaluation method of SHGC is based on the evaluation and labeling system established by the National Fenestration Rating Council (NFRC) according to the common door and window evaluation standards in North America. Generally speaking, the value of SHGC is between 0.25 and 0.8; in a preferred embodiment of the present invention, the value of SHGC is between 0.4 and 0.67.

[0067] Table 2

[0068] Table 3 Thickness(μm) Cooling capacity(℃) 5~15 -3.5 20~35 -6.3 40~55 -9.6

[0069] From the above results, it can be seen that when the liquid resin composition of the present invention is made into a film, it has good cooling ability, ultraviolet light blocking rate, infrared light blocking rate, visible light transmittance and SHGC performance at all thicknesses; when the film thickness is thicker, the visible light transmittance is still maintained at more than 70%, and the infrared and ultraviolet light blocking effects are excellent, thereby making the cooling effect more excellent. In addition, the film formed at the standard thickness is transparent and slightly blue, and has an ultraviolet light blocking rate of more than 70% when the film thickness is standard and thicker; and even when the film thickness is thinner, it can still have an ultraviolet light blocking rate of more than 45%.

[0070] In summary, the film formed by the liquid resin composition of the present invention can block infrared light and ultraviolet light, while maintaining a high visible light transmittance, thus having visual transparency and being able to block the radiant heat energy and ultraviolet light of sunlight; thereby, the present invention can achieve the purposes of natural indoor cooling, energy saving and carbon reduction, extending the service life of articles, and providing surface protection effects. In addition, the film of the present invention is convenient in construction and removal operations, and no residual glue will be formed on the surface of the coated object, and after removal, it has the additional effect of making the surface of the object clean.

[0071] Herein, all ranges provided are intended to include each specific range within a given range and combinations of sub-ranges between the given ranges. In addition, unless otherwise stated, all ranges provided herein include the endpoints of the ranges. Thus, ranges 1-5 specifically include 1, 2, 3, 4, and 5, as well as sub-ranges such as 2-5, 3-5, 2-3, 2-4, 1-4, etc.

[0072] The present invention has been described in detail above. However, what is described above is only a preferred embodiment of the present invention and should not be used to limit the scope of implementation of the present invention. That is, all equivalent changes and modifications made according to the scope of the patent application of the present invention should still fall within the scope of the patent of the present invention.

Explanation of symbols

[0073] 100: Continuous sunlight device 110: Halogen lamp 120: Glass 130: Sample 140: Thermocouple meter

Claims

1. A liquid resin composition comprising: (a) 20 to 80 wt% of a resin selected from the group consisting of a self-crosslinking acrylic resin and a polyurethane resin, and having a Tg of -20 to 25°C, (b) 1 to 10 wt% of thermal insulation particles and (c) 5 to 25 wt% of an aqueous solvent.

2. The liquid resin composition according to claim 1, wherein The heat-insulating particles are cesium tungsten oxide.

3. The liquid resin composition according to claim 1, wherein The aqueous solvent is selected from the group consisting of water, short-chain esters, ethers and alcohols.

4. The liquid resin composition according to any one of claims 1 to 3, wherein The composition further comprises an auxiliary agent, and the auxiliary agent is selected from the group consisting of UV absorbers, UV stabilizers, thickeners, leveling agents, rheological agents and defoaming agents.

5. The liquid resin composition according to claim 4, wherein The auxiliary agent is a UV absorber or a UV stabilizer, and accounts for 1 to 3 wt % of the liquid resin composition.

6. The liquid resin composition according to claim 4, wherein The auxiliary agent is a leveling agent, and accounts for 0.01 to 7 wt % of the liquid resin composition.

7. The liquid resin composition according to claim 4, wherein The auxiliary agent is a rheological agent, and accounts for 0.1 to 5 wt % of the liquid resin composition.

8. The liquid resin composition according to claim 4, wherein The auxiliary agent is a defoaming agent, and accounts for 0.05 to 3 wt % of the liquid resin composition.

9. A film that can be torn off on a substrate, wherein: The film is formed by coating the liquid resin composition according to any one of claims 1 to 8 on the substrate and drying it.

10. The film of claim 9, wherein The substrate is glass, polycarbonate or acrylic.

11. The film of claim 9, wherein The film has a thickness of 10 to 50 μm.

12. The membrane according to any one of claims 9 to 11, wherein The film has a visible light transmittance of 70 to 90%.

13. The film of claim 12, wherein The film has an infrared light blocking rate of 60 to 99%.

14. The film of claim 13, wherein The film has an ultraviolet light blocking rate of 45 to 95%.

15. The film of claim 14, wherein The film has a solar total transmittance (SHGC) of 0.4 to 0.

67.

16. A multilayer structure comprising the film according to any one of claims 9 to 15, wherein the multilayer structure is a wall material, a roof material, a window of a building or structure, or a window of a vehicle.

Citation Information

Patent Citations

  • Insulating mold coating of transparent glass and manufacturing method thereof

    CN101362630A

  • Thermal insulation optical thin film material

    CN105542405A

  • Waterborne peelable transparent heat-insulating glass coating and a preparing method thereof

    CN106634294A

  • Heat-ray shielding laminated glass and method for manufacturing heat-ray shielding laminated glass

    JP2014201450A

  • Thermal barrier film and thermal barrier laminated glass

    JP2017185669A