Composition, optical film, layer, optical filter, optical element, solid-state imaging device, and camera module
A composition of a phosphonic acid and copper compound with polyarylate polymer addresses durability and redispersibility issues in optical filters, ensuring high visible light and low near-infrared transmittance, even in harsh conditions.
Patent Information
- Application Number
- CN202410667880.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-19
- Filing Date
- 2024-05-28
- Publication Date
- 2024-12-03
AI Technical Summary
Conventional optical filters face issues with durability under high temperature and high humidity conditions, opacity, and poor redispersibility, leading to reduced visible light transmittance and increased near-infrared transmittance.
A composition comprising a light-absorbing compound containing a phosphonic acid component and a copper component, along with a polymer containing polyarylate, which forms an optical film or filter with high visible light transmittance and low near-infrared transmittance, and is durable even in harsh environments.
The composition provides an optical film and filter with excellent appearance, redispersibility, and durability, maintaining high visible light transmittance and low near-infrared transmittance, even under high temperature and humidity conditions.
Smart Images

Figure CN119065043A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composition, an optical film, a layer, an optical filter, an optical element, a solid-state imaging device, and a camera module. Background Art
[0002] In solid-state imaging devices such as video cameras, digital still cameras, and mobile phones with camera functions, charge coupled devices (CCDs) or complementary metal oxide semiconductor (CMOS) image sensors are used as solid-state imaging elements for color images. In these solid-state imaging elements, silicon photodiodes that are sensitive to near-infrared rays that are imperceptible to the human eye are used in their light receiving units. In these solid-state imaging elements, it is necessary to perform visual sensitivity correction to present natural colors to the human eye, and most of them use optical filters that selectively transmit or cut off light in a specific wavelength region (such as near-infrared cutoff filters).
[0003] As such near-infrared cut filters, filters manufactured by various methods have been used in the past. For example, there are known absorption glass type optical filters using absorption glass in which copper oxide is dispersed in phosphate glass as a base material (for example, see Patent Document 1), or optical filters in which near-infrared absorption pigments are added to resin films (for example, see Patent Document 2).
[0004] In recent years, with the improvement of the performance of solid-state imaging devices, there is a strong demand for reducing ghosting or flare in camera images. It is known that the improvement of the near-infrared absorption performance of the optical filter is effective in reducing ghosting or flare, and as near-infrared cut-off filters that can achieve this, an optical filter having a structure of a resin layer containing a near-infrared absorption pigment on an absorption glass substrate (for example, see Patent Document 3), an optical filter having a plurality of near-infrared absorption pigments added to a resin film (for example, see Patent Document 4), and an optical filter having a resin layer containing a copper phosphonate complex and a near-infrared absorption pigment on a transparent glass substrate (for example, see Patent Document 5) have been proposed.
[0005] [Prior art literature]
[0006] [Patent Document]
[0007] [Patent Document 1] International Publication No. 2011 / 071157
[0008] [Patent Document 2] Japanese Patent Application Publication No. 2011-100084
[0009] [Patent Document 3] International Publication No. 2014 / 030628
[0010] [Patent Document 4] Japanese Patent Application Publication No. 2019-032371
[0011] [Patent Document 5] Japanese Patent Application Publication No. 2020-129150 Summary of the invention
[0012] [Problems to be solved by the invention]
[0013] However, an optical filter using absorbing glass cannot avoid the problem of "crack" when dropped, and in a structure that absorbs a wide near-infrared wavelength region using only a near-infrared absorbing dye, a decrease in visible light transmittance becomes significant.
[0014] In addition, it is known that optical filters using copper phosphonate complexes and near-infrared absorbing pigments can achieve excellent spectral characteristics (combining high visible light transmittance and low near-infrared transmittance), but in previous optical filters, there are problems with the durability of copper phosphonate complexes under high temperature and high humidity conditions, and it is impossible to obtain practical optical filters.
[0015] Furthermore, it is found that conventional compositions containing copper phosphonate complexes may not have a highly transparent appearance or may become opaque and turbid when redispersed in a solvent, and that there is room for improvement in appearance and redispersibility.
[0016] The present invention has been made in view of the above circumstances, and an object thereof is to provide a composition which has excellent appearance and redispersibility, can form an optical film or optical filter having high visible light transmittance and low near infrared transmittance, and has excellent durability even in a high temperature and high humidity environment.
[0017] [Technical means to solve the problem]
[0018] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved according to the following structural examples, thereby completing the present invention.
[0019] [1] A composition (D) comprising: a light-absorbing compound (A) containing a phosphonic acid component and a copper component, and a polymer (B1) containing a polyarylate.
[0020] [2] The composition (D) according to [1], further comprising an ultraviolet absorbing compound (U).
[0021] [3] The composition (D) according to [1] or [2], further comprising a pigment (C) other than the compound (A).
[0022] [4] The composition (D) according to any one of [1] to [3], wherein the transmission spectrum of the composition (D) (wherein the transmission spectrum of the composition (D) adjusted to a transmittance of 10%±1% at a wavelength of 800 nm) satisfies the following requirements (i) to (iv).
[0023] (i) The average transmittance in the wavelength range of 800 nm to 1100 nm is 10% or less
[0024] (ii) The average transmittance in the wavelength range of 460 nm to 580 nm is 80% or more
[0025] (iii) A first cutoff wavelength having a transmittance of 50% in the wavelength range of 680 nm to 780 nm
[0026] (iv) A second cutoff wavelength having a transmittance of 50% in the wavelength range of 320 nm to 380 nm
[0027] [5] The composition (D) according to [4], wherein the transmission spectrum further satisfies the following requirement (v).
[0028] (v) The standard deviation of the transmittance in the wavelength range of 900 nm to 1100 nm is 0.5% or less
[0029] [6] An optical film formed from the composition (D) according to any one of [1] to [5].
[0030] [7] A layer (D1) formed from the composition (D) according to any one of [1] to [5], wherein the transmission spectrum satisfies the following requirements (I) to (V).
[0031] (I) The average transmittance in the wavelength range of 460nm to 580nm is 80% or more
[0032] (II) The average transmittance in the wavelength range of 800 nm to 1100 nm is 5% or less
[0033] (III) A third cutoff wavelength having a transmittance of 50% in the wavelength range of 680 nm to 730 nm
[0034] (IV) A fourth cutoff wavelength having a transmittance of 50% in the wavelength range of 340 nm to 400 nm
[0035] (V) The maximum transmittance at a wavelength of 950 nm is less than 1%
[0036] [8] An optical filter comprising a layer (D1) formed from the composition (D) according to any one of [1] to [5].
[0037] [9] An optical filter comprising:
[0038] A layer (D1) formed from the composition (D) according to any one of [1] to [5]; and
[0039] The layer (D2) is formed by a composition (D2) containing a pigment (C) other than the compound (A), and at least one selected from a polymer (B2-1) and a curable compound (B2-2) that is cured by light or heat.
[0040]
[10] The optical filter according to [8] or [9], comprising a dielectric multilayer film.
[0041]
[11] An optical element comprising the optical filter according to any one of [8] to
[10] .
[0042]
[12] A solid-state imaging device comprising the optical filter according to any one of [8] to
[10] .
[0043]
[13] A camera module having the optical filter according to any one of [8] to
[10] .
[0044]
[14] A composition (D) wherein
[0045] The composition (D) contains: a light absorbing compound (A) containing a phosphonic acid component and a copper component, and a polymer (B1) containing a polyarylate.
[0046] The solid content of the composition (D) is 15% to 85% by mass.
[0047] The content of the polymer (B1) in the composition (D) is 5% to 70% by mass.
[0048] The content of the polymer (B1) is 0.5 to 6 parts by mass based on 1 part by mass of the compound (A).
[0049] [Effects of the Invention]
[0050] According to the present invention, a composition having excellent appearance and redispersibility can be provided.
[0051] Furthermore, according to the present invention, it is possible to provide an optical film and an optical filter which have high visible light transmittance and low near infrared transmittance and are excellent in durability even in a high-temperature and high-humidity environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 (A) Figure 1(B) is a schematic diagram showing an example of an optical element, a solid-state imaging device or a module including the optical filter of the present invention.
[0053] Figure 2 (A) Figure 2 (B) is a schematic diagram showing an example of an optical element, a solid-state imaging device, or a module having the optical filter of the present invention and having no lens.
[0054] Figure 3 This is the spectral transmittance spectrum of Composition 1 obtained in Example A1.
[0055] Figure 4 This is the spectral transmittance spectrum of Composition 3 obtained in Example A3.
[0056] Figure 5 This is the spectral transmittance spectrum of Composition 5 obtained in Example A5.
[0057] Figure 6 This is the spectral transmittance spectrum of Composition 6 obtained in Example A6.
[0058] Figure 7 This is the spectral transmittance spectrum of the layer (D1-A1) obtained in Example A1.
[0059] Figure 8 It is the spectral transmittance spectrum of the layer (D1-A3) obtained in Example A3.
[0060] Fig. 9 It is the spectral transmittance spectrum of the layer (D1-A6) obtained in Example A6.
[0061] Fig.10 It is the spectral transmittance spectrum of the layer (D1-A8) obtained in Example A8.
[0062] Fig.11 This is the spectral transmittance spectrum of the substrate obtained in Example P1.
[0063] Fig.12 This is the spectral transmittance spectrum of the substrate obtained in Example P2.
[0064] Fig.13 This is the spectral transmittance spectrum of the substrate obtained in Example P3.
[0065] Fig.14 This is the spectral transmittance spectrum of the substrate obtained in Example P4.
[0066] Fig.15 It is the spectral transmittance spectrum of the optical filter obtained in Example P1.
[0067] Fig.16It is the spectral transmittance spectrum of the optical filter obtained in Example P2.
[0068] Fig.17 It is the spectral transmittance spectrum of the optical filter obtained in Example P3.
[0069] Fig.18 It is the spectral transmittance spectrum of the optical filter obtained in Example P4.
[0070] Fig.19 It is the spectral transmittance spectrum of the optical filter obtained in Example P5.
[0071] [Explanation of Symbols]
[0072] 1: Optical filter
[0073] 24: Image sensor 25: Image sensor framework
[0074] 26: Framework
[0075] 31: Frame
[0076] 32: Lens
[0077] 33: Lens replacement optical elements such as Fresnel zone plates or Fresnel lenses DETAILED DESCRIPTION
[0078] Hereinafter, the content of the present invention will be described in detail. The following description may be made based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.
[0079] In the present specification, "to" indicating a numerical range is used to mean that the numerical values described before and after it are included as the lower limit and the upper limit.
[0080] In the present specification, "to" indicating a numerical range means that any unit described before and after it represents the same unit unless otherwise specified.
[0081] In the embodiments of the present invention, "transmission" means that the transmittance is preferably 50% or more, more preferably 60% or more, and further preferably 70% or more in the wavelength or wavelength range of the object. "Shielding" means that the transmittance is preferably less than 10%, more preferably less than 5%, and further preferably less than 1% in the wavelength or wavelength range of the object. In addition, the so-called "light" means all light unless otherwise specified.
[0082] 《Composition (D)》
[0083] The composition (D) according to one embodiment of the present invention (hereinafter also referred to as “present composition 1”) is a composition containing a light absorbing compound (A) containing a phosphonic acid component and a copper component, and a polymer (B1) containing a polyarylate.
[0084] In addition, a composition (D) (hereinafter also referred to as "the present composition 2") according to another embodiment of the present invention is a composition comprising a light-absorbing compound (A) comprising a phosphonic acid component and a copper component, and a polymer (B1) comprising a polyarylate, wherein the content of the solid component in the present composition 2 is 15% by mass to 85% by mass, the content of the polymer (B1) in the present composition 2 is 5% by mass to 70% by mass, and the content of the polymer (B1) relative to 1 part by mass of the compound (A) is 0.5 parts by mass to 6 parts by mass.
[0085] Hereinafter, the present composition 1 and the present composition 2 are also collectively referred to as the "present composition".
[0086] The present composition can suppress the aggregation of the compound (A) in the present composition and suppress the degradation of the light absorbing compound (A). In addition, the present composition is excellent in appearance and redispersibility.
[0087] In addition, according to the present composition, especially the present composition 2, when forming an optical film or layer (D1) by a solution casting method (solvent casting method) or the like, uneven casting onto a carrier (support), a preferred drying speed under specified conditions, and unevenness or haze within the optical film or layer (D1) can be suppressed.
[0088] The content of the solid content in the present composition 1 is preferably 15% by mass to 85% by mass, more preferably 30% by mass to 85% by mass, and still more preferably 40% by mass to 85% by mass.
[0089] The content of the solid content in the present composition 2 is 15% by mass to 85% by mass, preferably 30% by mass to 85% by mass, and more preferably 40% by mass to 85% by mass.
[0090] The solid content in the present composition is the dry mass of the present composition, and is the content of components other than the solvent in the present composition, and is determined as follows.
[0091] The mass M1 of the present composition is measured. Next, the composition is heated in a heating oven to dry it, leaving only the solid content. The weight m1 of the remaining solid content is measured. The value of m1 / M1×100 is set as the content of the solid content in the present composition.
[0092] Furthermore, the present composition 1 may be a solid composition after the solvent has been removed. Such a solid composition is also one embodiment of the present composition.
[0093] The specific form of the solid composition includes, for example, granules, powders, and pellets. When the composition is distributed, the solid composition can be distributed more simply and cost-effectively than a composition containing a solvent.
[0094] Furthermore, the solid composition can be easily restored to a liquid state by redispersing it in a solvent such as the second solvent described below.
[0095] <Light-absorbing compound (A)>
[0096] The light absorbing compound (A) is a compound containing a phosphonic acid component and a copper component and is not particularly limited as long as it contains these components, but is preferably a copper complex containing a phosphonic acid component.
[0097] The compound (A) used in the present composition may be one kind or two or more kinds.
[0098] The compound (A) can be synthesized using a copper compound and phosphonic acid (phosphonic acid compound) as raw materials.
[0099] It is very difficult to explain the reaction process of the copper compound and the phosphonic acid compound in detail and to determine the structure of the obtained reaction product (compound (A)). Due to these circumstances, compound (A) is represented as a compound containing a phosphonic acid component and a copper component. The compound (A) is, for example, a copper phosphonate compound, for example, a complex of a phosphonic acid compound and a copper compound.
[0100] Compound (A) may be, for example, a compound comprising a phosphonic acid component, a phosphate component, and a copper component (e.g., a phosphonic acid-phosphate-copper compound), or a mixture of a compound comprising a phosphonic acid component and a copper component and a compound comprising a phosphonic acid component, a phosphate component, and a copper component, or a complex of these compounds.
[0101] These compounds (A) have a broad absorption band in the (near) infrared region, and by using the compounds (A), an optical film or layer (D1) having a low transmittance in the (near) infrared region and a high transmittance in the visible light region can be easily formed.
[0102] In addition, phosphonic acid, phosphinate, phosphate, phosphoric acid, metaphosphoric acid and pyrophosphoric acid are all compounds containing phosphorus atoms. In addition to phosphonic acid, compound (A) may also contain at least one component selected from phosphinate, phosphate, phosphoric acid, metaphosphoric acid and pyrophosphoric acid.
[0103] The content of the compound (A) in the present composition is preferably 5% by mass to 75% by mass, more preferably 7% by mass to 65% by mass, and still more preferably 8% by mass to 55% by mass.
[0104] By having the content of compound (A) within the above range, compound (A) is difficult to agglomerate in the present composition and is appropriately dispersed. When an optical film or layer (D1) is formed from the present composition, compound (A) is also difficult to agglomerate during the process of forming the optical film or layer (D1), and an optical film or layer (D1) in which compound (A) is sufficiently dispersed can be formed, thereby easily forming an optical film or layer (D1) having desired spectral characteristics.
[0105] (Copper content)
[0106] The copper component is a component derived from a copper compound as a raw material used when synthesizing the compound (A), and is a concept including copper ions, copper complexes, and copper-containing compounds.
[0107] The copper component contained in the compound (A) may be one kind or two or more kinds.
[0108] The copper component may have a preferred absorption characteristic for a portion of light in the near-infrared region. Specifically, it is believed that the light of the wavelength in the near-infrared region corresponding to the energy is selectively absorbed by the migration of electrons in the d orbit of the divalent copper ion, thereby exerting excellent near-infrared absorption characteristics. For example, the copper component may have a hexacoordinated structure through one or more ligands, and such a copper component is expected to improve the absorption capacity of light in the near-infrared region.
[0109] The raw material of the copper component is not particularly limited, and examples thereof include copper compounds of organic acids such as copper acetate, copper benzoate, copper pyrophosphate, and copper stearate, and hydrates of these copper compounds. These may be used alone or in combination of two or more.
[0110] From the viewpoint of easily obtaining a compound having excellent light absorption capacity in the near-infrared region, the content of the copper component in the compound (A) is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 20% by mass, and still more preferably 2% by mass to 15% by mass, in terms of the content of copper atoms.
[0111] (phosphonic acid component)
[0112] The phosphonic acid component is a component derived from the phosphonic acid (phosphonic acid compound) which is a raw material used when synthesizing the compound (A).
[0113] The phosphonic acid component contained in the compound (A) may be one kind or two or more kinds.
[0114] Examples of the phosphonic acid compound include a compound represented by the following formula (a1) and a compound represented by the following formula (a2).
[0115] As the phosphonic acid compound, one or more compounds represented by the following formula (a1) can be used, one or more compounds represented by the following formula (a2) can be used, or one or more compounds represented by the following formula (a1) and one or more compounds represented by the following formula (a2) can be used.
[0116] For example, the compound (A) obtained by using the compound represented by the following formula (a1) has the following tendency: the absorption capacity of light in the wavelength range of 800nm to 1200nm is high, but the absorption capacity of light in the wavelength range of 700nm and 350nm is low. Therefore, the light passing through the optical film or layer (D1) using the compound (A) is sometimes slightly insufficient in terms of consistency with human visual sensitivity.
[0117] On the other hand, the compound (A) obtained by using the compound represented by the following formula (a2) tends to have a low absorption capacity for light in the wavelength range of 800 nm to 1200 nm, but a high absorption capacity for light in the wavelength range of 700 nm and 350 nm.
[0118] In terms of complementing these properties, the present composition preferably comprises a compound (A) using a compound represented by the following formula (a1) and a compound represented by the following formula (a2). In addition, it is preferably a combination of a compound (A) using a compound represented by the following formula (a1) and a compound (A) using a compound represented by the following formula (a2).
[0119] [Chemistry 1]
[0120]
[0121] In the formula (a1), R1 is an alkyl group or a halogenated alkyl group in which at least one hydrogen atom in the alkyl group is substituted with a halogen atom.
[0122] If the phosphonic acid compound represented by the formula (a1) is used as a raw material for synthesizing the compound (A), the long-wavelength side of the transmission band of the optical film or layer (D1) formed by the present composition containing the obtained compound (A) is near a wavelength of 700 nm, and the optical film or layer (D1) easily has the desired transmittance characteristics.
[0123] Examples of the phosphonic acid compound represented by the formula (a1) include methylphosphonic acid, ethylphosphonic acid, n-propylphosphonic acid, isopropylphosphonic acid, n-butylphosphonic acid, isobutylphosphonic acid, sec-butylphosphonic acid, tert-butylphosphonic acid, n-hexylphosphonic acid, and bromomethylphosphonic acid.
[0124] [Chemistry 2]
[0125]
[0126] In formula (a2), R2 is an aryl group, or a group in which at least one hydrogen atom in the aryl group is substituted by at least one selected from a halogen atom, a nitro group and a hydroxyl group.
[0127] When the phosphonic acid compound represented by the formula (a2) is used as a raw material for synthesizing the compound (A), the optical film or layer (D1) formed from the present composition containing the obtained compound (A) is more likely to have desired transmittance characteristics.
[0128] Examples of the phosphonic acid compound represented by the formula (a2) include phenylphosphonic acid, bromophenylphosphonic acid, benzylphosphonic acid, fluorophenylphosphonic acid, iodophenylphosphonic acid, nitrophenylphosphonic acid, hydroxyphenylphosphonic acid, tolylphosphonic acid, xylylphosphonic acid, and naphthylphosphonic acid.
[0129] The content of the phosphonic acid component in the compound (A) is preferably 1 to 60% by mass, more preferably 2 to 40% by mass, and even more preferably 4 to 28% by mass, from the viewpoint of easily obtaining a compound having excellent light transmittance in the visible light region.
[0130] (Phosphate ester component)
[0131] The compound (A) may further contain a phosphoric acid ester component. However, it is preferred to contain a phosphoric acid ester component from the viewpoint of further suppressing aggregation of the compound (A) in the solvent.
[0132] When the compound (A) contains a phosphoric acid ester component, the compound (A) can be easily and appropriately dispersed in the present composition and the optical film or layer (D1) formed from the present composition due to the action of the phosphoric acid ester component.
[0133] The phosphate ester component may function as a dispersant for the compound (A), and a part of the phosphate ester component may react with a metal component such as a copper component to form a compound.
[0134] For example, the phosphate component may form a portion of a complex with the copper component.
[0135] The phosphate component is a component derived from a phosphate compound which is a raw material that can be used when synthesizing the compound (A).
[0136] The phosphate ester component contained in the compound (A) may be one kind or two or more kinds.
[0137] Examples of the phosphate ester compound include compounds having a polyoxyalkyl group, phosphate diesters represented by the following formula (b1), and phosphate monoesters represented by the following formula (b2), and these phosphate esters may be mixed in any ratio.
[0138] [Chemistry 3]
[0139]
[0140] [Where R 21 , R 22 and R3 are each independently -(CH2CH2O) n R4 is a monovalent functional group, n is an integer of 1 to 25, R4 is an alkyl group having 6 to 25 carbon atoms, 21 , R 22 and R3 may be the same group or different groups]
[0141] Examples of the phosphate compound include PLYSURF A208N (polyoxyethylene alkyl (C12, C13) ether phosphate), PLYSURF A208F (polyoxyethylene alkyl (C8) ether phosphate), PLYSURF A208B (polyoxyethylene lauryl ether phosphate), PLYSURF A219B (polyoxyethylene lauryl ether phosphate), PLYSURF A212C (polyoxyethylene tridecyl ether phosphate), and PLYSURF A215C (polyoxyethylene tridecyl ether phosphate) manufactured by Daiichi Kogyo Seiyaku Co., Ltd.; and NIKKOL DDP-2 (polyoxyethylene alkyl ether phosphate), NIKKOL DDP-4 (polyoxyethylene alkyl ether phosphate), and NIKKOL DDP-6 (polyoxyethylene alkyl ether phosphate) manufactured by Nikko Chemical Co., Ltd.
[0142] When compound (A) contains a phosphate component, the content of the phosphate component in compound (A) is preferably 0.5% by mass to 50% by mass, more preferably 1% by mass to 30% by mass, and even more preferably 2% by mass to 25% by mass, in order to further suppress the aggregation of compound (A) in the solvent.
[0143] (Synthesis Method of Compound (A))
[0144] The synthesis method of compound (A) is not particularly limited, and for example, the copper compound, the phosphonic acid compound, and the phosphate compound as required are mixed and stirred to synthesize the compound. In addition, during the synthesis, a solvent (hereinafter also referred to as "first solvent") is preferably used.
[0145] When the phosphate ester compound is used, the compound (A) is preferably synthesized by mixing and stirring a solution a obtained by mixing and stirring the copper compound and the phosphate ester compound dissolved in a first solvent and a solution b obtained by mixing and stirring the phosphonic acid compound dissolved in the first solvent.
[0146] The amount of each raw material used in the above synthesis is preferably such that the content of the component derived from each raw material in the compound (A) is within the above range.
[0147] The first solvent is not particularly limited, and examples thereof include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, 2-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylbutanol, 2-pentanol, tert-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, 1-hexanol, 2-hexanol, 2-ethylbutanol, 1-heptanol, 2-heptanol, 3-heptanol, n-octanol, 2-ethylhexanol, 2-octanol, n-nonyl alcohol, 2,6 - Alcohols such as dimethyl-4-heptanol, n-decanol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, diacetone alcohol; ketones such as heptanone, cyclopentanone, cyclohexanone; hydrocarbons such as cyclopentane, cyclohexane, xylene, toluene; amides such as dimethylformamide, dimethylacetamide; heterocyclic compounds such as tetrahydrofuran (THF) and oxetane; chlorine-based solvents such as methylene chloride (dichloromethane), chloroform, dichloroethane, tetrachloroethane, dichlorobenzene, etc.
[0148] The first solvent may be used alone or in combination of two or more.
[0149] As the first solvent, a so-called poor solvent relative to the compound (A) may be used so that when the liquid a and the liquid b are mixed and stirred, the reaction product (compound (A)) is precipitated. By using such a poor solvent, the solid component of the compound (A) is easily separated from the solvent and taken out.
[0150] Compound (A) can be obtained as a solid compound (A) by, for example, separating the reaction product obtained by mixing and stirring the liquid a and liquid b from the first solvent by filtration. Furthermore, the solid reaction product obtained by separation can be further put into a poor solvent of the reaction product, stirred for several minutes to several hours, and the reprecipitated precipitate can be separated from the solvent by filtration. The separation based on the reprecipitation and filtration can be repeated once or twice or more.
[0151] Furthermore, among the compounds (A), for example, a reaction product containing the first solvent obtained by mixing and stirring the liquid a and the liquid b may be used directly as a raw material for preparing the present composition.
[0152] In addition, compound (A) does not contain components other than phosphonic acid components and copper components. For example, water or acetate ions (CH3COO -) etc. can also coordinate with copper ions, so the reaction product may also contain these etc. and may also contain the first solvent.
[0153] <Polymer (B1) containing polyarylate>
[0154] The polymer (B1) containing polyarylate is not particularly limited, and examples thereof include polymers containing structural units derived from dihydric phenol and structural units derived from aromatic dicarboxylic acid. Preferred examples thereof include polymers (B1a) containing polyarylate represented by the following formula (I).
[0155] By using a polymer (B1) containing polyarylate, even when an optical filter containing a copper phosphonate complex is prepared, durability under high temperature and high humidity conditions is improved. In addition, by using a polymer (B1) containing polyarylate, it is also easy to obtain the present composition having excellent appearance and redispersibility.
[0156] The polymer (B1) used in the present composition may be one kind or two or more kinds.
[0157] [Chemistry 4]
[0158]
[0159] In the formula (I), l, m and n are l+m+n=100 (mol %), l=0-100, m=0-100, and n=0-100.
[0160] l:m is preferably 0:100 to 90:10 (molar ratio).
[0161] In addition, the l is preferably 50 mol% to 70 mol%.
[0162] When l is within the above range, a polymer (B1) having excellent solvent solubility and impact resistance can be easily obtained.
[0163] Examples of the dihydric phenol include 2,2-bis(4-hydroxyphenyl)propane (hereinafter also referred to as “bisphenol A”), 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane (hereinafter also referred to as “bisphenol TMC”), and 4,4-dihydroxybiphenyl (hereinafter also referred to as “biphenol”).
[0164] Bisphenol A is an inexpensive compound, and by including a structural unit derived from bisphenol A, a polymer (B1a) having excellent mechanical properties, particularly impact resistance, can be easily obtained.
[0165] Bisphenol TMC has three methyl substituents on the cyclohexane ring. Therefore, by including the structural unit derived from bisphenol TMC, a polymer (B1a) having excellent solvent solubility and heat resistance can be easily obtained.
[0166] Furthermore, since biphenol has a rigid structure, by including the structural unit derived from the biphenol, a polymer (B1a) having excellent heat resistance and thermal rigidity can be easily obtained.
[0167] The dihydric phenols may be used alone or in combination of two or more.
[0168] As the dihydric phenol, it is preferred to use at least one selected from bisphenol A, bisphenol TMC and biphenol, it is more preferred to use at least two selected from these, and it is particularly preferred to use bisphenol A, bisphenol TMC and biphenol.
[0169] As the aromatic dicarboxylic acid, phthalic acid is preferred.
[0170] Examples of the phthalic acid include terephthalic acid, isophthalic acid, ortho-phthalic acid, and mixtures thereof.
[0171] Among these, it is preferred to use a mixture of isophthalic acid and terephthalic acid from the viewpoint of being able to carry out a good synthesis reaction when synthesizing the polymer (B1a). In such a case, from the viewpoint of having a good balance of properties of the obtained polymer (B1a) and being excellent, the mixing ratio of terephthalic acid and isophthalic acid is preferably terephthalic acid / isophthalic acid = 8 / 2 to 2 / 8, more preferably 7 / 3 to 3 / 7 in terms of molar ratio. An equimolar mixture of the two is most preferred.
[0172] In addition, as the polymer (B1), a part of the structural units derived from aromatic dicarboxylic acids may be replaced with structural units derived from one or more other aliphatic dicarboxylic acids within a range that does not hinder the effect of the present invention. Examples of such aliphatic dicarboxylic acids include dicarboxymethylcyclohexane, cyclohexanedicarboxylic acid, adipic acid, sebacic acid, glutaric acid, and dodecanedioic acid.
[0173] The method of polymerizing polymer (B1) is not particularly limited, preferably interfacial polymerization. According to interfacial polymerization, compared with solution polymerization, reaction is fast, for example, when using isophthalic acid halide as raw material, the hydrolysis of the isophthalic acid halide can be suppressed to minimum, so the polymer (B1) of high molecular weight can be easily synthesized. In addition, according to interfacial polymerization, the viscosity of the polymer (B1) obtained can be controlled, and then the polymer (B1) with few impurities can be easily synthesized.
[0174] Specific examples of the method for polymerizing the polymer (B1) include the methods described in Japanese Patent No. 5355330 or Japanese Patent No. 5749621.
[0175] The content of the polyarylate in the polymer (B1) is preferably 70 to 100% by mass, more preferably 90 to 100% by mass, and particularly preferably 100% by mass. That is, the polymer (B1) is particularly preferably a polyarylate (containing only a polyarylate).
[0176] When the content of the polyarylate in the polymer (B1) is other than 100 mass %, components other than the polyarylate contained in the polymer (B1) include raw materials (unreacted components) and additives used in synthesizing the polymer (B1).
[0177] The content of the polymer (B1) in the present composition 1 is preferably 5% by mass to 70% by mass, more preferably 8% by mass to 60% by mass, and still more preferably 10% by mass to 50% by mass.
[0178] The content of the polymer (B1) in the present composition 2 is 5% by mass to 70% by mass, preferably 8% by mass to 60% by mass, and more preferably 10% by mass to 50% by mass.
[0179] If the content of the polymer (B1) in the present composition is within the above range, the present composition having excellent appearance and redispersibility can be easily obtained, and the compound (A) in the present composition is difficult to agglomerate but is appropriately dispersed. When an optical film or layer (D1) is formed from the present composition, the compound (A) is also difficult to agglomerate during the process of forming the optical film or layer (D1), and an optical film or layer (D1) in which the compound (A) is sufficiently dispersed can be formed, so that an optical film or layer (D1) having desired spectral characteristics can be easily formed.
[0180] In the present composition 1, the content of the polymer (B1) is preferably 0.5 to 6 parts by mass, more preferably 0.8 to 5.5 parts by mass, and even more preferably 1.0 to 5.0 parts by mass based on 1 part by mass of the compound (A).
[0181] In the present composition 2, the content of the polymer (B1) is 0.5 to 6 parts by mass, preferably 0.8 to 5.5 parts by mass, and more preferably 1.0 to 5.0 parts by mass based on 1 part by mass of the compound (A).
[0182] If the content of the polymer (B1) relative to 1 part by mass of the compound (A) is within the above range, the present composition having excellent appearance and redispersibility can be easily obtained, and the compound (A) in the present composition is difficult to agglomerate but is appropriately dispersed. When an optical film or layer (D1) is formed from the present composition, the compound (A) is also difficult to agglomerate during the process of forming the optical film or layer (D1), and an optical film or layer (D1) in which the compound (A) is sufficiently dispersed can be formed, so that an optical film or layer (D1) having desired spectral characteristics can be easily formed.
[0183] <Other ingredients>
[0184] The present composition 1 may contain other components other than the compound (A) and the polymer (B1) within a range that does not impair the effects of the present invention. In addition, the present composition 2 may contain other components other than the compound (A), the polymer (B1) and the solvent (second solvent) within a range that does not impair the effects of the present invention.
[0185] As the other components, for example, there can be mentioned: a pigment (C) other than the compound (A), an ultraviolet absorbing compound (U), a solvent (second solvent), a light stabilizer, a silane coupling agent, an antioxidant, a close adhesion promoter, a fluorescent matting agent, a polymer other than the polymer (B1), a plasticizer, and a filler. In addition, when the optical film or layer (D1) is formed from the present composition by casting, etc., in order to facilitate the formation of the optical film or layer (D1), a leveling agent, a defoaming agent, a peeling accelerator, etc. can also be mentioned as other components.
[0186] These other components may be used alone or in combination of two or more.
[0187] These other ingredients may be mixed together with the compound (A) and the polymer (B1) when preparing the present composition, or may be added when synthesizing the compound (A) or the polymer (B1).
[0188] Examples of polymers other than the polymer (B1) include cyclic (poly)olefin polymers, polyether polymers, polyimide polymers, polyester polymers, polycarbonate polymers, polyamide (aromatic polyamide) polymers, polysulfone polymers, polyethersulfone polymers, polyparaphenylene polymers, polyamideimide polymers, polyethylene naphthalate (PEN) polymers, fluorinated aromatic polymer polymers, (modified) acrylic polymers, and epoxy polymers.
[0189] Specific examples of these polymers include resins described in International Publication No. 2019 / 168090.
[0190] Furthermore, as a polymer other than the polymer (B1), a polymer (B2-1) described later may also be used.
[0191] In the present composition, the content of polymers other than polymer (B1) is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 5 parts by mass or more and 30 parts by mass or less, based on 100 parts by mass of polymer (B1).
[0192] 〔Pigment (C)〕
[0193] The pigment (C) is not particularly limited as long as it is a compound other than the compound (A) and the ultraviolet absorbing compound (U) described below, and may be appropriately selected from conventionally known pigments depending on the application of the present composition.
[0194] When a dye (C) is used in the present composition, the dye (C) used in the present composition may be one kind or two or more kinds.
[0195] The pigment (C) is preferably a visible light absorber or a (near) infrared absorber, and more preferably a (near) infrared absorber having the ability to sufficiently transmit light in the visible light region (e.g., 430 nm to 580 nm) and sufficiently absorb light in the near infrared wavelength region (e.g., 700 nm to 1100 nm).
[0196] Furthermore, the dye (C) is preferably a solvent-soluble dye compound.
[0197] The coloring matter (C) is not particularly limited to any of inorganic compounds, organic compounds, and organic-inorganic compounds, and for example, various known compounds used as dyes or coloring matters can be used.
[0198] Examples of these compounds include azo compounds, azomethine compounds, azopyridone compounds, pyrazolone azo compounds, indole compounds, anthraquinone compounds, quinophthalone compounds, coumarin compounds, dipyrromethene compounds, pyrrolopyrrole compounds, diketopyrrolopyrrole compounds, diphenylmethane compounds, triarylmethane compounds, xanthene compounds, acridine compounds, polymethine compounds, oxonol compounds, merocyanine compounds, arylene compounds, benzylene compounds, cyanine compounds, squarylium compounds, crotonium compounds, perylene compounds, dioxazine compounds, phthalocyanine compounds, porphyrin compounds, tetrazaporphyrin compounds, subphthalocyanine compounds, metal chelate compounds thereof, and metal dithiolate compounds.
[0199] The polymethine compounds are polymethine compounds excluding oxocyanine compounds, merocyanine compounds, arylene compounds, benzylidene compounds, cyanine compounds, squarylium compounds, and crotonium compounds, and the phthalocyanine compounds are phthalocyanine compounds excluding porphyrin compounds and porphyrin tetraza compounds.
[0200] Among these, at least one selected from azomethine compounds, azopyridone compounds, pyrazolone azo compounds, indole compounds, anthraquinone compounds, coumarin compounds, dipyrromethene compounds, triarylmethane compounds, xanthene compounds, polymethine compounds, merocyanine compounds, benzylidene compounds, cyanine compounds, squarylium compounds, crotonium compounds, perylene compounds, dioxazine compounds, phthalocyanine compounds, porphyrin compounds, tetrazaporphyrin compounds, subphthalocyanine compounds, and metal chelate compounds thereof is preferred.
[0201] More preferably, it is at least one selected from azomethine compounds, azopyridone compounds, pyrazolone azo compounds, indole compounds, coumarin compounds, dipyrromethene compounds, triarylmethane compounds, xanthene compounds, polymethine compounds, merocyanine compounds, cyanine compounds, squarylium compounds, crotonium compounds, phthalocyanine compounds, porphyrin compounds, tetrazaporphyrin compounds, subphthalocyanine compounds, and metal chelate compounds thereof.
[0202] The specific structure of the pigment is described in, for example, "New Edition Dye Handbook" (edited by the Society of Synthetic Organic Chemistry; Maruzen, 1970), "Pigment Handbook" (edited by Okawara Nobuyuki et al.; Kodansha, 1986), and the like.
[0203] When the present composition contains a dye (C), the content of the dye (C) is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.2 to 2 parts by mass, based on 100 parts by mass of the polymer (B1).
[0204] When the content of the dye (C) is within the above range, the light absorption characteristics of the dye (C) are sufficiently exhibited, and an optical film or layer (D1) having desired optical characteristics can be easily formed.
[0205] [Ultraviolet absorbing compound (U)]
[0206] The present composition may contain an ultraviolet absorbing compound (U) that absorbs at least a portion of light in the (near) ultraviolet region.
[0207] When the present composition contains the compound (U), deterioration of the polymer (B1) or the compound (A) can be suppressed.
[0208] When the compound (U) is used in the present composition, the compound (U) used in the present composition may be one kind or two or more kinds.
[0209] The compound (U) is preferably selected from the viewpoints of absorbing light of a desired wavelength range, having compatibility with a specific solvent, being well dispersed in the present composition, and having excellent environmental resistance. In addition, in order to expand the absorption width of ultraviolet rays, two or more compounds (U) having different maximum absorption wavelengths can be used.
[0210] Examples of the compound (U) include benzophenone compounds, benzotriazole compounds, salicylic acid compounds, cyanoacrylate compounds, and triazine compounds.
[0211] Specific examples of the compound (U) include compounds described in paragraphs
[0258] to
[0259] of JP-A-2012-18395 and compounds described in JP-A-2007-72163.
[0212] As compound (U), a commercially available product can be used. Examples of the commercially available product include Tinuvin PS, Tinuvin 99-2, Tinuvin 234, Tinuvin 326, Tinuvin 329, Tinuvin 900, Tinuvin 928, Tinuvin 400, Tinuvin 405, Tinuvin 460, Tinuvin 477, Tinuvin 479 and Tinuvin 1577 (all manufactured by BASF).
[0213] When the present composition contains the compound (U), the content of the compound (U) is preferably 0.1 to 5 parts by mass based on 100 parts by mass of the polymer (B1).
[0214] When the content of the compound (U) is within the above range, the light absorption property of the compound (U) is sufficiently exhibited, and an optical film or layer (D1) having desired optical properties can be easily formed.
[0215] [Method (second solvent)]
[0216] The present composition may contain a second solvent within a range that does not impair the effects of the present invention, and preferably contains a second solvent.
[0217] The present composition 1 and the present composition 2 preferably contain one or two or more second solvents.
[0218] When a second solvent is used in the present composition, the second solvent used in the present composition may be one type or two or more types.
[0219] In addition, the present composition may also contain a first solvent that can be used when synthesizing compound (A).
[0220] When the present composition contains the first solvent, the content thereof is preferably 5% by mass or less, more preferably 3% by mass or less, and further preferably 1% by mass or less.
[0221] The second solvent is not particularly limited, and examples thereof include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, 2-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylbutanol, 2-pentanol, tert-pentanol, 3-methoxybutanol, n-hexanol, 2-methylpentanol, 1-hexanol, 2-hexanol, 2-ethylbutanol, 1-heptanol, 2-heptanol, 3-heptanol, n-octanol, 2-ethylhexanol, 2-octanol, n-nonyl alcohol, 2,6-dimethyl-4-heptanol, n-decanol, cyclohexanol, methanol Alcohols such as 3-methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, diacetone alcohol; ketones such as acetone, heptanone, cyclopentanone, cyclohexanone; hydrocarbons such as pentane, hexane, cyclohexane, xylene, toluene; amides such as dimethylformamide, dimethylacetamide; heterocyclic compounds such as tetrahydrofuran (THF) and oxetane; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, tetrachloroethane, dichlorobenzene; ethers such as diethyl ether; esters such as ethyl formate and methyl acetate.
[0222] The second solvent can be determined in consideration of the properties of the polymer (B1), the stability of the present composition, the stability of the process when forming the optical film or layer (D1), the properties required for the optical film or layer (D1), and the like.
[0223] When the optical film or layer (D1) is formed by a solution casting method or the like, a low boiling point solvent (eg, a chlorine-based solvent) is preferably used as the second solvent.
[0224] In the case of forming an optical film or layer (D1) by a solution casting method, with regard to forming the optical film or layer (D1) by removing the solvent after casting, it is preferred to select a solvent with a lower boiling point as the second solvent. In the above case, a solvent with a boiling point of less than 115°C is preferred, a solvent with a boiling point of less than 80°C is more preferred, a solvent with a boiling point of less than 70°C is further preferred, and a solvent with a boiling point of less than 60°C is particularly preferred.
[0225] In addition, when a solvent with a high boiling point is used as the second solvent, when the optical film or layer (D1) is formed, the solvent may remain excessively in the optical film or layer (D1). If the optical film or layer (D1) with a large amount of residual solvent is used in a camera module, part of the solvent may evaporate and may cause adverse effects on electronic components or optical components.
[0226] On the other hand, if the boiling point of the second solvent is less than 30° C., the solvent may evaporate during preparation of the present composition, thereby increasing the viscosity or significantly shortening the pot life.
[0227] Based on the above, the boiling point of the second solvent is preferably 30°C to 115°C, more preferably 30°C to 80°C, further preferably 35°C to 70°C, and particularly preferably 35°C to 60°C.
[0228] As such a second solvent, for example, preferred examples include acetone (56°C), chloroform (61°C), dichloromethane (40°C), diethyl ether (35°C), ethyl formate (52°C), hexane (69°C), methanol (65°C), methyl acetate (57°C), pentane (36°C), tetrahydrofuran (66°C), methyl ethyl ketone (80°C), and toluene (111°C).
[0229] When the present composition contains the second solvent, the content thereof is preferably 15% by mass to 85% by mass, more preferably 20% by mass to 70% by mass.
[0230] 〔Light stabilizer〕
[0231] The present composition may contain a light stabilizer for the purpose of suppressing degradation of the polymer (B1) or the compound (A) due to the action of light including ultraviolet rays.
[0232] When a photostabilizer is used in the present composition, the photostabilizer used in the present composition may be one kind or two or more kinds.
[0233] As a light stabilizer, a hindered amine light stabilizer (HALS) is mentioned, for example.
[0234] As hindered amine-based light stabilizers, for example, Adekastab series manufactured by ADEKA Co., Ltd. can be mentioned.
[0235] When the present composition contains a photostabilizer, the content of the photostabilizer is preferably 0.001 to 20 parts by mass, more preferably 0.01 to 10 parts by mass, and even more preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the polymer (B1), from the perspective of sufficiently suppressing the degradation of the polymer (B1) or the compound (A).
[0236] 〔Silane coupling agent〕
[0237] The present composition may contain a silane coupling agent.
[0238] It is believed that by using a silane coupling agent, the bonding between the compound (A) and the polymer (B1) in the present composition can be enhanced, and weather resistance can be improved. In addition, for example, when an optical film or layer (D1) is formed on an adherend (for example, an inorganic support such as glass) from the present composition, the peeling between the support and the optical film or layer (D1) can be suppressed.
[0239] When a silane coupling agent is used in the present composition, the silane coupling agent used in the present composition may be one kind or two or more kinds.
[0240] Examples of the silane coupling agent include alkoxysilane monomers and hydrolyzates thereof.
[0241] Examples of the alkoxysilane monomer include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, 3-aminopropyltriethoxysilane, N- 2-(Aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-N'-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, vinyltrimethoxysilane, N-2-(N-vinylbenzylaminoethyl)-3-aminopropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane.
[0242] When the present composition contains a silane coupling agent, the content of the silane coupling agent is preferably 0.1 to 20 parts by mass, more preferably 1 to 10 parts by mass, relative to 100 parts by mass of the polymer (B1), from the viewpoint that a present composition having excellent weather resistance can be easily obtained, and an optical film or layer (D1) having excellent adhesion to an adherend can be easily formed.
[0243] <Method for preparing the present composition>
[0244] The present composition can be prepared by mixing the compound (A), the polymer (B1), and, if necessary, the other components mentioned above.
[0245] The mixing order at this time is not particularly limited, and it is preferred to mix and stir a solution obtained by dissolving the polymer (B1) in an appropriate amount of the second solvent with the compound (A) obtained as described above. At this time, it is preferred to stir at room temperature for about 5 minutes to 60 minutes, for example, until no aggregation or lumps are visually recognized in the obtained composition.
[0246] In addition, the purpose of adjusting the concentration of the compound (A) in the present composition obtained is also included, and a certain degree of the second solvent can be removed from the composition obtained as described by distillation or the like. The distillation is preferably carried out at a temperature at or near the boiling point of the second solvent to be removed, or above the boiling point. For example, when the distillation is carried out at a temperature exceeding 85°C, thermal damage may occur to the compound (A). Therefore, when the distillation is carried out, it is preferably carried out at a temperature below 85°C. On the other hand, with respect to the relationship between the boiling point of the selected second solvent, distillation accompanied by reduced pressure (reduced pressure distillation) may also be carried out for the purpose of lowering the actual boiling point.
[0247] <Optical properties of this composition>
[0248] The present composition may also have a certain transmission spectrum when the compound (A) is dispersed in a liquid state, and preferably satisfies the following requirements (i) to (iv) as characteristics related to the transmission spectrum. When measuring the characteristics related to the transmission spectrum of the present composition, for example, the present composition is placed in a transparent cell made of quartz so that the physical optical path length of the light passing therethrough is 1 mm ± 0.25 mm. Here, the so-called physical optical path length is the length without considering the refractive index of the medium.
[0249] The characteristics related to the transmission spectrum of the present composition are the characteristics when the transmittance at a wavelength of 800 nm is 10%±1%, using a measurement sample in which the amount of solvent is adjusted as needed (by removing or adding the solvent), and the measurement is carried out at a temperature of 25°C±5°C. Specifically, the measurement is carried out using the method described in the "Measurement of the Transmission Spectrum of the Composition" in the following example.
[0250] Requirement (i): The average value of the transmittance in the wavelength range of 800 nm to 1100 nm is 10% or less.
[0251] The average value of the transmittance is preferably 8% or less, and more preferably 6% or less.
[0252] By using the present composition whose average transmittance in the wavelength range of 800nm to 1100nm is within the above range, an optical film or layer (D1) having sufficient infrared shielding properties can be easily formed, and a camera device having the above optical film or layer (D1) can set the light reaching the camera element to light close to the visual sensitivity of people who generally cannot perceive light in the infrared region.
[0253] When the present composition containing compound (A) is used to form a layer (D1), etc., the transmission spectrum obtained varies depending on the thickness of the layer (D1), etc. For example, the thickness can be adjusted according to the characteristics of the obtained transmittance by increasing the thickness of the layer (D1) etc. when the transmittance in the wavelength range of 800nm to 1100nm is to be further reduced, and decreasing the thickness of the layer (D1), etc. when the transmittance in a part of the visible light region of 460nm to 580nm is to be increased.
[0254] In addition, in the present invention, the average value of the transmittance at wavelengths A nm to B nm (average transmittance) is the value obtained by measuring the transmittance at each wavelength above A nm and below B nm with a scale of 1 nm, and dividing the total of the transmittance by the number of measured transmittances (wavelength range, B-A+1).
[0255] Requirement (ii): The average transmittance in the wavelength range of 460 nm to 580 nm is 80% or more.
[0256] By using the present composition having an average transmittance in the wavelength range of 460 nm to 580 nm within the above range, an optical film or layer (D1) having excellent transmittance of light in the visible light region can be easily formed, and an imaging device having the above optical film or layer (D1) can easily obtain a brighter image.
[0257] Requirement (iii): having a first cutoff wavelength at which the transmittance is 50% within the wavelength range of 680 nm to 780 nm.
[0258] By using the present composition having a first cutoff wavelength within the above range, an optical film or layer (D1) having excellent shielding properties for light belonging to the infrared region can be easily formed, and an imaging device having the above optical film or layer (D1) can set the light reaching the imaging element to be close to the visual sensitivity of people who generally cannot perceive light in the infrared region.
[0259] Requirement (iv): having a second cutoff wavelength with a transmittance of 50% within a wavelength range of 320 nm to 380 nm.
[0260] By using the present composition having a second cutoff wavelength within the above-mentioned range, an optical film or layer (D1) having excellent shielding properties for light belonging to the ultraviolet region can be easily formed. An imaging device having the above-mentioned optical film or layer (D1) can set the light reaching the imaging element to be close to the visual sensitivity of a person who generally cannot perceive light in the ultraviolet region. In addition, the influence of color bleeding such as purple fringing caused by the inclusion of short-wavelength light in the light reaching the imaging element can be reduced.
[0261] The present composition may satisfy the following requirements (v) to (vii) in addition to the above requirements (i) to (iv), and preferably satisfies the following requirements (v) to (vii).
[0262] Requirement (v): The standard deviation of the transmittance in the wavelength range of 900 nm to 1100 nm is 0.5% or less.
[0263] The standard deviation is preferably 0.3% or less.
[0264] When the concentration or amount of compound (A) is adjusted to increase the absorptivity of light in the wavelength range of 800 nm to 1200 nm, the absorptivity of light in the wavelength range of 900 nm to 1100 nm can be easily reduced when the deviation of the transmittance is small and the transmission spectrum is flatter.
[0265] When the standard deviation exceeds the above range, for example, even when the transmittance of light in the wavelength range of 800 nm to 1200 nm is sufficiently reduced, the transmittance in a part of the wavelength range may not be reduced sufficiently.
[0266] In the present invention, the standard deviation of the transmittance at wavelengths A nm to B nm is the standard deviation of the transmittance measured at each wavelength of A nm to B nm with 1 nm as a scale.
[0267] Requirement (vi): In the wavelength range of 300 nm to 1200 nm, the wavelength width of the band where the transmittance is 50% or more is 350 nm to 420 nm.
[0268] Requirement (vi) determines the width of the so-called transmission band. If the wavelength width is within the above range, there is a tendency that the transmission band in the visible light region becomes sufficiently long, a part of the transmission band is difficult to be shielded, and light outside the transmission band is easily shielded sufficiently.
[0269] Requirement (vii): The average value of the transmittance in the wavelength range of 1100 nm to 1200 nm is 10% or less.
[0270] The average value of the transmittance is preferably 8% or less.
[0271] In the case of a composition containing compound (A), the transmittance of light in a wavelength range of 1100 nm or more tends to be higher, but according to the present composition, the requirement (vii) can be easily satisfied. The present composition satisfying the requirement (vii) has the following tendencies: for example, the transmittance of light in a wavelength range of 800 nm to 1100 nm can be sufficiently reduced, and the transmittance of light with a wavelength of more than 1100 nm can be suppressed to a low level.
[0272] 《Optical films and layers (D1)》
[0273] The optical film and layer (D1) of the present invention are formed from the present composition. The optical film refers to a film obtained by forming a film from the present composition using a previously known method, and has the same meaning as layer (D1). Therefore, the following description related to layer (D1) can also be applied to the optical film. Hereinafter, the optical film and layer (D1) are also referred to as "layer (D1) etc."
[0274] When the layer (D1) etc. is used, for example, in an image pickup device or a camera module, the thinner the layer (D1) etc. is, the more advantageous it is for reducing the height of the image pickup device or the camera module. On the other hand, if the layer (D1) etc. is too thin, for example, the rigidity or mechanical strength is significantly reduced, and thus the handling of the layer (D1) etc. may become difficult.
[0275] Taking these into consideration, the thickness of the layer (D1) and the like is preferably 230 μm or less, more preferably 35 μm to 220 μm, and still more preferably 50 μm to 210 μm.
[0276] When the thickness of layer (D1) etc. is set to be less than 230 μm, the transmission spectrum when light with an incident angle of 0° is incident on the main surface (the surface with the largest area) of layer (D1) etc. may have the following characteristics (I) to (V), and preferably has the following characteristics (I) to (V).
[0277] Here, the characteristics related to the transmission spectrum of layer (D1) etc., especially the following characteristics (I) to (VIII) can be obtained specifically by the method described in "Measurement of the transmission spectrum of layer (D1-A1)" in the following Examples.
[0278] Characteristics (I): The average value of the transmittance in the wavelength range of 460 nm to 580 nm is 80% or more, preferably 85% or more.
[0279] In an imaging device having a layer (D1) satisfying characteristic (I), a beam of light in the visible light region that passes through the layer (D1) and reaches an imaging element becomes larger, making it easier to form a brighter image.
[0280] Characteristic (II): The average value of the transmittance in the wavelength range of 800 nm to 1100 nm is 5% or less, preferably 3% or less.
[0281] The layer (D1) etc. satisfying characteristic (II) can sufficiently shield light in the near-infrared region, and the imaging device etc. having the layer (D1) etc. can set the light reaching the imaging element etc. to light close to the visual sensitivity of people who generally cannot perceive light in the near-infrared region.
[0282] Characteristic (III): A third cutoff wavelength having a transmittance of 50% within a wavelength range of 680 nm to 730 nm. The third cutoff wavelength is preferably within a range of 680 nm to 720 nm.
[0283] The layer (D1) having the third cutoff wavelength within the above-mentioned range has excellent shielding properties for light in the near-infrared region, and the imaging device having the above-mentioned layer (D1) can set the light reaching the imaging element to be close to the visual sensitivity of people who generally cannot perceive light in the near-infrared region.
[0284] Furthermore, the absolute value of the difference between the third cutoff wavelength and the first cutoff wavelength is preferably 10 nm to 60 nm, and more preferably 15 nm to 55 nm.
[0285] The layer (D1) or the like in which the absolute value of the difference between the third cutoff wavelength and the first cutoff wavelength is within the above range does not significantly aggregate the compound (A) over time and has an excellent shelf life.
[0286] Characteristic (IV): A fourth cutoff wavelength having a transmittance of 50% in the wavelength range of 340 nm to 400 nm. The fourth cutoff wavelength is preferably in the range of 350 nm to 400 nm, and more preferably in the range of 360 nm to 400 nm.
[0287] The layer (D1) satisfying characteristic (IV) has excellent shielding properties for light in the ultraviolet region. An imaging device having the layer (D1) can set the light reaching the imaging element to be close to the visual sensitivity of a person who generally cannot perceive light in the ultraviolet region. In addition, the effects of color bleeding such as purple fringing caused by the inclusion of short-wavelength light in the light reaching the imaging element can be reduced.
[0288] Characteristic (V): The maximum value of the transmittance at a wavelength of 950 nm is 1% or less, preferably 0.5% or less, and more preferably 0.2% or less.
[0289] The layer (D1) or the like satisfying the characteristic (V) can shield light in the near-infrared region having a wavelength of 900 nm to 1100 nm to a level that does not cause adverse effects due to the near-infrared light.
[0290] Furthermore, when the thickness of the layer (D1) is set to 230 μm or less, the transmission spectrum when light with an incident angle of 0° is incident on the main surface of the layer (D1) may have the following characteristics (VI) to (VIII), preferably the following characteristics (VI) to (VIII). These characteristics are indicators showing the shielding properties of light in the infrared region, and are sometimes valued as evaluation indicators of the layer (D1) etc.
[0291] Characteristics (VI): Transmittance at a wavelength of 800 nm is less than 3%
[0292] Characteristic (VII): Transmittance at a wavelength of 1000 nm is less than 0.5%
[0293] Characteristic (VIII): Transmittance at a wavelength of 1100nm is less than 0.5%
[0294] <Method for forming layer (D1) etc.>
[0295] The method for forming the layer (D1) and the like is not particularly limited, and the layer (D1) and the like can be formed by a conventionally known method other than using the present composition.
[0296] As a method for forming a monolayer layer (D1), for example, melt forming, casting method (casting method), extrusion forming method, and calender method can be cited. Among these, when the layer (D1) is used for an optical part, considering the smoothness or low haze required for the optical part, mass production, and the thermal properties of the compound (A) contained in the present composition, melt forming and casting method are preferred.
[0297] Melt forming
[0298] As the melt forming, specifically, the following methods can be cited: a method of melt forming pellets obtained by melt kneading the present composition; a method of melt forming the present composition; a method of melt forming pellets obtained by removing the solvent from the present composition in a liquid state containing a solvent. Examples of the melt forming method include injection molding, melt extrusion molding, or blow molding.
[0299] ·Casting method
[0300] In the casting method, for example, the liquid composition is cast on the main surface of a support such as a smooth glass plate or a metal belt using a dispenser or a mold, and then dried to form a coating film, and then the coating film is peeled off from the support to form a layer (D1) or the like.
[0301] Furthermore, the peeled layer (D1) and the like may be post-cured as necessary.
[0302] The main surface of the support on which the present composition is cast may be coated with, for example, a peeling accelerator (for example, a surface treatment agent containing a fluorine compound) to facilitate peeling of the obtained coating film from the support.
[0303] In addition, in order to form a layer (D1) of a specified thickness, for example, a frame (frame) of any shape can be arranged on the main surface of the support body, and a specified amount of the present composition can be cast in the frame, thereby controlling the thickness of the formed layer (D1) etc.
[0304] In addition, as a method for forming a layer (D1) suitable for mass production, for example, the present composition containing a solvent is applied by a slit die or the like on a support such as a smooth metal belt that is continuously moved by a plurality of rollers or the like, at least a portion of the solvent is evaporated on the support, and the applied present composition is dried and cured to form a coating film, and then the coating film is peeled off from the support to form a layer (D1) or the like. The obtained layer (D1) or the like may be passed through an oven, for example, as necessary, to evaporate the solvent to a nearly complete extent (post-curing).
[0305] Furthermore, the obtained layer (D1) and the like may be stretched as necessary, or may be wound up using a winding roll or the like.
[0306] Optical Filters
[0307] The optical filter of the present invention (hereinafter also referred to as "the present filter") is a filter having the layer (D1), and preferably further comprises a dielectric multilayer film in terms of being able to easily obtain an optical filter having desired optical characteristics. In addition, the layers (films) other than the dielectric multilayer film constituting the present filter are hereinafter also referred to as "substrate (i)".
[0308] The layer (D1) included in the filter may be one layer, or the filter may have two or more identical or different layers (D1).
[0309] In terms of further exerting the effects of the present invention, the present filter is preferably a so-called near-infrared cutoff filter that transmits light in the visible light region and blocks light in the near-infrared region, or a so-called dual-bandpass filter that transmits light in the visible light region and a portion of light in the near-infrared region and blocks light in the near-infrared region other than the portion of light in the near-infrared region to be transmitted, and is more preferably a near-infrared cutoff filter.
[0310] When the filter is used, for example, in an image pickup device or camera module, the thinner the filter is, the more advantageous it is for reducing the height of the image pickup device or camera module. On the other hand, if the filter is too thin, for example, the rigidity or mechanical strength may be significantly reduced.
[0311] Taking these into consideration, the thickness of the present filter is preferably 60 μm to 300 μm, more preferably 70 μm to 280 μm, and even more preferably 80 μm to 250 μm.
[0312] <Base material (i)>
[0313] The substrate (i) is not particularly limited as long as it has the layer (D1), and may be a single layer or a multilayer.
[0314] In addition, the substrate (i) may have one layer or two or more layers of at least one selected from an outer coating layer and a functional film.
[0315] The substrate (i) is preferably a substrate (i-1) comprising a layer (D1-1) containing the compound (A), the polymer (B1) and the dye (C) as the layer (D1), or
[0316] The substrate (i) preferably comprises a layer (D1-2) as the layer (D1) not containing the dye (C), and a layer (D2) containing a dye (C) other than the compound (A) and not containing the compound (A).
[0317] The substrate (i-1) may have two or more layers (D1-1), and may further have one or two or more layers of at least one layer selected from the layer (D1-2) and the layer (D2) described below.
[0318] In addition, the substrate (i-2) may have two or more layers (D1-2), or may have two or more layers (D2).
[0319] The layer (D1-1) and the layer (D1-2) are the same layers as those described in the column of the layer (D1) except that they contain or do not contain the dye (C).
[0320] The substrate (i) may be laminated with a layer (D1) on a glass support, and preferably further laminated with a layer (D2). In such a substrate (i), there is no particular problem in the lamination order of the glass support, the layer (D1), and the layer (D2), and the glass support, the layer (D1), and the layer (D2) may each be two or more layers.
[0321] The glass support is not particularly limited, and examples thereof include fluorophosphate glass, near infrared absorbing glass (e.g., absorbing glass obtained by adding CuO or the like to phosphate glass), soda-lime glass, borosilicate glass, alkali-free glass, quartz glass, sapphire glass, etc. In addition, the "phosphate glass" also includes silicophosphate glass in which a part of the glass skeleton is composed of SiO2.
[0322] The thickness of the substrate (i) can be appropriately selected according to the desired use without particular limitation, but is ideally selected to reduce the incident angle dependence of the obtained optical filter, preferably 20 μm to 230 μm, more preferably 35 μm to 220 μm, and particularly preferably 50 μm to 210 μm.
[0323] When the thickness of the substrate (i) is within the above range, an optical filter using the substrate (i) can be made thinner and lighter, and can be preferably used in various applications such as a solid-state imaging device.
[0324] Although it depends on the purpose of the present filter, the substrate (i) preferably satisfies the following (α) to (ε). In addition, the following (α) to (ε) relate to the measurement of the transmittance of light incident from a direction of 0° relative to the main surface of the substrate (i).
[0325] (α): There is a wavelength at which the transmittance increases from less than 50% to more than 50% in the wavelength range of 350 nm to 450 nm, preferably 375 nm to 435 nm, and more preferably 400 nm to 420 nm.
[0326] (β): The average value of the transmittance at a wavelength of 430 nm to 570 nm (visible region) is 70% or more, preferably 72.5% or more, and more preferably 75% or more.
[0327] The average value of the transmittance is preferably high, and therefore the upper limit thereof is not particularly limited, and may be 100%.
[0328] (γ): There is a wavelength (IR50) at which the transmittance changes from more than 50% to less than 50% in the wavelength range of 600 nm to 700 nm.
[0329] IR50 is preferably present in the range of preferably 610 nm or more, more preferably 615 nm or more, further preferably 620 nm or more, particularly preferably 630 nm or more, and preferably less than 700 nm, more preferably less than 690 nm, further preferably less than 690 nm, particularly preferably less than 685 nm.
[0330] In the presence of such a wavelength, a substrate (i) having both wide-range, steep near-infrared absorption and high visible light transmittance can be easily obtained, and unnecessary near-infrared rays can be selectively and efficiently cut off. Moreover, when a dielectric multilayer film is formed on the substrate (i), the incident angle dependence of the optical properties near the visible light wavelength to near-infrared wavelength region can be reduced, and a good camera image with reduced ghosting or color shading can be easily obtained.
[0331] (δ): In the wavelength range of 700 nm to 800 nm, the average transmittance is 1% or less, preferably 0.75% or less, and more preferably 0.5% or less.
[0332] (ε): In the wavelength range of 800 nm to 1100 nm, the maximum transmittance is 40% or less, preferably 35% or less, and more preferably 30% or less.
[0333] [Layer (D2)]
[0334] The layer (D2) is not particularly limited as long as it contains the pigment (C) and does not contain the compound (A), but is preferably a layer (D2) formed by a composition (D2) containing the pigment (C) and at least one selected from a polymer (B2-1) and a curable compound (B2-2) that is cured by light or heat.
[0335] The present filter having layer (D2) can achieve a steeper cutoff characteristic than the present filter containing compound (A) and not containing pigment (C) due to the absorption characteristics of pigment (C), and has a tendency to have less change in spectral characteristics caused by the incident angle of light incident on the present filter.
[0336] When the layer (D2) is used, for example, for installation in an imaging device or a camera module, the thinner the layer (D2), the more advantageous it is for reducing the height of the imaging device or the camera module. On the other hand, if the layer (D2) is too thin, in order to achieve the target spectral characteristics, the concentration of the pigment (C) in the layer (D2) may have to be increased, and for example, the precipitation or storage stability of the pigment (C) may become a problem.
[0337] Taking these into consideration, the thickness of the layer (D2) is preferably 1 μm to 120 μm, more preferably 2 μm to 110 μm, and even more preferably 3 μm to 100 μm.
[0338] [Pigment (C)]
[0339] The pigment (C) is the same pigment as the pigment (C) described in the column of the present composition.
[0340] The coloring matter (C) used in the composition (D2) may be one kind or two or more kinds.
[0341] The content of the pigment (C) in the composition (D2) is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.2 to 2 parts by mass, relative to 100 parts by mass of the total of the polymer (B2-1) and the curable compound (B2-2).
[0342] When the content of the dye (C) is within the above range, the light absorption characteristics of the dye (C) are fully exhibited, and the present filter having the formed layer (D2) has desired optical characteristics.
[0343] [Polymer (B2-1)]
[0344] The polymer (B2-1) is not particularly limited as long as it is a polymer other than the curable compound (B2-2) described later.
[0345] When the polymer (B2-1) is used in the composition (D2), the polymer (B2-1) used may be one kind or two or more kinds.
[0346] As the polymer (B2-1), for example, in terms of ensuring thermal stability or formability of the layer (D2) and easily obtaining a layer that can form a dielectric multilayer film by high-temperature evaporation at a evaporation temperature of about 100°C or above, there can be listed polymers having a glass transition temperature (Tg) of preferably 110°C to 380°C, more preferably 110°C to 370°C, and particularly preferably 120°C to 360°C.
[0347] When the Tg of the polymer (B2-1) is 140°C or higher, a layer capable of forming a dielectric multilayer film by vapor deposition at a higher temperature can be obtained, which is particularly preferred.
[0348] As the polymer (B2-1), it is desirable to use a polymer having a total light transmittance (Japanese Industrial Standards (JIS) K 7375: 2008) of preferably 75% to 95%, more preferably 78% to 95%, and particularly preferably 80% to 95% of a plate having a thickness of 0.1 mm containing the polymer.
[0349] When the polymer (B2-1) having a total light transmittance within the above range is used, a layer (D2) or an optical filter having excellent transparency can be easily obtained.
[0350] The weight average molecular weight (Mw) of the polymer (B2-1) measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 15,000 to 350,000, more preferably 30,000 to 250,000, and the number average molecular weight (Mn) is preferably 10,000 to 150,000, more preferably 20,000 to 100,000.
[0351] Examples of the polymer (B2-1) include cyclic (poly) olefin polymers, polyether polymers, polyimide polymers, polyester polymers, polycarbonate polymers, polyamide (aromatic polyamide) polymers, polysulfone polymers, polyethersulfone polymers, polyparaphenylene polymers, polyamideimide polymers, polyethylene naphthalate (PEN) polymers, fluorinated aromatic polymer polymers, (modified) acrylic polymers, and epoxy polymers.
[0352] Specific examples of these polymers include resins described in International Publication No. 2019 / 168090.
[0353] Furthermore, as the polymer (B2-1), the above-mentioned polymer (B1) can also be used.
[0354] When the composition (D2) contains the polymer (B2-1), the content of the polymer (B2-1) is preferably 5% by mass to 30% by mass, more preferably 10% by mass to 25% by mass, in terms of the viscosity (applicability) of the composition (D2).
[0355] [Curing compound (B2-2)]
[0356] The curable compound (B2-2) is not particularly limited as long as it is a compound that is cured by light or heat.
[0357] When the compound (B2-2) is used in the composition (D2), the compound (B2-2) used may be one kind or two or more kinds.
[0358] Examples of the compound (B2-2) include epoxy compounds, allyl ester curable compounds, silsesquioxane photocurable compounds, acrylic photocurable compounds, acrylic thermosetting compounds, and vinyl photocurable compounds. Among these, epoxy compounds, silsesquioxane photocurable compounds, acrylic photocurable compounds, and acrylic thermosetting compounds are preferred.
[0359] As the compound (B2-2), it is desirable that the total light transmittance (JIS K 7375:2008) of the layer (D2) with a thickness of 0.1 mm obtained from the composition (D2) containing the compound (B2-2) is preferably 75% to 95%, more preferably 78% to 95%, and particularly preferably 80% to 95%.
[0360] As compound (B2-2), for example, in terms of ensuring thermal stability and formability of layer (D2) and easily obtaining a layer that can form a dielectric multilayer film by high-temperature vapor deposition at a vapor deposition temperature of about 100°C or above, it is ideal to use a compound that can form a layer (D2) having a glass transition temperature (Tg) of preferably 110°C to 380°C, more preferably 110°C to 370°C, and even more preferably 120°C to 360°C.
[0361] Furthermore, when a compound capable of forming a layer (D2) having a Tg of 140° C. or higher is used, a layer (D2) capable of being molded or processed at a high temperature can be obtained, which is more preferred.
[0362] (Epoxy compounds)
[0363] Examples of the epoxy compound include unsaturated compounds having an oxetane group, such as oxetane (cyclo)alkyl (meth)acrylates, oxetane (cyclo)alkyl α-alkylacrylates, and glycidyl ether compounds having an unsaturated bond; and unsaturated compounds having an oxetane group, such as (meth)acrylates having an oxetane group.
[0364] Examples of the oxirane (cyclo)alkyl (meth)acrylate include glycidyl (meth)acrylate, 2-methylglycidyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, 3,4-epoxybutyl (meth)acrylate, 6,7-epoxyheptyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, and 3,4-epoxycyclohexylmethyl (meth)acrylate.
[0365] Examples of the oxacyclopropyl (cyclo)alkyl α-alkylacrylate include glycidyl α-ethylacrylate, glycidyl α-n-propylacrylate, glycidyl α-n-butylacrylate, 6,7-epoxyheptyl α-ethylacrylate, and 3,4-epoxycyclohexyl α-ethylacrylate.
[0366] Examples of the glycidyl ether compound having an unsaturated bond include o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, and p-vinylbenzyl glycidyl ether.
[0367] Examples of the (meth)acrylate having an oxetane group include 3-((meth)acryloyloxymethyl)oxetane, 3-((meth)acryloyloxymethyl)-3-ethyloxetane, 3-((meth)acryloyloxymethyl)-2-methyloxetane, 3-((meth)acryloyloxyethyl)-3-ethyloxetane, 2-ethyl-3-((meth)acryloyloxyethyl)oxetane, 3-methyl-3-(meth)acryloyloxymethyloxetane, and 3-ethyl-3-(meth)acryloyloxymethyloxetane.
[0368] Among these, glycidyl methacrylate, 2-methylglycidyl methacrylate, 3,4-epoxycyclohexyl methacrylate, 3,4-epoxycyclohexylmethyl methacrylate, 3-methacryloyloxymethyl-3-ethyloxetane, 3-methyl-3-methacryloyloxymethyloxetane, or 3-ethyl-3-methacryloyloxymethyloxetane is particularly preferred in terms of polymerizability and the like.
[0369] (Silsesquioxane-based photocurable compound)
[0370] The silsesquioxane-based photocurable compound is preferably a compound represented by the following formula (1).
[0371] [RSiO 3 / 2 ] n (1)
[0372] (In formula (1), R is an organic functional group having any one of (meth)acryloyl, glycidyl, oxetanyl or vinyl, and n is 8, 10, 12 or 14)
[0373] The silsesquioxane-based photocurable compound is preferably a compound obtained by subjecting a silicon compound represented by the following formula (2) to hydrolysis reaction in the presence of an organic polar solvent and an alkaline catalyst, partially condensing the hydrolysis product, and further condensing the hydrolysis product in the presence of a non-polar solvent and an alkaline catalyst.
[0374] RSiX3(2)
[0375] (In formula (2), R is an organic functional group having any one of a (meth)acryloyl group, a glycidyl group, an oxetanyl group or a vinyl group, and X is a hydrolyzable group)
[0376] Examples of the organic functional group having any one of a (meth)acryloyl group, a glycidyl group, an oxetanyl group or a vinyl group in formula (1) and formula (2) include organic functional groups represented by the following formula (3), formula (4), formula (5) or formula (6).
[0377] [Chemistry 5]
[0378]
[0379] (In formula (3) and formula (4), m is an integer of 1 to 3, and in formula (3), R1 is a hydrogen atom or a methyl group)
[0380] [Chemistry 6]
[0381]
[0382] (In formula (6), R 5 , R 6 , R 7 , R 8 and R 9 are independently a hydrogen atom, a fluorine atom, an alkyl group having 1 to 4 carbon atoms, a phenyl group or a perfluoroalkyl group having 1 to 4 carbon atoms, and n is an integer of 1 to 6)
[0383] (Acrylic photocurable compound)
[0384] Examples of the acrylic photocurable compound include trimethylolpropane tri(meth)acrylate, di-trimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentyl (meth)acrylate, phenoxyethyl (meth)acrylate, glycerol tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, ethylene glycol di(meth)acrylate, 1,3-butanediol dimethacrylate, Hydroxyl-containing (meth)acrylates such as (meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and bis(2-hydroxyethyl)isocyanurate di(meth)acrylate; poly(meth)acrylates which are ethylene oxide or propylene oxide adducts on these hydroxyl groups; oligoester (meth)acrylates having two or more (meth)acryloyl groups in the molecule; oligoether (meth)acrylates; oligourethane (meth)acrylates; and oligoepoxy (meth)acrylates.
[0385] Among these, tricyclodecane dimethanol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, pentaerythritol tetra(meth)acrylate, and di-trimethylolpropane tetra(meth)acrylate are preferred.
[0386] Examples of commercially available products of the acrylic photocurable compound include Aronix M-400, M-408, M-450, M-305, M-309, M-310, M-315, M-320, M-350, M-360, M-208, M-210, M-215, M-220, M-225, M-233, M-240, M-245, M-260, M-270, M-1100, M-1200, M-1210, M-1260, and M-1300. 310, M-1600, M-221, M-203, TO-924, TO-1270, TO-1231, TO-595, TO-756, TO-1343, TO-902, TO-904, TO-905, TO-1330; KAYARAD D-310, D-330, DPHA, DPCA-20, DPCA-30, DPCA-60, DPCA-120, DN-0075, DN-2475, SR-295 manufactured by Nippon Kayaku Co., Ltd. , SR-355, SR-399E, SR-494, SR-9041, SR-368, SR-415, SR-444, SR-454, SR-492, SR-499, SR-502, SR-9020, SR-9035, SR-111, SR-212, SR-213, SR-230, SR-259, SR-268, SR-272, SR-344, SR-349, SR-601, SR-602, SR-610, SR-9003, PET- 30, T-1420, GPO-303, TC-120S, HDDA, NPGDA, TPGDA, PEG400DA, MANDA, HX-220, HX-620, R-551, R-712, R-167, R-526, R-712, R-604, R-684, TMPTA, THE-330, TPA-320, TPA-330, KS-HDDA, KS-TPGDA, KS-TMPTA; Light Acrylate PE-4A, DPE-6A, DTMP-4A manufactured by Kyoeisha Chemical Co., Ltd.; FA-511AS, FA-512AS manufactured by Resonac Co., Ltd.; NK Ester A-TMM-3LM-N, A-DPH manufactured by Shin-Nakamura Chemical Co., Ltd.
[0387] When an acrylic photocurable compound is used as the compound (B2-2), a photopolymerization initiator is usually used together with the acrylic photocurable compound.
[0388] When an acrylic photocurable compound is used as the compound (B2-2), a composition (D2) containing an acrylic photocurable compound and a photopolymerization initiator may be used, or a composition (D2) containing a cured product obtained by reacting and curing an acrylic photocurable compound and a photopolymerization initiator may be used.
[0389] The photopolymerization initiator is preferably a compound that can be decomposed by light irradiation to generate free radicals to start polymerization of the acrylic photocurable compound. Specific examples thereof include acetophenone, acetophenone benzyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2,2-dimethoxy-1,2-diphenylethane-1-one, xanthone, fluorenone, benzaldehyde, fluorene, anthraquinone, triphenylamine, carbazole, 3-methylacetophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, 4,4'-diaminobenzophenone, benzoin propyl ether, benzoin ethyl ether, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropane-1-one , 2-hydroxy-2-methyl-1-phenylpropane-1-one, thioxanthone, diethyl thioxanthone, 2-isopropyl thioxanthone, 2-chlorothioxanthone, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)acetone).
[0390] Examples of commercially available photopolymerization initiators include Irgacure 184, 369, 651, 500, 819, 907, 784, 2959, CGI1700, CGI1750, CGI1850, CG24-61, Darocur 1116, 1173, and Lucirin TPO manufactured by BASF; Uvecryl P36 manufactured by UCB; and Esacure KIP150, KIP65LT, KIP100F, KT37, KT55, KTO46, and KIP75 / B manufactured by Fratelli Lamberti.
[0391] The amount of the photopolymerization initiator used is preferably 0.5 to 15% by mass, more preferably 1 to 8% by mass, based on 100% by mass of the acrylic photocurable compound in order to sufficiently cure the acrylic photocurable compound.
[0392] (Acrylic thermosetting compound)
[0393] The acrylic thermosetting compound is not particularly limited, but preferably is a copolymer (a12) obtained by using at least one compound (a1) selected from the group consisting of unsaturated carboxylic acids and unsaturated carboxylic anhydrides and at least one compound (a2) selected from the group consisting of oxacyclopropyl-containing unsaturated compounds and oxacyclobutyl-containing unsaturated compounds. Such a copolymer (a12) can be produced by free radical copolymerization of an unsaturated mixture containing the compound (a1) and the compound (a2) in a solvent in the presence of a polymerization initiator.
[0394] Compound (a1) is an unsaturated carboxylic acid and / or an unsaturated carboxylic acid anhydride having free radical polymerizability, and examples thereof include: monocarboxylic acids, dicarboxylic acids, anhydrides of dicarboxylic acids, mono(meth)acryloyloxyalkyl) esters of polycarboxylic acids, mono(meth)acrylates of polymers having carboxyl groups and hydroxyl groups at both ends, polycyclic compounds having carboxyl groups and anhydrides thereof.
[0395] Examples of the unsaturated compound having an oxirane group include glycidyl (meth)acrylate, α-ethyl glycidyl (meth)acrylate, α-n-propyl glycidyl (meth)acrylate, α-n-butyl glycidyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 6,7-epoxyheptyl (meth)acrylate, α-ethyl (meth)acrylate-6,7-epoxyheptyl ester, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxycyclohexyl (meth)acrylate, methyl (meth)acrylate, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, and p-vinylbenzyl glycidyl ether. Among these, glycidyl methacrylate, 6,7-epoxyheptyl methacrylate, o-vinylbenzyl glycidyl ether, m-vinylbenzyl glycidyl ether, p-vinylbenzyl glycidyl ether, 3,4-epoxycyclohexyl methacrylate, 3,4-epoxycyclohexylmethyl methacrylate, and the like are preferred in terms of improving copolymerization reactivity and the heat resistance and chemical resistance of the obtained layer (D2).
[0396] Examples of the oxetane group-containing unsaturated compound include compounds in which the oxetane group of the above-mentioned oxetane group-containing unsaturated compound is replaced with an oxetane group.
[0397] The ratio of the mass of the structural unit derived from the compound (a2) to the mass of the structural unit derived from the compound (a1) in the copolymer (a12) ((a2) / (a1)) is preferably 1 or more, more preferably 1.1 or more, and even more preferably 1.2 or more.
[0398] When (a2) / (a1) is within the above range, a composition (D2) having high low-temperature storage stability, capable of long-term storage, and excellent in heat resistance, chemical resistance, etc. can be easily obtained.
[0399] The content of the structural unit derived from the compound (a2) is preferably 10 mass % or more, more preferably 15 mass % or more, and further preferably 20 mass % or more, relative to 100 mass % of all structural units constituting the copolymer (a12).
[0400] When the content of the structural unit is within the above range, a composition (D2) having high low-temperature storage stability, capable of long-term storage, and excellent in heat resistance, chemical resistance, etc. can be easily obtained.
[0401] The copolymer (a12) may have a structural unit derived from another unsaturated compound (a3) copolymerizable with the compound (a1) and the compound (a2), in addition to the structural unit derived from the compound (a1) and the compound (a2).
[0402] The compound (a3) is not particularly limited as long as it is an unsaturated compound having free radical polymerizability, and examples thereof include: (meth) alkyl acrylates, (meth) cyclic alkyl acrylates, (meth) aryl acrylates, unsaturated dicarboxylic acid diesters, (meth) acrylates having a hydroxyl group, bicyclic unsaturated compounds, maleimide compounds, unsaturated aromatic compounds, conjugated dienes, unsaturated compounds having at least one skeleton selected from a tetrahydrofuran skeleton, a furan skeleton, a tetrahydropyran skeleton, a pyran skeleton and a (poly) alkanediol skeleton, and unsaturated compounds having a phenolic hydroxyl group.
[0403] In terms of being able to easily form a layer (D2) having excellent heat resistance and chemical resistance, the content of the structural unit derived from compound (a1) is preferably 5% by mass to 40% by mass, and more preferably 5% by mass to 25% by mass, relative to 100% by mass of the total of the structural units derived from compound (a1), compound (a2) and compound (a3).
[0404] In terms of being able to easily form a layer (D2) having excellent heat resistance and chemical resistance, the content of the structural unit derived from compound (a2) is preferably 10% by mass to 80% by mass, and more preferably 20% by mass to 60% by mass, relative to 100% by mass of the total of the structural units derived from compound (a1), compound (a2) and compound (a3).
[0405] When an unsaturated compound having an alicyclic structure is used as compound (a3), in terms of easily being able to form a layer (D2) having better heat resistance, etc., the content of the structural unit derived from the unsaturated compound is preferably 10% by mass to 80% by mass, and more preferably 20% by mass to 60% by mass, relative to 100% by mass of the total of the structural units derived from compound (a1), compound (a2) and compound (a3).
[0406] The polystyrene-equivalent weight average molecular weight Mw of the acrylic thermosetting compound is preferably 2×10 3 ~1×10 5 , more preferably 5×10 3 ~5×10 4 .
[0407] The molecular weight distribution (Mw / Mn) of the acrylic thermosetting compound is preferably 5.0 or less, and more preferably 3.0 or less.
[0408] The acrylic thermosetting compound can be synthesized, for example, by polymerizing the compound (a1), the compound (a2), and the compound (a3) in an appropriate solvent in the presence of a radical polymerization initiator.
[0409] [additive]
[0410] The composition (D2) may contain additives other than the dye (C), the polymer (B2-1), and the compound (B2-2) within a range that does not impair the effects of the present invention.
[0411] Examples of the additive include the ultraviolet absorbing compound (U), a solvent, the light stabilizer, the silane coupling agent, an antioxidant, an adhesion promoter, a fluorescent matting agent, a plasticizer, and a filler. In addition, when the layer (D2) is formed from the composition (D2) by casting or the like, a leveling agent, a defoaming agent, a peeling accelerator, etc. may be used as an additive to facilitate the formation of the layer (D2).
[0412] These additives may be used alone or in combination of two or more.
[0413] These additives may be mixed together with the pigment (C), polymer (B2-1) and compound (B2-2) when preparing the composition (D2), or may be added when synthesizing the polymer (B2-1) or the compound (B2-2).
[0414] (solvent)
[0415] The composition (D2) is preferably prepared by mixing the dye (C) and at least one selected from the group consisting of the polymer (B2-1) and the compound (B2-2) in one or more solvents.
[0416] Examples of the solvent include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone;
[0417] Esters such as ethyl acetate and butyl acetate;
[0418] Alcohols such as isopropyl alcohol and ethyl alcohol;
[0419] Aromatic hydrocarbons such as benzene, toluene, xylene, methoxybenzene, and 1,2-dimethoxybenzene;
[0420] Phenol, parachlorophenol and other phenols;
[0421] Halogenated hydrocarbons such as chloroform, dichloromethane, dichloroethane, tetrachloroethane, trichloroethylene, tetrachloroethylene, and chlorobenzene;
[0422] Diethylene glycol alkyl ethers such as diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and diethylene glycol ethyl methyl ether;
[0423] Propylene glycol monoalkyl ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether and propylene glycol mono-n-butyl ether;
[0424] Propylene glycol monoalkyl ether acetates such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, propylene glycol mono-n-propyl ether acetate, and propylene glycol mono-n-butyl ether acetate;
[0425] 2-methoxypropionic acid methyl ester, 2-methoxypropionic acid ethyl ester, 2-methoxypropionic acid n-propyl ester, 2-methoxypropionic acid n-butyl ester, 2-ethoxypropionic acid methyl ester, 2-ethoxypropionic acid ethyl ester, 2-ethoxypropionic acid n-propyl ester, 2-ethoxypropionic acid n-butyl ester, 2-n-propoxypropionic acid methyl ester, 2-n-propoxypropionic acid ethyl ester, 2-n-propoxypropionic acid n-propyl ester, 2-n-propoxypropionic acid n-butyl ester, 2-n-butoxypropionic acid methyl ester, 2-n-butoxypropionic acid ethyl ester, 2-n-butoxypropionic acid n-propyl ester, 2-n-butoxypropionic acid n-butyl ester, 3-methoxy Alkoxypropionic acid alkyl esters such as methyl propionate, ethyl 3-methoxypropionate, n-propyl 3-methoxypropionate, n-butyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, n-propyl 3-ethoxypropionate, n-butyl 3-ethoxypropionate, methyl 3-n-propoxypropionate, ethyl 3-n-propoxypropionate, n-propyl 3-n-propoxypropionate, n-butyl 3-n-propoxypropionate, methyl 3-n-butoxypropionate, ethyl 3-n-butoxypropionate, n-propyl 3-n-butoxypropionate, and n-butyl 3-n-butoxypropionate.
[0426] When an acrylic photocurable compound is used as the composition (D2), it is preferred to use a solvent so that the viscosity of the composition (D2) is usually 0.1 mPa·sec / 25°C to 50,000 mPa·sec / 25°C, preferably 0.5 mPa·sec / 25°C to 10,000 mPa·sec / 25°C.
[0427] (Leveling agent)
[0428] The leveling agent is not particularly limited, and examples thereof include silicone-based and fluorine-based leveling agents.
[0429] When a leveling agent is used, one type of leveling agent may be used, or two or more types of leveling agents may be used.
[0430] As a silicone-based leveling agent, polydimethylsiloxane, polymethylalkylsiloxane, polyether-modified polydimethylsiloxane, and polysiloxane which has a (meth)acrylic group are mentioned, for example.
[0431] When a leveling agent is used, the amount of the leveling agent used is preferably 10% by mass or less, more preferably 3% by mass or less, based on 100% by mass of the solid content of the composition (D2).
[0432] (Antioxidant)
[0433] Examples of the antioxidant include hindered phenol-based, sulfur-based, and phosphorus-based antioxidants.
[0434] When an antioxidant is used, one kind of antioxidant may be used or two or more kinds of antioxidants may be used.
[0435] When an antioxidant is used, the amount of the antioxidant used is preferably 10% by mass or less, more preferably 3% by mass or less, based on 100% by mass of the solid content of the composition (D2).
[0436] [Method for forming layer (D2)]
[0437] The method for forming the layer (D2) is not particularly limited, and the layer (D2) can be formed by a conventionally known method except for using the composition (D2).
[0438] When a polymer such as the polymer (B2-1) is used as the composition (D2), the layer (D2) can be formed by the same method as the method for forming the layer (D1).
[0439] When a photocurable compound such as the acrylic photocurable compound is used as the composition (D2), the composition (D2) can be cured by irradiating light, preferably ultraviolet rays or electron beams, to form a layer (D2).
[0440] For example, when irradiating ultraviolet rays, the irradiation amount of ultraviolet rays is preferably 0.01 J / cm 2 ~10J / cm 2 , more preferably 0.1 J / cm 2 ~2J / cm 2 In addition, for example, in the case of electron beam irradiation, the electron beam irradiation conditions include the following conditions: the acceleration voltage is preferably 10 kV to 300 kV, and the electron density is preferably 0.02 mA / cm 2 ~0.30mA / cm 2 The electron beam irradiation amount is preferably 1 Mrad to 10 Mrad.
[0441] Moreover, when using the photocurable composition (D2) containing a solvent, it is preferable to irradiate light after drying the solvent (volatile component) at 0°C to 200°C, for example.
[0442] [Method for producing substrate (i)]
[0443] The method for producing the substrate (i) is not particularly limited, and the substrate (i) can be produced by a conventionally known method.
[0444] When the substrate (i) is a single layer of the layer (D1), the substrate (i) can be produced by the same method as the method for forming the layer (D1).
[0445] When the substrate (i) has, for example, a layer (D1) and a layer (D2), it can be produced by, for example, a method including the following lamination method 1 to lamination method 3.
[0446] ·Layering method 1
[0447] The lamination method 1 is a method in which the layer (D1) and the layer (D2) are separately formed in advance by the same method as described above, and the formed layer (D1) and the layer (D2) are directly bonded together or bonded together via an adhesive layer.
[0448] In such a case, the layer (D2) is preferably a layer formed of a composition (D2) using the polymer (B2-1).
[0449] As a method for direct lamination, the following method can be mentioned: for example, a solvent that dissolves the polymers contained in both layer (D1) and layer (D2) is applied to the lamination surface of layer (D1) and / or layer (D2), and the two layers are laminated and dried.
[0450] The adhesive layer is not particularly limited as long as it can bond the layer (D1) and the layer (D2), and examples thereof include a thermoplastic resin layer, a photocurable resin layer, and a thermosetting resin layer. The following adhesive layers may also include the same layers.
[0451] Among these, a method of bonding via a thermoplastic resin layer is particularly preferred in terms of less curing shrinkage during bonding, etc. When bonding via a thermoplastic resin layer, for example, the following method can be cited: a resin solution obtained by dissolving a thermoplastic resin in a solvent that is soluble in both the polymers contained in the layer (D1) and the layer (D2) is applied to the layer (D1) and / or the layer (D2), and the two layers are bonded and dried.
[0452] ·Layering method 2
[0453] The lamination method 2 is a method in which a layer (D1) is formed in advance by the same method as described above, a composition (D2) is applied on the formed layer (D1), and heat is applied to the applied composition (D2), thereby forming a layer (D2).
[0454] In such a case, the layer (D2) is preferably a layer formed of a composition (D2) using a thermosetting compound such as an acrylic thermosetting compound.
[0455] In the method 2, before coating the layer (D2), an intermediate layer may be provided on the layer (D1), or the surface of the layer (D1) may be subjected to a desired surface treatment (for example, surface treatment such as corona treatment or plasma treatment).
[0456] The coating method is not particularly limited, and known methods can be used, such as spraying, roller coating, spin coating, slot die coating, rod coating, and printing (e.g., inkjet printing). The following coating methods can also be listed in the same way.
[0457] The heating conditions when applying the heat may be appropriately set according to the composition (D2) or layer (D1) used, and examples thereof include heating at a heating temperature of 120° C. to 200° C. for 5 minutes to 1 hour.
[0458] Examples of the intermediate layer include a thermoplastic resin layer, a photocurable resin layer, and a thermosetting resin layer. The following intermediate layers may also be exemplified by the same.
[0459] ·Layering method 3
[0460] The lamination method 3 is a method of forming a layer (D1) in advance by the same method as described above, applying a composition (D2) on the formed layer (D1), and irradiating the applied composition (D2) with light to form a layer (D2).
[0461] In such a case, the layer (D2) is preferably a layer formed of a composition (D2) using a photocurable compound such as an acrylic photocurable compound.
[0462] In the method 3, before coating the layer (D2), an intermediate layer may be provided on the layer (D1), or the surface of the layer (D1) may be subjected to a desired surface treatment.
[0463] Examples of the irradiation conditions for the light irradiation include the same conditions as those for the ultraviolet ray or electron beam irradiation described in the section of the method for forming the layer (D2).
[0464] In the above-mentioned lamination methods 1 to 3, the layer (D1) and / or the layer (D2) may have two or more layers. An adhesive layer or an intermediate layer may be provided between the two or more layers (D1) or between the two or more layers (D2) in the same manner as described above.
[0465] In addition, in the lamination method 2 or the lamination method 3, the order of forming the layer (D1) and the layer (D2) may be reversed, that is, after the layer (D2) is formed in advance, the layer (D1) is formed on the formed layer (D2).
[0466] 〔Outer coating and functional film〕
[0467] The substrate (i) may have an outer coating layer or a functional film (eg, an antireflection film, a hard coating film, an antistatic film) within a range that does not impair the effects of the present invention.
[0468] The thickness of the outer coating layer or the functional film is preferably 0.1 μm to 20 μm, more preferably 0.5 μm to 10 μm, and particularly preferably 0.7 μm to 5 μm.
[0469] The material forming the outer coating layer or the functional film may be a composition containing a polymer as a main component used in the layer (D1) or the layer (D2). However, it is assumed that the outer coating layer or the functional film does not contain the compound (A) and the pigment (C).
[0470] In addition, the overcoat layer or the functional film may be formed by lamination as in the lamination method 1, or may be formed by coating as in the lamination method 2 or the lamination method 3.
[0471] There are no particular restrictions on the method for manufacturing the substrate (i) having an outer coating or a functional film, and the substrate can be manufactured by a previously known method. For example, the following method can be cited: using a rod coater, at least one coating agent selected from an antireflective agent, an outer coating agent, an intermediate layer agent, and an antistatic agent is applied to the adherend on which the outer coating or the functional film is to be formed, and then hardened by ultraviolet irradiation or the like.
[0472] Furthermore, before the coating, the adherend may be subjected to a surface treatment such as a corona treatment or a plasma treatment in order to improve the adhesion of the formed top coat layer or functional film.
[0473] Examples of the coating agent include a coating agent containing an ultraviolet (UV) / electron beam (EB) curable compound or a thermosetting compound.
[0474] Specific examples of these compounds include vinyl-based, urethane-based, urethane acrylate-based, acrylate-based, epoxy-based, and epoxy acrylate-based compounds.
[0475] In addition, the coating agent may also contain a polymerization initiator.
[0476] As the polymerization initiator, a known photopolymerization initiator or thermal polymerization initiator may be used, or a photopolymerization initiator and a thermal polymerization initiator may be used in combination. The polymerization initiator may be used alone or in combination of two or more.
[0477] When the total amount of the coating agent is set to 100 mass %, the mixing ratio of the polymerization initiator is preferably 0.1 mass % to 10 mass %, more preferably 0.5 mass % to 10 mass %, and further preferably 1 mass % to 5 mass %. If the mixing ratio of the polymerization initiator is within the above range, a coating agent with excellent curing characteristics and operability can be easily obtained, and an outer coating or functional film with a desired hardness can be easily obtained.
[0478] Furthermore, an organic solvent may be added to the coating agent, and a known organic solvent may be used.
[0479] Specific examples of the organic solvent include: alcohols such as methanol, ethanol, isopropanol, butanol, and octanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate, butyl acetate, ethyl lactate, γ-butyrolactone, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate; ethers such as ethylene glycol monomethyl ether and diethylene glycol monobutyl ether; aromatic hydrocarbons such as benzene, toluene, and xylene; and amides such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone.
[0480] These organic solvents may be used alone or in combination of two or more.
[0481] 〔Dielectric multilayer film〕
[0482] Examples of the dielectric multilayer film include a laminate in which high-refractive index material layers and low-refractive index material layers are alternately laminated.
[0483] Although it depends on the application of the present filter, when the present filter is used as a filter that shields at least a part of near-infrared rays, the dielectric multilayer film is preferably a laminate having a capability of reflecting near-infrared rays.
[0484] The dielectric multilayer film may be provided on one side or both sides of the substrate (i). When the dielectric multilayer film is provided on one side of the substrate (i), the manufacturing cost or manufacturing ease is excellent. In addition, when the dielectric multilayer film is provided on both sides of the substrate (i), an optical filter having high strength and not prone to warping or torsion can be easily obtained. When the present filter is used for solid-state imaging elements, it is preferred that the dielectric multilayer film be provided on both sides of the substrate (i) for filters having preferably small warping or torsion.
[0485] As the material constituting the high refractive index material layer, a material having a refractive index of 1.7 or more can be used, and a material having a refractive index of 1.7 to 2.5 is generally selected. Such a material includes, for example, titanium oxide, zirconium oxide, tantalum pentoxide, niobium pentoxide, lanthanum oxide, yttrium oxide, zinc oxide, zinc sulfide, or indium oxide as a main component, and a material containing a small amount (for example, 0 mass % to 10 mass % relative to the main component) of tin oxide and / or cerium oxide.
[0486] As the material constituting the low refractive index material layer, a material having a refractive index of 1.6 or less can be used, and a material having a refractive index of generally 1.2 to 1.6 is selected. Examples of such materials include silicon dioxide, aluminum oxide, lanthanum fluoride, magnesium fluoride, and sodium aluminum hexafluoride.
[0487] There is no particular limitation on the method of stacking the high refractive index material layer and the low refractive index material layer, as long as a dielectric multilayer film formed by stacking these material layers is formed. For example, a dielectric multilayer film formed by alternately stacking high refractive index material layers and low refractive index material layers can be directly formed on the substrate (i) by chemical vapor deposition (CVD), sputtering, vacuum evaporation, ion-assisted evaporation or ion plating.
[0488] In the case where the dielectric multilayer film is set to a dielectric multilayer film having the ability to reflect near-infrared rays, if the wavelength of the near-infrared rays to be blocked is set to λ(nm), the thickness of each layer of the high refractive index material layer and the low refractive index material layer is usually preferably 0.1λ to 0.5λ. As the value of λ(nm), for example, 700nm to 1400nm, preferably 750nm to 1300nm. If the thickness is in the range, the product (n×d) of the refractive index (n) and the film thickness (d) becomes the same value as the optical film thickness (nd) calculated using λ / 4, and the thickness of each layer of the high refractive index material layer and the low refractive index material layer, and according to the relationship between the optical characteristics of reflection and refraction, there is a tendency to easily control the blocking and transmission of specific wavelengths.
[0489] The total number of stacked layers of high refractive index material layers and low refractive index material layers in the dielectric multilayer film is preferably 6 to 70 layers, more preferably 10 to 60 layers, based on the entire filter. If the thickness of each layer, the thickness of the dielectric multilayer film based on the entire filter, or the total number of stacked layers is within the above range, sufficient manufacturing margin can be ensured, and warping of the filter or cracks in the dielectric multilayer film can be reduced.
[0490] If the types of materials constituting the high refractive index material layer and the low refractive index material layer, the thickness of each layer of the high refractive index material layer and the low refractive index material layer, the stacking order, and the number of stacking layers are appropriately selected in combination with the absorption characteristics of the substrate (i), it is easy to obtain this filter which ensures sufficient transmittance in the visible light region, has sufficient light cutting characteristics in the near infrared region, and reduces the reflectivity when the near infrared light is incident from an oblique direction.
[0491] <Application of this filter>
[0492] Since the filter has the layer (D1), it has high visible light transmittance and low near infrared transmittance, and has excellent durability even in a high temperature and high humidity environment.
[0493] By using this filter, a good camera image with good red, green and blue (RGB) balance and reduced ghosting or color shading can be obtained.
[0494] Therefore, the present filter is effectively used for the purpose of correcting the visual sensitivity of solid-state imaging elements such as CCD or CMOS image sensors of camera modules. In particular, the present filter is effectively used in digital still cameras, cameras for smartphones, cameras for mobile phones, digital video cameras, cameras for wearable devices, personal computer (PC) cameras, surveillance cameras, car cameras, televisions, car navigation, portable information terminals, video game consoles, portable game consoles, fingerprint authentication systems, digital music players, etc. Furthermore, the present filter is also effectively used as an infrared cut filter installed on glass plates of cars or buildings, etc.
[0495] 《Optical element, solid-state imaging device, and camera module》
[0496] The optical element, solid-state imaging device, and camera module of the present invention are not particularly limited as long as they include the present filter, and may be of a conventionally known configuration.
[0497] A camera module is a preferred example of the solid-state imaging device.
[0498] Here, the solid-state imaging device and camera module are image sensors including solid-state imaging elements such as CCD or CMOS image sensors, and can be specifically used in digital still cameras, cameras for smartphones, cameras for mobile phones, cameras for wearable devices, digital video cameras, and the like.
[0499] The optical element, the solid-state imaging device, and the camera module may have the following structures: Figure 1 (A) Figure 1 The structure of the lens may be as shown in (B). Figure 2 (A) Figure 2 The structure does not have a lens as in (B).
[0500] Figure 1 (A) Figure 1 (B) shows an example of the configuration of each component when the filter is used in an optical element, a solid-state imaging device or a module. Figure 1 (A) Figure 1 In (B), the filter 1 is formed together with the lens 32 and the imaging element (image sensor) 24. The optical filter 1 can be Figure 1 (A) is located in front of the lens 32 (on the opposite side of the imaging element 24 of the lens 32), or Figure 1 As shown in (B), it is located behind the lens 32 (on the imaging element 24 side of the lens 32).
[0501] In addition, this filter can also be Figure 2As in (A), it is used in a lensless solid-state imaging device using an optical element 33 having a function as a lens such as a Fresnel zone plate, a Fresnel lens, or a metalens.
[0502] [Example]
[0503] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples at all.
[0504] <Polymer B1-1 to Polymer B1-4>
[0505] Using the dihydric phenol component and the aromatic dicarboxylic acid halide as raw materials at the values (molar ratio) described in Table 1 below, a polymer was obtained in the same manner as described in Japanese Patent Nos. 5355330 and 5749621.
[0506] [Table 1]
[0507]
[0508] As the dihydric phenol component and the aromatic dicarboxylic acid halide in Table 1, the following products were used, respectively.
[0509] Bisphenol A: [2,2-bis(4-hydroxyphenyl)propane] (Mitsui Chemicals, Inc., "Bisphenol A")
[0510] Bisphenol TMC: [Bisphenol-3,3,5-trimethylcyclohexane] (manufactured by Honshu Chemical Industry Co., Ltd., "BisP-TMC")
[0511] Biphenol: [4,4-dihydroxybiphenyl] ("biphenol" manufactured by Honshu Chemical Industry Co., Ltd.)
[0512] Isophthaloyl chloride: (Iharanikkei Chemical Industry Co., Ltd., "isophthaloyl chloride")
[0513] <Polymer B2-1-1>
[0514] 8-methyl-8-methoxycarbonyltetracyclic [4.4.0.1 2,5 .1 7,10] 100g of dodecyl-3-ene (hereinafter also referred to as "DNM"), 18g of 1-hexene (molecular weight regulator) and 300g of toluene (solvent for ring-opening polymerization reaction) were placed in a nitrogen-substituted reaction vessel, and the obtained solution was heated to 80°C. Then, 0.2g of a toluene solution (0.6mol / liter) of triethylaluminum as a polymerization catalyst and 0.9g of a toluene solution (concentration 0.025mol / liter) of tungsten hexachloride modified with methanol were added to the solution in the reaction vessel, and the obtained solution was heated and stirred at 80°C for 3 hours, thereby performing a ring-opening polymerization reaction to obtain a ring-opening polymer solution. The polymerization conversion rate in the polymerization reaction was 97%.
[0515] [Chemistry 7]
[0516]
[0517] 1,000 g of the obtained ring-opening polymer solution was placed in an autoclave, and 0.12 g of RuHCl(CO)[(C6H5)3]3 was added to the ring-opening polymer solution. 2 , reaction temperature 165 ° C, heating and stirring for 3 hours to carry out hydrogenation reaction. After cooling the obtained reaction solution (hydrogenated polymer solution), the hydrogen gas is depressurized. The obtained reaction solution is injected into a large amount of methanol and the coagulant is separated and recovered, and the coagulant is dried to obtain a hydrogenated polymer. The number average molecular weight (Mn) of the obtained polymer is 32,000, the weight average molecular weight (Mw) is 137,000, and the glass transition temperature (Tg) is 165 ° C. It is set as polymer B2-1-1.
[0518] <Polymer B2-1-2>
[0519] ZEONOR (Mn: 18,000, Mw: 38,000) manufactured by Nippon Zeon Co., Ltd. was used as polymer B2-1-2.
[0520] <Polymer B2-1-3>
[0521] 35.12 g (0.253 mol) of 2,6-difluorobenzonitrile, 87.60 g (0.250 mol) of 9,9-bis(4-hydroxyphenyl)fluorene, 41.46 g (0.300 mol) of potassium carbonate, 443 g of N,N-dimethylacetamide, and 111 g of toluene were added to a 3 L four-necked flask. A thermometer, a stirrer, a three-way stopcock with a nitrogen inlet tube, a Dean-Stark tube, and a cooling tube were then installed in the four-necked flask.
[0522] Then, after replacing the flask with nitrogen, the obtained solution was reacted at 140°C for 3 hours, removing generated water from the Dean-Stark tube as needed. When the generation of water was no longer confirmed, the temperature was gradually raised to 160°C, and the reaction was continued for 6 hours at the temperature in this state.
[0523] After cooling to room temperature (25°C), the generated salt was removed by filter paper, and the filtrate was placed in methanol for reprecipitation, and the filtrate (residue) was separated by filtration. The obtained filtrate was vacuum dried at 60°C overnight to obtain a white powder (hereinafter also referred to as "polymer B2-1-3") (yield 95%). The number average molecular weight (Mn) of the obtained polymer B2-1-3 was 75,000, the weight average molecular weight (Mw) was 188,000, and the glass transition temperature (Tg) was 285°C.
[0524] <Polymer B2-1-4>
[0525] Under nitrogen flow, 27.66 g (0.08 mol) of 1,4-bis(4-amino-α,α-dimethylbenzyl)benzene and 7.38 g (0.02 mol) of 4,4'-bis(4-aminophenoxy)biphenyl were placed in a 500 mL five-necked flask equipped with a thermometer, a stirrer, a nitrogen inlet tube, a dropping funnel with a side tube, a Dean-Stark tube, and a cooling tube, and dissolved in 68.65 g of γ-butyrolactone and 17.16 g of N,N-dimethylacetamide. The obtained solution was cooled to 5°C using an ice-water bath, and 22.62 g (0.1 mol) of 1,2,4,5-cyclohexanetetracarboxylic dianhydride and 0.50 g (0.005 mol) of triethylamine as an imidization catalyst were added while maintaining the temperature. After the addition was completed, the temperature was raised to 180°C, and the distillate was removed by distillation at any time while reflux was performed for 6 hours. After the reaction is completed, air cooling is performed until the internal temperature reaches 100°C, and then 143.6 g of N,N-dimethylacetamide is added for dilution. The mixture is cooled while stirring to obtain 264.16 g of a polyimide resin solution having a solid content concentration of 20% by mass. A portion of the polyimide resin solution is injected into 1 L of methanol to precipitate the polyimide. The filtered and separated polyimide is washed with methanol and dried in a vacuum dryer at 100°C for 24 hours to obtain a white powder (hereinafter also referred to as "polymer B2-1-4"). The IR spectrum of the obtained polymer B2-1-4 was measured, and the results showed that the 1704 cm-1 peculiar to the imide group -1 、1770cm -1 The glass transition temperature (Tg) of polymer B2-1-4 was 310°C, and the logarithmic viscosity was measured to be 0.87.
[0526] In addition, the logarithmic viscosity of the polymer B2-1-4 was measured by the following method.
[0527] A portion of the polyimide resin solution was put into anhydrous methanol to precipitate the polyimide resin, which was filtered and separated from the unreacted monomer. 0.1 g of the polyimide obtained by vacuum drying at 80° C. for 12 hours was dissolved in 20 mL of N-methyl-2-pyrrolidone, and the logarithmic viscosity (μ) at 30° C. was calculated using the following formula using a Cannon-Fenske viscometer.
[0528] μ={ln(t s / t0)} / C
[0529] t0: solvent flow time
[0530] t s : Flow time of dilute polymer solution
[0531] C: 0.5 g / dL
[0532] <Polymer B2-1-5>
[0533] In a reactor equipped with a thermometer, a stirrer, and a reflux cooler, 14863 parts by mass of ion exchange water and 5772 parts by mass of a 48% sodium hydroxide aqueous solution were added, 2148 parts by mass of 1,1-bis(4-hydroxyphenyl)cyclohexane and 4 parts by mass of sodium hydrogen sulfite were dissolved, 8518 parts by mass of dichloromethane were added, and 1000 parts by mass of phosgene was blown in at 23°C to 27°C for 60 minutes while stirring. After the blowing of phosgene was completed, 38 parts by mass of p-tert-butylphenol was added, and 2 parts by mass of triethylamine were added, and the mixture was stirred at 20°C to 27°C for 40 minutes to terminate the reaction. After washing the dichloromethane layer containing the product with dilute hydrochloric acid and pure water, the dichloromethane was evaporated to obtain a polycarbonate having a repeating unit represented by the following formula (7). The viscosity average molecular weight of the obtained polycarbonate was 21,000, and the glass transition temperature (Tg) was 174°C. The obtained polycarbonate was designated as polymer B2-1-5.
[0534] [Chemistry 8]
[0535]
[0536] <Polymer B2-2-1>
[0537] In a flask equipped with a cooling tube and a stirrer, 7 parts by mass of 2,2′-azobis(2,4-dimethylvaleronitrile) and 200 parts by mass of diethylene glycol ethyl methyl ether were charged in advance based on 100 parts by mass of the unsaturated mixture described below.
[0538] 100 parts by mass of an unsaturated mixture containing 20% by mass of methacrylic acid, 30% by mass of glycidyl methacrylate, and 50% by mass of methyl methacrylate was added thereto, and after nitrogen substitution, stirring was slowly started. The temperature of the solution was raised to 70° C. and maintained at the temperature for 4 hours to terminate the polymerization.
[0539] After that, the reaction solution was added dropwise to a large amount of methanol to solidify the reactant. The solidified product was washed with water, redissolved in tetrahydrofuran, and solidified again using a large amount of methanol. The redissolution-solidification operation was performed a total of 3 times, and the obtained solidified product was vacuum dried at 60° C. for 48 hours to obtain the target polymer B2-2-1.
[0540] [Example A1]
[0541] 4.88 g of copper acetate monohydrate (hereinafter also referred to as "CAM". Manufactured by Kanto Chemical Co., Ltd.) was mixed with 195.12 g of ethanol (manufactured by Kanto Chemical Co., Ltd., EL grade for the electronics industry) as a first solvent, and stirred for 3 hours to obtain a copper acetate solution. Next, 2.572 g of a phosphate compound (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name: Plysurf A208N) was added to the obtained copper acetate solution, and stirred for 30 minutes to obtain a1 solution as a copper acetate-phosphate solution.
[0542] Next, 2.886 g of n-butylphosphonic acid (hereinafter also referred to as "BPA") and 40 g of ethanol were added, and the mixture was stirred for 10 minutes to obtain liquid b1 which is a phosphonic acid solution.
[0543] While stirring the a1 liquid, the b1 liquid was added to the a1 liquid, and the mixture was stirred at room temperature for 15 minutes to react, thereby obtaining the c1 liquid which is a phosphate-phosphonic acid-copper solution. It can be visually confirmed that a solid substance generated by the reaction is precipitated in the c1 liquid. The reaction product is considered to be a compound containing part or all of the phosphonic acid, phosphoric acid ester and copper components.
[0544] The liquid c1 containing the precipitate was suction filtered to obtain a solid reaction product. The solid reaction product was added to 200 g of ethanol, stirred at room temperature for 10 minutes, and suction filtered again to obtain a primary purified solid compound A-1.
[0545] 3.22 g of polymer B1-1 was added to 80 g of toluene as the second solvent, and stirred at room temperature for 10 minutes to obtain a solution. Compound A-1 was added to the obtained solution, and stirred at room temperature for another 10 minutes to obtain liquid d1 in which compound A-1 was dispersed in the solution.
[0546] In the d1 solution, no solid matter of Compound A-1 was visible, and Compound A-1 was in a dispersed state. This suggests that a certain amount of phosphate ester having a dispersing effect was also contained in the solid Compound A-1, and the phosphate ester contributed to the dispersion of Compound A-1 in the toluene solvent.
[0547] After that, the d1 liquid was placed in a flask, and while being heated in an oil bath set at 60°C (manufactured by Tokyo Rika Instruments Co., Ltd., model: OSB-2100), a solvent removal treatment was performed using a rotary evaporator (manufactured by Tokyo Rika Instruments Co., Ltd., model: N-1110SF), thereby refining the d1 liquid. At this time, a vacuum pump was used to reduce the pressure in the flask from normal pressure in stages while paying attention to sudden boiling, and the pressure was reduced until it finally reached 100 hPa. After that, the operation was completed after confirming that the amount of solvent had decreased to a certain extent, thereby obtaining 11.45 g of Composition 1.
[0548] Phosphonic acid, phosphoric acid ester, and compound A-1 containing part or all of the copper component are dispersed in composition 1, and it can be confirmed that the appearance of composition 1 is transparent green.
[0549] In Table 2, for compositions having a transparent green appearance, “Appearance” is marked as ◯.
[0550] It is believed that in the above process, acetic acid is produced as a by-product along with the production of compound A-1 (particularly copper phosphonate compound) by using copper acetate monohydrate as a supply source of the copper component. However, no odor peculiar to acetic acid is felt in the obtained composition 1, suggesting that acetic acid is sufficiently removed. It is believed that this is the result of the effective functioning of the precipitation of compound A-1 caused by the action of a poor solvent such as ethanol, the purification or washing process by filtration, and the solvent removal process by distillation.
[0551] (Calculation of solid content)
[0552] 10 g (M1) of composition 1 was accurately measured and placed in an aluminum culture dish whose mass was measured in advance. The culture dish was placed on a hot plate whose surface temperature was set to 180°C. In the above state, the dish was left to stand for about 10 minutes, and it was confirmed that the liquid components in the culture dish were almost completely volatilized. The mass of the culture dish in which the dried composition 1 was placed was measured, and the mass m1 obtained by subtracting the mass of the culture dish from the measured mass was measured, and m1 / M1×100 was calculated as the solid content (mass %) of composition 1.
[0553] The solid content of the composition 1 was 80.3% by mass. When components other than the solid content m1 were considered as the solvent, the content of the solvent in the composition 1 was calculated to be 19.7% by mass.
[0554] Furthermore, when the composition 1 is set to 100 mass%, the polymer B1-1 added is 28.1 mass% based on the mass of the polymer B1-1 added and the mass of the obtained composition 1, so 52.2 mass% after deducting 19.7 mass% of the solvent and 28.1 mass% of the polymer B1-1 is calculated as compound A-1. When the compound A-1 is considered to be a copper complex compound, the compound A-1 (copper complex compound) contained in the composition 1 is calculated to be 52.2 mass%.
[0555] The ratio of the compound A-1 (copper complex compound) to the solid content of the composition 1 was 0.65, and the ratio of the compound A-1 (copper complex compound) to the polymer B1-1 was 1.86.
[0556] (Evaluation of redispersibility)
[0557] In order to confirm whether Composition 1 has redispersibility, the amount of solvent was adjusted so that the solid content of Composition 1 was 10% by mass in the same solvent (second solvent) as that used for distillation, and Composition 1 was redispersed. As a result, it was confirmed that Composition 1 after redispersion had a green, highly transparent appearance and was in a good state without opaque turbidity, that is, it was confirmed that Composition 1 had good redispersibility.
[0558] In Table 2, compositions showing high redispersibility with no turbidity and transparency were indicated as "○" when visually observed under sufficiently bright lighting.
[0559] (Measurement of Transmission Spectrum of Composition)
[0560] Composition 1 was placed in a quartz cell (manufactured by Starna Scientific, model: 20 / C / Q1, optical path length: 1 mm, optical path width: 10 mm, outer dimensions: length 3.5 mm, width 12.5 mm, height 45 mm, capacity: 0.31 mL), and a UV-visible-near-infrared spectrophotometer (manufactured by JASCO Corporation, model: V770) was used to irradiate the surface of the quartz cell with light at an incident angle of 0°, and the transmittance at each wavelength in the range of 300 nm to 1200 nm was measured.
[0561] In addition, regarding the sample for transmission spectrum measurement, the concentration of Composition 1 was adjusted by adding an appropriate amount of the same second solvent as used in preparing Composition 1 so that the transmittance at a wavelength of 800 nm was 10%±1%.
[0562] The transmission spectrum of composition 1 is shown in Figure 3 In addition, Table 3 shows parameters in a specific wavelength or wavelength region that can be grasped from the transmission spectrum.
[0563] (Production of layer (D1))
[0564] 0.1 g of a surface antifouling coating agent (manufactured by Daikin Industries, Ltd., product name: Optool DSX, active ingredient concentration: 20% by mass) was mixed with 19.9 g of a hydrofluoroether-containing liquid (manufactured by 3M, product name: Novec 7100), and stirred for 5 minutes to prepare a fluorine treatment agent (active ingredient concentration: 0.1% by mass). The fluorine treatment agent was applied to one main surface of a borosilicate glass (manufactured by SCHOTT, product name: D263T eco) having a size of 130 mm × 100 mm × 0.70 mm. Thereafter, the glass substrate was placed at room temperature for 24 hours to dry the coating of the fluorine treatment agent, and then the glass surface was gently wiped with a dust-free cloth containing Novec 7100 to remove excess fluorine treatment agent. A fluorine-treated substrate was prepared in this way.
[0565] Next, composition 1 was applied using a dispenser to form a coating film in a 50 mm × 50 mm range in the center of the main surface of the fluorine-treated substrate. The obtained coating film was fully dried under a room temperature and low humidity environment, and then calcined at 85° C. for 3 hours. Thereafter, the obtained coating film was peeled off from the substrate to prepare an optical film (D1-A1) having a thickness of 155 μm.
[0566] (Measurement of Transmission Spectrum of Layer (D1-A1))
[0567] Using an ultraviolet-visible-near-infrared spectrophotometer (manufactured by JASCO Corporation, model: V770), the main surface of the obtained layer (D1-A1) was irradiated with light at an incident angle of 0°, and the transmittance of the layer (D1-A1) at each wavelength in the range of 300 nm to 1200 nm was measured.
[0568] The transmission spectrum of layer (D1-A1) is shown in Figure 7 In addition, Table 4 shows parameters in a specific wavelength or wavelength region that can be grasped from the transmission spectrum.
[0569] [Example A2]
[0570] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound (reaction product) A-2, and 12.33 g of composition 2 having a solid content of 76.6% by mass and a solvent content of 23.4% by mass was prepared. The content of compound A-2 (copper complex compound) in composition 2 was 49.8% by mass, the content of polymer B1-2 was 26.8% by mass, the ratio of compound A-2 (copper complex compound) to the solid content of composition 2 was 0.65, and the ratio of compound A-2 (copper complex compound) to polymer B1-2 was 1.85.
[0571] The appearance and redispersibility of Composition 2 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0572] raw materials
[0573] First solvent: methanol
[0574] Copper acetate monohydrate 4.88g
[0575] Phosphonic acid: n-butylphosphonic acid 2.835 g
[0576] Phosphate ester: plysurf A208N 2.829g
[0577] Polymer (B1): Polymer B1-2 3.31 g
[0578] Second solvent: toluene
[0579] [Example A3]
[0580] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-3, and 15.22 g of composition 3 having a solid content of 75.9% by mass and a solvent content of 24.1% by mass was prepared. The content of compound A-3 (copper complex compound) in composition 3 was 41.7% by mass, the content of polymer B1-1 was 34.2% by mass, the ratio of compound A-3 (copper complex compound) to the solid content of composition 3 was 0.55, and the ratio of compound A-3 (copper complex compound) to polymer B1-1 was 1.22.
[0581] The appearance and redispersibility of Composition 3 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0582] The transmission spectrum of Composition 3 was measured under the same conditions and method as in Example A1. The transmission spectrum of Composition 3 is shown in Figure 4 Table 3 shows parameters in a specific wavelength or wavelength region that can be grasped from the transmission spectrum.
[0583] Furthermore, a layer (D1-A3) having a thickness of 182 μm was prepared using the same conditions and method as in Example A1, and the transmission spectrum of the layer (D1-A3) was measured. The transmission spectrum of the layer (D1-A3) of Example A3 is shown in Figure 8 In addition, Table 4 shows parameters in a specific wavelength or wavelength region that can be grasped from the transmission spectrum.
[0584] raw materials
[0585] First solvent: methanol
[0586] Copper acetate monohydrate 4.88g
[0587] Phosphonic acid: n-butylphosphonic acid 2.780 g
[0588] Phosphate: Plysurf A208F (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 3.086 g
[0589] Polymer (B1): Polymer B1-1 5.20g
[0590] Second solvent: toluene
[0591] [Example A4]
[0592] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-4, and 19.08 g of composition 4 having a solid content of 78.7% by mass and a solvent content of 21.3% by mass was prepared. The content of compound A-4 (copper complex compound) in composition 4 was 31.2% by mass, the content of polymer B1-2 was 47.5% by mass, the ratio of compound A-4 (copper complex compound) to the solid content of composition 4 was 0.40, and the ratio of compound A-4 (copper complex compound) to polymer B1-2 was 0.66.
[0593] The appearance and redispersibility of Composition 4 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0594] raw materials
[0595] First solvent: ethanol
[0596] Copper acetate monohydrate 4.88g
[0597] Phosphonic acid: n-butylphosphonic acid 2.886 g
[0598] Phosphate ester: plysurf A208N 2.572g
[0599] Polymer (B1): Polymer B1-2 9.06g
[0600] Second solvent: toluene
[0601] [Example A5]
[0602] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-5, and 37.88 g of composition 5 having a solid content of 80.7% by mass and a solvent content of 19.3% by mass was prepared. The content of compound A-5 (copper complex compound) in composition 5 was 16.1% by mass, the content of polymer B1-1 was 64.6% by mass, the ratio of compound A-5 (copper complex compound) to the solid content of composition 5 was 0.20, and the ratio of compound A-5 (copper complex compound) to polymer B1-1 was 0.25.
[0603] The appearance and redispersibility of Composition 5 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0604] The transmission spectrum of Composition 5 was measured under the same conditions and method as in Example A1. The transmission spectrum of Composition 5 is shown in Figure 5 In addition, Table 3 shows parameters in a specific wavelength or wavelength region that can be grasped from the transmission spectrum.
[0605] raw materials
[0606] First solvent: ethanol
[0607] Copper acetate monohydrate 4.88g
[0608] Phosphonic acid: n-butylphosphonic acid 2.835 g
[0609] Phosphate ester: plysurf A208N 2.829g
[0610] Polymer (B1): Polymer B1-1 24.47 g
[0611] Second solvent: toluene
[0612] [Example A6]
[0613] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the purification (reduced pressure distillation) conditions of the d1 liquid were changed as follows. The same conditions and methods as in Example A1 were used to obtain compound A-6, and 11.30 g of composition 6 having a solid content of 81.9% by mass and a solvent content of 18.1% by mass was prepared. The content of compound A-6 (copper complex compound) in composition 6 was 52.9% by mass, the content of polymer B1-3 was 29.0% by mass, the ratio of compound A-6 (copper complex compound) to the solid content of composition 6 was 0.65, and the ratio of compound A-6 (copper complex compound) to polymer B1-3 was 1.82.
[0614] The appearance and redispersibility of Composition 6 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0615] The transmission spectrum of Composition 6 was measured under the same conditions and method as in Example A1. The transmission spectrum of Composition 6 is shown in Figure 6 In addition, Table 3 shows parameters in a specific wavelength or wavelength region that can be grasped from the transmission spectrum.
[0616] Furthermore, a layer (D1-A6) having a thickness of 168 μm was prepared using the same conditions and method as in Example A1, and the transmission spectrum of the layer (D1-A6) was measured. The transmission spectrum of the layer (D1-A6) of Example A6 is shown in Fig. 9 In addition, Table 4 shows parameters in a specific wavelength or wavelength region that can be grasped from the transmission spectrum.
[0617] raw materials
[0618] First solvent: ethanol
[0619] Copper acetate monohydrate 4.88g
[0620] Phosphonic acid: n-butylphosphonic acid 2.886 g
[0621] Phosphate ester: plysurf A208N 2.572g
[0622] Polymer (B1): Polymer B1-3 3.28g
[0623] Second solvent: dichloromethane
[0624] Purification (reduced pressure distillation) conditions
[0625] Oil bath temperature: 30°C
[0626] Pressure in distillation container: 500hPa
[0627] [Example A7]
[0628] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the purification (reduced pressure distillation) conditions of the d1 liquid were changed as follows. The same conditions and methods as in Example A1 were used to obtain compound A-7, and 14.23 g of composition 7 having a solid content of 75.8% by mass and a solvent content of 24.2% by mass was prepared. The content of compound A-7 (copper complex compound) in composition 7 was 42.1% by mass, the content of polymer B1-1 was 33.7% by mass, the ratio of compound A-7 (copper complex compound) to the solid content of composition 7 was 0.55, and the ratio of compound A-7 (copper complex compound) to polymer B1-1 was 1.25.
[0629] The appearance and redispersibility of Composition 7 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0630] raw materials
[0631] First solvent: ethanol
[0632] Copper acetate monohydrate 4.88g
[0633] Phosphonic acid: n-butylphosphonic acid 2.886 g
[0634] Phosphate ester: plysurf A208N 2.572g
[0635] Polymer (B1): Polymer B1-1 4.80g
[0636] Second solvent: dichloromethane
[0637] Purification (reduced pressure distillation) conditions
[0638] Oil bath temperature: 30°C
[0639] Pressure in distillation container: 500hPa
[0640] [Example A8]
[0641] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and composition, and the purification (reduced pressure distillation) conditions of liquid d1 were changed as follows. The same conditions and methods as in Example A1 were used to obtain compound A-8, and 24.14 g of composition 8 having a solid content of 68.4% by mass and a solvent content of 31.6% by mass was prepared. The content of compound A-8 (copper complex compound) in composition 8 was 28.1% by mass, the content of polymer B1-2 was 40.3% by mass, the ratio of compound A-8 (copper complex compound) to the solid content of composition 8 was 0.41, and the ratio of compound A-8 (copper complex compound) to polymer B1-2 was 0.70.
[0642] The appearance and redispersibility of Composition 8 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0643] Furthermore, a layer (D1-A8) having a thickness of 126 μm was prepared using the same conditions and method as in Example A1, and the transmission spectrum of the layer (D1-A8) was measured. The transmission spectrum of the layer (D1-A8) of Example A8 is shown in Fig.10 In addition, Table 4 shows parameters in a specific wavelength or wavelength region that can be grasped from the transmission spectrum.
[0644] raw materials
[0645] First solvent: ethanol
[0646] Copper acetate monohydrate 4.88g
[0647] Phosphonic acid: n-butylphosphonic acid 3.284 g
[0648] Phosphate ester: Nikko (Nikko) DDP-2 (Nikko Chemical Co., Ltd.) 3.088g
[0649] Polymer (B1): Polymer B1-2 9.74g
[0650] Second solvent: dichloromethane
[0651] Purification (reduced pressure distillation) conditions
[0652] Oil bath temperature: 30°C
[0653] Pressure in distillation container: 500hPa
[0654] [Example A9]
[0655] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-9, and 16.50 g of composition 9 having a solid content of 56.9% by mass and a solvent content of 43.1% by mass was prepared. The content of compound A-9 (copper complex compound) in composition 9 was 36.0% by mass, the content of polymer B1-3 was 20.9% by mass, the ratio of compound A-9 (copper complex compound) to the solid content of composition 9 was 0.63, and the ratio of compound A-9 (copper complex compound) to polymer B1-3 was 1.72.
[0656] In addition, the appearance and redispersibility of Composition 9 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0657] raw materials
[0658] First solvent: ethanol
[0659] Copper acetate monohydrate 4.88g
[0660] Phosphonic acid: n-butylphosphonic acid 2.886 g
[0661] Phosphate ester: plysurf A208N 2.572g
[0662] Polymer (B1): Polymer B1-3 3.45g
[0663] Second solvent: toluene
[0664] [Example A10]
[0665] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and composition, and 26.1 mg of ultraviolet absorbing compound (U-1) was added when polymer (B1) was mixed with toluene as a second solvent to obtain a solution. The same conditions and methods as in Example A1 were used to obtain compound A-10, and 21.52 g of composition 10 having a solid content of 54.6% by mass and a solvent content of 45.4% by mass was prepared. The content of compound A-10 (copper complex compound) in composition 10 was 24.3% by mass, the content of polymer B1-3 was 30.3% by mass, the ratio of compound A-10 (copper complex compound) to the solid content of composition 10 was 0.45, the ratio of compound A-10 (copper complex compound) to polymer B1-3 was 0.80, and the ratio of ultraviolet absorbing compound (U-1) to polymer B1-3 was 4.0×10 -3 .
[0666] In addition, the appearance and redispersibility of the composition 10 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0667] raw materials
[0668] First solvent: ethanol
[0669] Copper acetate monohydrate 4.88g
[0670] Phosphonic acid: methylphosphonic acid 2.019 g
[0671] Phosphate ester: plysurf A208N 2.572g
[0672] Polymer (B1): Polymer B1-3 6.52g
[0673] Ultraviolet absorbing compound (U-1) 26.1 mg
[0674] Second solvent: toluene
[0675] [Example A11]
[0676] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-11, and 25.72 g of composition 11 having a solid content of 65.7% and a solvent content of 34.3% was prepared. The content of compound A-11 (copper complex compound) in composition 11 was 22.0% by mass, the content of polymer B1-1 was 43.7% by mass, the ratio of compound A-11 (copper complex compound) to the solid content of composition 11 was 0.33, and the ratio of compound A-11 (copper complex compound) to polymer B1-1 was 0.50.
[0677] The appearance and redispersibility of composition 11 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0678] raw materials
[0679] First solvent: ethanol
[0680] Copper acetate monohydrate 4.88g
[0681] Phosphonic acid: Ethylphosphonic acid 2.259 g
[0682] Phosphate ester: plysurf A208N 2.829g
[0683] Polymer (B1): Polymer B1-1 11.25g
[0684] Second solvent: toluene
[0685] [Example A12]
[0686] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-12, and 16.33 g of composition 12 having a solid content of 65.1% by mass and a solvent content of 34.9% by mass was prepared. The content of compound A-12 (copper complex compound) in composition 12 was 41.2% by mass, the content of polymer B1-1 was 23.9% by mass, the ratio of compound A-12 (copper complex compound) to the solid content of composition 12 was 0.63, and the ratio of compound A-12 (copper complex compound) to polymer B1-1 was 1.72.
[0687] In addition, the appearance and redispersibility of Composition 12 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0688] raw materials
[0689] First solvent: ethanol
[0690] Copper acetate monohydrate 4.88g
[0691] Phosphonic acid: n-butylphosphonic acid 3.284 g
[0692] Phosphate ester: NIKKOL DDP-2 3.088g
[0693] Polymer (B1): Polymer B1-1 3.91 g
[0694] Second solvent: toluene
[0695] [Example A13]
[0696] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-13, and 16.75 g of composition 13 having a solid content of 62.8% by mass and a solvent content of 37.2% by mass was prepared. The content of compound A-13 (copper complex compound) in composition 13 was 39.6% by mass, the content of polymer B1-2 was 23.2% by mass, the ratio of compound A-13 (copper complex compound) to the solid content of composition 13 was 0.63, and the ratio of compound A-13 (copper complex compound) to polymer B1-2 was 1.71.
[0697] The appearance and redispersibility of Composition 13 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0698] raw materials
[0699] First solvent: methanol
[0700] Copper acetate monohydrate 4.88g
[0701] Phosphonic acid: n-butylphosphonic acid 3.334 g
[0702] Phosphate: NIKKOL DDP-2 2.984g
[0703] Polymer (B1): Polymer B1-2 3.88g
[0704] Second solvent: toluene
[0705] [Example A14]
[0706] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and composition, and 36.1 mg of ultraviolet absorbing compound (U-1) was added when polymer (B1) was mixed with toluene as a second solvent to obtain a solution. The same conditions and methods as in Example A1 were used to obtain compound A-14, and 24.93 g of composition 14 having a solid content of 62.1% by mass and a solvent content of 37.9% by mass was prepared. The content of compound A-14 (copper complex compound) in composition 14 was 25.9% by mass, the content of polymer B1-4 was 36.2% by mass, the ratio of compound A-14 (copper complex compound) to the solid content of composition 14 was 0.42, the ratio of compound A-14 (copper complex compound) to polymer B1-4 was 0.71, and the ratio of ultraviolet absorbing compound (U-1) to polymer B1-4 was 4.0×10 -3 .
[0707] The appearance and redispersibility of Composition 14 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0708] raw materials
[0709] First solvent: ethanol
[0710] Copper acetate monohydrate 4.88g
[0711] Phosphonic acid: n-hexylphosphonic acid 3.472 g
[0712] Phosphate ester: plysurf A208N 2.572g
[0713] Polymer (B1): Polymer B1-4 9.03g
[0714] Ultraviolet absorbing compound (U-1) 36.1 mg
[0715] Second solvent: toluene
[0716] [Example A15]
[0717] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-15, and 30.02 g of composition 15 having a solid content of 35.0% by mass and a solvent content of 65.0% by mass was prepared. The content of compound A-15 (copper complex compound) in composition 15 was 19.3% by mass, the content of polymer B1-3 was 15.7% by mass, the ratio of compound A-15 (copper complex compound) to the solid content of composition 15 was 0.55, and the ratio of compound A-15 (copper complex compound) to polymer B1-3 was 1.23.
[0718] The appearance and redispersibility of Composition 15 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0719] raw materials
[0720] First solvent: ethanol
[0721] Copper acetate monohydrate 4.88g
[0722] Phosphonic acid: n-butylphosphonic acid 2.943 g
[0723] Phosphate ester: plysurf A208N 2.315g
[0724] Polymer (B1): Polymer B1-3 4.71 g
[0725] Second solvent: toluene
[0726] [Example A16]
[0727] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-16, and 70.25 g of composition 16 having a solid content of 40.3% by mass and a solvent content of 59.7% by mass was prepared. The content of compound A-16 (copper complex compound) in composition 16 was 8.2% by mass, the content of polymer B1-1 was 32.1% by mass, the ratio of compound A-16 (copper complex compound) to the solid content of composition 16 was 0.20, and the ratio of compound A-16 (copper complex compound) to polymer B1-1 was 0.26.
[0728] In addition, the appearance and redispersibility of Composition 16 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0729] raw materials
[0730] First solvent: ethanol
[0731] Copper acetate monohydrate 4.88g
[0732] Phosphonic acid: n-butylphosphonic acid 2.943 g
[0733] Phosphate ester: plysurf A208N 2.315g
[0734] Polymer (B1): Polymer B1-1 22.53g
[0735] Second solvent: toluene
[0736] [Example A17]
[0737] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-17, and 44.81 g of composition 17 having a solid content of 20.6% by mass and a solvent content of 79.4% by mass was prepared. The content of compound A-17 (copper complex compound) in composition 17 was 13.3% by mass, the content of polymer B1-2 was 7.3% by mass, the ratio of compound A-17 (copper complex compound) to the solid content of composition 17 was 0.64, and the ratio of compound A-17 (copper complex compound) to polymer B1-2 was 1.81.
[0738] In addition, the appearance and redispersibility of Composition 17 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0739] raw materials
[0740] First solvent: ethanol
[0741] Copper acetate monohydrate 4.88g
[0742] Phosphonic acid: n-butylphosphonic acid 2.886 g
[0743] Phosphate ester: plysurf A208N 2.572g
[0744] Polymer (B1): Polymer B1-2 3.28g
[0745] Second solvent: toluene
[0746] [Example A18]
[0747] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-18, and 63.57 g of composition 18 having a solid content of 17.8% by mass and a solvent content of 82.2% by mass was prepared. The content of compound A-18 (copper complex compound) in composition 18 was 9.5% by mass, the content of polymer B1-3 was 8.3% by mass, the ratio of compound A-18 (copper complex compound) to the solid content of composition 18 was 0.53, and the ratio of compound A-18 (copper complex compound) to polymer B1-3 was 1.14.
[0748] The appearance and redispersibility of Composition 18 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0749] raw materials
[0750] First solvent: ethanol
[0751] Copper acetate monohydrate 4.88g
[0752] Phosphonic acid: n-butylphosphonic acid 2.886 g
[0753] Phosphate ester: plysurf A208N 2.572g
[0754] Polymer (B1): Polymer B1-3 5.29g
[0755] Second solvent: toluene
[0756] [Example A19]
[0757] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-19, and 23.88 g of composition 19 having a solid content of 70.6% by mass and a solvent content of 29.4% by mass was prepared. The content of compound A-19 (copper complex compound) in composition 19 was 24.0% by mass, the total content of polymer B1-1 and polymer B1-2 was 46.6% by mass, the ratio of compound A-19 (copper complex compound) to the solid content of composition 19 was 0.34, and the ratio of compound A-19 (copper complex compound) to the total of polymer B1-1 and polymer B1-2 was 0.51.
[0758] The appearance and redispersibility of Composition 19 were evaluated under the same conditions and methods as in Example A1, and the results were both good.
[0759] raw materials
[0760] First solvent: ethanol
[0761] Copper acetate monohydrate 4.88g
[0762] Phosphonic acid: Ethylphosphonic acid 2.259 g
[0763] Phosphate ester: plysurf A208N 2.829g
[0764] Polymer (B1): 11.14 g of a mixture of 50% by mass of polymer B1-1 and polymer B1-2
[0765] Second solvent: toluene
[0766] [Example A20]
[0767] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and the same conditions and methods as in Example A1 were used to obtain compound A-20, and 12.31 g of composition 20 having a solid content of 64.2% by mass and a solvent content of 35.8% by mass was prepared. The content of compound A-20 (copper complex compound) in composition 20 was 48.3% by mass, the content of polymer B1-2 was 15.9% by mass, the ratio of compound A-20 (copper complex compound) to the solid content of composition 20 was 0.75, and the ratio of compound A-20 (copper complex compound) to polymer B1-2 was 3.03.
[0768] In addition, the appearance and redispersibility of Composition 20 were evaluated under the same conditions and method as in Example A1.
[0769] Composition 20 was a green transparent liquid in which no aggregation or the like was observed, and the appearance evaluation was judged to be without problems (evaluation: ○). However, during the redispersion of composition 20, slight aggregation of the components constituting the composition 20 was observed in the liquid, which is permissible depending on the application or specification, but the redispersion property was judged to be slightly inferior compared to compositions 1 to 19, and was marked as △ in Table 2.
[0770] raw materials
[0771] First solvent: ethanol
[0772] Copper acetate monohydrate 4.88g
[0773] Phosphonic acid: n-butylphosphonic acid 2.886 g
[0774] Phosphate ester: plysurf A208N 2.572g
[0775] Polymer (B1): Polymer B1-2 1.96g
[0776] Second solvent: toluene
[0777] [Comparative Example a1]
[0778] In Example A1, the following raw materials were used as raw materials for compound A-1 (reaction product) and the composition, and polymer (B1) was not added. The same conditions and methods as in Example A1 were used to obtain compound A-21, and 10.31 g of composition 21 having a solid content of 57.7% by mass and a solvent content of 42.3% by mass was prepared. The content of compound A-21 (copper complex compound) in composition 21 was 57.7% by mass, and the ratio of compound A-21 (copper complex compound) to the solid content of composition 21 was 1.
[0779] In addition, the appearance and redispersibility of Composition 21 were evaluated under the same conditions and method as in Example A1.
[0780] Composition 21 was a green transparent liquid in which no aggregation or the like was observed, and the appearance evaluation was judged to be without problems (evaluation: ○). However, during the redispersion of composition 21, aggregation of the components constituting the composition 21 in the liquid was observed, and the result was not considered to be good redispersion, which was marked as × in Table 2. This suggests that if polymer (B1) is not used, aggregation occurs during redispersion, and a suitable composition cannot be obtained.
[0781] raw materials
[0782] First solvent: ethanol
[0783] Copper acetate monohydrate 4.88g
[0784] Phosphonic acid: n-butylphosphonic acid 2.886 g
[0785] Phosphate ester: plysurf A208N 2.572g
[0786] Polymer(B1): None
[0787] Second solvent: toluene
[0788] [Table 2]
[0789]
[0790] The abbreviations in Table 2 represent the following compounds, respectively.
[0791] CAM: Cupric acetate monohydrate
[0792] BPA: n-butylphosphonic acid
[0793] MPA: Methylphosphonic acid
[0794] EPA: Ethylphosphonic acid
[0795] HPA: n-hexylphosphonic acid
[0796] Ultraviolet absorbing compound (U-1): a compound represented by the following formula (U-1) (absorption maximum wavelength in dichloromethane is 364 nm)
[0797] [Chemistry 9]
[0798]
[0799] [Table 3]
[0800]
[0801] [Table 4]
[0802]
[0803] <Example D1-1>
[0804] As shown in Table 5, 100 parts by mass of polymer B1-1, 50 parts by mass of compound A-11 obtained in Example A11, and dichloromethane as a solvent were added and mixed to prepare a solution having a solid content concentration of 20% by mass (composition D1-1 for forming layer (D1)).
[0805] <Example D1-2 to Example D1-5, and Comparative Example D1-6 to Comparative Example D1-9>
[0806] In Example D1-1, the types and amounts of polymer (B1), polymer (B2-1), compound A, and ultraviolet absorbing compound (U-1) as other compounds are changed as shown in Table 5, and compositions D1-2 to D1-9 for forming layer (D1) are prepared in the same manner as in Example D1-1.
[0807] [Table 5]
[0808]
[0809] <Preparation Example D2-1>
[0810] As shown in Table 6, 100 parts by mass of polymer B2-1-1, 0.07 parts by mass of near-infrared absorbing pigment C-1, 0.07 parts by mass of near-infrared absorbing pigment C-2, and dichloromethane as a solvent were added and mixed to prepare a solution having a solid content concentration of 20% by mass (composition D2-1 for forming layer (D2)).
[0811] <Preparation Example D2-2 and Preparation Example D2-3>
[0812] In Preparation Example D2-1, except that the addition amounts of the polymer (B2-1) and the near-infrared absorbing pigment were changed as shown in Table 6, a composition D2-2 for forming a layer (D2) and a composition D2-3 for forming a layer (D2) were prepared in the same manner as Preparation Example D2-1.
[0813] [Table 6]
[0814]
[0815] The near infrared absorbing dye C-1 in Table 6 is a compound represented by the following formula (C-1) (the absorption maximum wavelength in dichloromethane is 711 nm).
[0816] [Chemistry 10]
[0817]
[0818] The near infrared absorbing dye C-2 in Table 6 is a compound represented by the following formula (C-2) (the absorption maximum wavelength in dichloromethane is 738 nm).
[0819] [Chemistry 11]
[0820]
[0821] The near infrared absorbing dye C-3 in Table 6 is a compound represented by the following formula (C-3) (the absorption maximum wavelength in dichloromethane is 715 nm).
[0822] [Chemistry 12]
[0823]
[0824] The near infrared absorbing dye C-4 in Table 6 is a compound represented by the following formula (C-4) (the absorption maximum wavelength in dichloromethane is 776 nm).
[0825] [Chemistry 13]
[0826]
[0827] <Preparation Example D2-4>
[0828] 100 parts by mass of polymer B2-2-1, 0.70 parts by mass of the near-infrared absorbing pigment C-1, 0.70 parts by mass of the near-infrared absorbing pigment C-2, 0.40 parts by mass of KF-643 manufactured by Shin-Etsu Chemical Co., Ltd. as a surfactant, 1.8 parts by mass of γ-glycidyloxypropyltrimethoxysilane as an adhesion promoter, and cyclopentanone and dichloromethane as solvents were added and mixed to prepare a solution having a solid content concentration of 22% (composition D2-4 for forming layer (D2)).
[0829] <Preparation Example D2-5>
[0830] 100 parts by mass of tricyclodecane dimethanol diacrylate, 5 parts by mass of 1-hydroxycyclohexyl phenyl ketone, 1.40 parts by mass of the near-infrared absorbing pigment C-1, 1.40 parts by mass of the near-infrared absorbing pigment C-2, 0.20 parts by mass of KF-643 manufactured by Shin-Etsu Chemical Co., Ltd. as a surfactant, and methyl ethyl ketone as a solvent were added and mixed to prepare a solution having a solid content concentration of 35% by mass (composition D2-5 for forming layer (D2)).
[0831] <Preparation Example E1>
[0832] 100 parts by mass of tricyclodecane dimethanol diacrylate, 5 parts by mass of 1-hydroxycyclohexyl phenyl ketone, 0.20 parts by mass of KF-643 manufactured by Shin-Etsu Chemical Co., Ltd. as a surfactant, and methyl ethyl ketone as a solvent were added and mixed to prepare a solution having a solid content concentration of 35% by mass (Composition E1).
[0833] [Example P1]
[0834] The composition D1-1 for forming layer (D1) was cast on a smooth glass plate, dried at 20°C for 8 hours, and then peeled from the glass plate. The peeled coating film was further dried at 120°C for 8 hours under reduced pressure to prepare a layer D1-1 having a thickness of 0.10 mm, a length of 60 mm, and a width of 60 mm as layer (D1).
[0835] The composition D2-1 for forming layer (D2) was cast on a smooth glass plate, dried at 20°C for 8 hours, and then peeled from the glass plate. The peeled coating film was further dried at 100°C for 8 hours under reduced pressure to prepare a layer D2-1 having a thickness of 0.10 mm, a length of 60 mm, and a width of 60 mm as layer (D2).
[0836] After methyl-n-amyl ketone was coated on layer D1-1 using a rod coater in such a manner that the liquid film thickness became 2.0 μm, layer D2-1 was bonded to the surface coated with methyl-n-amyl ketone using a laminator (manufactured by Youbon Co., Ltd., product name; Lamiman IKO-650E) to produce a substrate EX1-Sub with a thickness of 0.2 mm.
[0837] Composition E1 was applied on one of the main surfaces of substrate EX1-Sub using a bar coater and heated in an oven at 70° C. for 2 minutes to volatilize and remove the solvent. At this time, the coating conditions of the bar coater were adjusted so that the thickness after drying was 2 μm.
[0838] Next, the exposure was performed using a conveyor type exposure machine (exposure amount 500 mJ / cm 2 , 200mW), the composition E1 was cured to form an outer coating on the substrate EX1-Sub. Similarly, an outer coating comprising the composition E1 was formed on the other main surface of the substrate EX1-Sub to obtain a substrate EX1-Stack. The spectral transmittance of the substrate was measured using a product name: "V-7300" manufactured by JASCO Corporation. The obtained transmission spectrum is shown in Fig.11 .
[0839] Next, a dielectric multilayer film (I) is formed on one of the main surfaces of the obtained substrate EX1-Stack (formed on the outer coating layer on layer (D2)), and then a dielectric multilayer film (II) is formed on the other main surface of the substrate (formed on the outer coating layer on layer (D1)) to produce an optical filter with a thickness of approximately 0.209 mm.
[0840] The dielectric multilayer film (I) is formed by alternately stacking silicon dioxide (SiO2) layers and titanium dioxide (TiO2) layers at a vapor deposition temperature of 100°C (a total of 26 layers). The dielectric multilayer film (II) is formed by alternately stacking silicon dioxide (SiO2) layers and titanium dioxide (TiO2) layers at a vapor deposition temperature of 100°C (a total of 20 layers). In either the dielectric multilayer film (I) or the dielectric multilayer film (II), the silicon dioxide layer and the titanium dioxide layer are alternately stacked in the order of titanium dioxide layer, silicon dioxide layer, titanium dioxide layer, ... silicon dioxide layer, titanium dioxide layer, silicon dioxide layer from the substrate side, and the outermost layer of the optical filter is set to be a silicon dioxide layer.
[0841] The dielectric multilayer film (I) and the dielectric multilayer film (II) are designed as follows.
[0842] The thickness and number of each layer were optimized using optical thin film design software (Essential Macleod, manufactured by Thin Film Center) in order to achieve the antireflection effect in the visible light region and the desired cutoff performance in the near infrared region, in combination with the wavelength dependence of the refractive index of the substrate. When optimizing, the input parameters (target values) to the software were set as shown in Table 7 below in this Example P1.
[0843] [Table 7]
[0844]
[0845] The result of the film structure optimization is that in Example P1, the dielectric multilayer film (I) is a multilayer vapor-deposited film with 26 layers stacked alternately by stacking silicon dioxide layers with a physical film thickness of about 31nm to 157nm and titanium dioxide layers with a physical film thickness of about 10nm to 95nm.
[0846] The dielectric multilayer film (II) is a multilayer vapor-deposited film having 20 layers stacked alternately, in which silicon dioxide layers having a physical film thickness of approximately 37 nm to 194 nm and titanium dioxide layers having a physical film thickness of approximately 12 nm to 114 nm are stacked.
[0847] Table 8 shows an example of the optimized membrane structure.
[0848] [Table 8]
[0849]
[0850] *λ=550nm
[0851] <Optical properties>
[0852] The transmittance of light incident from the vertical direction of the main surface of the obtained optical filter was measured using a product name: "V-7300" manufactured by JASCO Corporation, and the average transmittance at a wavelength of 450nm to 580nm and the average transmittance at a wavelength of 800nm to 1000nm were calculated. The results are shown in Table 11, and the obtained transmission spectra are shown in Fig.15 .
[0853] Durability
[0854] The optical filter cut into 3 cm squares was placed in a constant temperature and humidity oven (Espec (co., Ltd., manufactured by: SH-222) set at 85°C / 85%RH and left to stand for 1000 hours. The spectral characteristics of each wavelength region after 1000 hours were measured using "V-7300" to calculate the average transmittance at wavelengths of 450nm to 580nm and the average transmittance at wavelengths of 800nm to 1000nm. The results are shown in Table 11.
[0855] The durability of the optical filter can be evaluated based on the difference in the values of the average transmittances before and after being placed in a constant temperature and humidity oven.
[0856] [Example P2]
[0857] In Example P1, layer (D1) forming composition D1-2 was used instead of layer (D1) forming composition D1-1 to prepare layer D1-2, and layer (D2) forming composition D2-2 was used instead of layer (D2) forming composition D2-1 to prepare layer D2-2 with a thickness of 0.05 mm.
[0858] A substrate EX2-Stack and an optical filter were produced in the same manner as in Example P1 except that the produced layer D1-2 and layer D2-2 were used.
[0859] The spectral transmittance of the prepared substrate was measured in the same manner as in Example P1. The obtained transmission spectrum is shown in Fig.12 .
[0860] In addition, the optical properties and durability of the prepared optical filter were evaluated in the same manner as in Example P1. The results are shown in Table 11, and the transmission spectra obtained are shown in Fig.16 .
[0861] [Example P3]
[0862] In Example P1, a substrate EX3-Stack and an optical filter were prepared in the same manner as in Example P1, except that the layer D2-3 was prepared using the layer (D2)-forming composition D2-3 instead of the layer (D2)-forming composition D2-1.
[0863] The spectral transmittance of the prepared substrate was measured in the same manner as in Example P1. The obtained transmission spectrum is shown in Fig.13 .
[0864] In addition, the optical properties and durability of the prepared optical filter were evaluated in the same manner as in Example P1. The results are shown in Table 11, and the transmission spectra obtained are shown in Fig.17 .
[0865] [Example P4]
[0866] In Example P1, the composition D1-3 for forming a layer (D1) was used instead of the composition D1-1 for forming a layer (D1) to prepare a layer D1-4 having a thickness of 0.20 mm.
[0867] The composition D2-4 for forming the layer (D2) was applied to one of the main surfaces of the layer D1-4 using a bar coater, and heated in an oven at 70°C for 3 minutes to volatilize and remove the solvent, thereby forming the layer D2-4. At this time, the coating conditions of the bar coater were adjusted so that the thickness after drying was 10 μm. Then, the layer D2-4 was cured by heating in an oven at 150°C for 20 minutes to obtain a substrate EX4-Stack.
[0868] The spectral transmittance of the prepared substrate was measured in the same manner as in Example P1. The obtained transmission spectrum is shown in Fig.14 .
[0869] Then, similarly to Example P1, a dielectric multilayer film (I) is formed on the surface of the substrate EX4-Stack on which the hardened layer D2-4 is formed, and a dielectric multilayer film (II) is formed on the other main surface of the substrate EX4-Stack, thereby producing an optical filter with a thickness of approximately 0.215 mm.
[0870] The optical filter thus produced was used to evaluate the optical properties and durability in the same manner as in Example P1. The results are shown in Table 11, and the transmission spectra obtained are shown in Fig.18 .
[0871] [Example P5]
[0872] In Example P4, instead of using the layer (D1) forming composition D1-3 to produce the layer D1-4 with a thickness of 0.20 mm, the layer (D1) forming composition D1-3 was used to produce the layer D1-5 with a thickness of 0.10 mm. The substrate EX5-Stack was produced in the same manner as in Example P4.
[0873] Next, a dielectric multilayer film (III) is formed on the surface of the obtained substrate EX5-Stack on which the hardened layer D2-4 is formed, and a dielectric multilayer film (IV) is further formed on the other main surface of the substrate, thereby producing an optical filter with a thickness of approximately 0.114 mm.
[0874] The dielectric multilayer film (III) is formed by alternately stacking silicon dioxide (SiO2) layers and titanium dioxide (TiO2) layers at a vapor deposition temperature of 100°C (a total of 38 layers). The dielectric multilayer film (IV) is formed by alternately stacking silicon dioxide (SiO2) layers and titanium dioxide (TiO2) layers at a vapor deposition temperature of 100°C (a total of 8 layers). In either the dielectric multilayer film (III) or the dielectric multilayer film (IV), the silicon dioxide layer and the titanium dioxide layer are alternately stacked in the order of titanium dioxide layer, silicon dioxide layer, titanium dioxide layer, ... silicon dioxide layer, titanium dioxide layer, silicon dioxide layer from the substrate side, and the outermost layer of the optical filter is set to be a silicon dioxide layer.
[0875] The design of the dielectric multilayer film (III) and the dielectric multilayer film (IV) was carried out in the same manner as in Example P1 except that the input parameters for optimization were as shown in Table 9 below.
[0876] [Table 9]
[0877]
[0878] The result of the film structure optimization is that in Example P5, the dielectric multilayer film (III) is a multilayer vapor-deposited film with 38 layers stacked alternately by stacking silicon dioxide layers with a physical film thickness of about 27nm to 174nm and titanium dioxide layers with a physical film thickness of about 10nm to 101nm.
[0879] The dielectric multilayer film (IV) is a multilayer vapor-deposited film having eight layers stacked alternately, in which silicon dioxide layers having a physical film thickness of approximately 12 nm to 107 nm and titanium dioxide layers having a physical film thickness of approximately 12 nm to 78 nm are stacked.
[0880] Table 10 shows an example of the optimized membrane structure.
[0881] [Table 10]
[0882]
[0883]
[0884] The optical filter thus produced was used to evaluate the optical properties and durability in the same manner as in Example P1. The results are shown in Table 11, and the transmission spectra obtained are shown in Fig.19 .
[0885] [Example P6]
[0886] The composition D1-4 for forming the layer (D1) was cast on a smooth glass plate, dried at 20°C for 8 hours, and then peeled from the glass plate. The peeled coating film was then dried at 120°C for 8 hours under reduced pressure to prepare a layer D1-6A having a thickness of 0.10 mm, a length of 60 mm, and a width of 60 mm. Furthermore, a layer D1-6B having a thickness of 0.10 mm, a length of 60 mm, and a width of 60 mm was prepared by the same procedure.
[0887] After methyl-n-amyl ketone was applied on layer D1-6A using a rod coater in such a manner that the liquid film thickness became 2.0 μm, layer D1-6B was laminated on the surface coated with methyl-n-amyl ketone using a laminator (manufactured by Youbon Co., Ltd., product name: Lamiman IKO-650E) to produce layer D1-6 as layer (D1).
[0888] Next, in the same manner as in Example P4, layer D2-4 was formed on one of the main surfaces of layer D1-6 and cured, thereby obtaining a base material EX6-Stack.
[0889] Similar to Example P1, a dielectric multilayer film (I) is formed on the surface of the substrate EX6-Stack on which the hardened layer D2-4 is formed, and a dielectric multilayer film (II) is formed on the other main surface of the substrate EX6-Stack, thereby producing an optical filter.
[0890] Using the produced optical filter, the optical characteristics and durability were evaluated in the same manner as in Example P1. The results are shown in Table 11.
[0891] [Example P7]
[0892] In Example P4, a layer D1-7 having a thickness of 0.20 mm was prepared in the same manner as in Example P4 except that the layer (D1) forming composition D1-5 was used instead of the layer (D1) forming composition D1-3.
[0893] The layer (D2) forming composition D2-5 was applied onto one of the main surfaces of the layer D1-7 using a bar coater, and heated in an oven at 70° C. for 2 minutes to volatilize and remove the solvent, thereby forming the layer D2-7. At this time, the coating conditions of the bar coater were adjusted so that the thickness after drying was 5 μm.
[0894] Next, the exposure was performed using a conveyor type exposure machine (exposure amount 500 mJ / cm 2 , 200mW), to harden layer D2-7 and obtain substrate EX7-Stack.
[0895] Similar to Example P1, a dielectric multilayer film (I) is formed on the surface of the substrate EX7-Stack on which the hardened layer D2-7 is formed, and a dielectric multilayer film (II) is formed on the other main surface of the substrate EX7-Stack, thereby producing an optical filter.
[0896] Using the produced optical filter, the optical characteristics and durability were evaluated in the same manner as in Example P1. The results are shown in Table 11.
[0897] [Example P8]
[0898] The composition D1-1 for forming the layer (D1) was cast on a smooth glass plate, dried at 20°C for 8 hours, and then peeled from the glass plate. The peeled coating film was then dried at 120°C for 8 hours under reduced pressure to prepare a layer D1-8A having a thickness of 0.07 mm, a length of 60 mm, and a width of 60 mm. Furthermore, a layer D1-8B having a thickness of 0.07 mm, a length of 60 mm, and a width of 60 mm was prepared by the same procedure.
[0899] After methyl-n-amyl ketone was applied on layer D1-8A using a rod coater in such a manner that the liquid film thickness became 2.0 μm, layer D1-8B was laminated on the surface coated with methyl-n-amyl ketone using a laminator (manufactured by Youbon Co., Ltd., product name: Lamiman IKO-650E) to produce layer D1-8 with a thickness of 0.14 mm as layer (D1).
[0900] The composition D2-2 for forming the layer (D2) was cast on a smooth glass plate, dried at 20°C for 8 hours, and then peeled from the glass plate. The peeled coating film was further dried at 100°C for 8 hours under reduced pressure to prepare a layer D2-8 having a thickness of 0.03 mm, a length of 60 mm, and a width of 60 mm as the layer (D2).
[0901] 100 parts by weight of polymer B2-1-1 and dichloromethane as a solvent were added and mixed to prepare a solution having a solid content concentration of 20% by weight. The solution was cast on a smooth glass plate, dried at 20°C for 8 hours, and then peeled off from the glass plate. The peeled coating was then dried at 100°C for 8 hours under reduced pressure to prepare a film F-1 having a thickness of 0.03 mm, a length of 60 mm, and a width of 60 mm.
[0902] After methyl-n-amyl ketone was applied to one of the main surfaces of layer D1-8 using a bar coater so that the liquid film thickness was 2.0 μm, layer D2-8 was bonded to the surface coated with methyl-n-amyl ketone using a laminator (manufactured by Youbon Co., Ltd., product name: Lamiman IKO-650E). Subsequently, film F-1 was bonded to the other main surface of layer D1-8 in the same manner to prepare a substrate EX8-Sub having a thickness of 0.20 mm.
[0903] Next, an overcoat layer was formed on both surfaces of the obtained substrate EX8-Sub in the same manner as in Example P1, thereby obtaining a substrate EX8-Stack.
[0904] Using the prepared substrate EX8-Stack, an optical filter was prepared in the same manner as in Example P1. At this time, a dielectric multilayer film (I) was formed on one of the main surfaces of the obtained substrate EX8-Stack (on the outer coating formed on the layer D2-8), and a dielectric multilayer film (II) was formed on the other main surface of the substrate (on the outer coating formed on the film F-1).
[0905] Using the produced optical filter, the optical characteristics and durability were evaluated in the same manner as in Example P1. The results are shown in Table 11.
[0906] [Comparative Example P1]
[0907] In Example P3, layer D1-9 was prepared by using composition D1-6 for forming layer (D1) instead of composition D1-1 for forming layer (D1).
[0908] A substrate EX9-Stack and an optical filter were produced in the same manner as in Example P3 except that the produced layer D1-9 was used.
[0909] The spectral transmittance of the produced substrate was measured in the same manner as in Example P3.
[0910] Furthermore, using the produced optical filter, the optical characteristics and durability were evaluated in the same manner as in Example P3. The results are shown in Table 11.
[0911] [Comparative Example P2]
[0912] In Example P3, layer (D1)-forming composition D1-7 was used instead of layer (D1)-forming composition D1-1 to produce layer D1-10.
[0913] A substrate EX10-Stack and an optical filter were produced in the same manner as in Example P3 except that the produced layer D1-10 was used.
[0914] The spectral transmittance of the produced substrate was measured in the same manner as in Example P3.
[0915] Furthermore, using the produced optical filter, the optical characteristics and durability were evaluated in the same manner as in Example P3. The results are shown in Table 11.
[0916] [Comparative Example P3]
[0917] In Example P3, layer D1-11 was prepared by using composition D1-8 for forming layer (D1) instead of composition D1-1 for forming layer (D1).
[0918] A substrate EX11-Stack and an optical filter were produced in the same manner as in Example P3 except that the produced layer D1-11 was used.
[0919] The spectral transmittance of the produced substrate was measured in the same manner as in Example P3.
[0920] Furthermore, using the produced optical filter, the optical characteristics and durability were evaluated in the same manner as in Example P3. The results are shown in Table 11.
[0921] [Comparative Example P4]
[0922] In Example P3, layer D1-12 was prepared by using composition D1-9 for forming layer (D1) instead of composition D1-1 for forming layer (D1).
[0923] A substrate EX12-Stack and an optical filter were produced in the same manner as in Example P3 except that the produced layer D1-12 was used.
[0924] The spectral transmittance of the produced substrate was measured in the same manner as in Example P3.
[0925] Furthermore, using the produced optical filter, the optical characteristics and durability were evaluated in the same manner as in Example P3. The results are shown in Table 11.
[0926] [Table 11]
[0927]
Claims
1. A composition (D) comprising: a light-absorbing compound (A) containing a phosphonic acid component and a copper component, and a polymer (B1) containing a polyarylate.
2. The composition (D) according to claim 1, further comprising an ultraviolet absorbing compound (U). 3 . The composition (D) according to claim 1 , further comprising a pigment (C) other than the compound (A).
4. The composition (D) according to claim 1, wherein the transmission spectrum of the composition (D) satisfies the following requirements (i) to (iv), wherein the transmission spectrum of the composition (D) is adjusted to have a transmittance of 10%±1% at a wavelength of 800 nm, (i) The average transmittance in the wavelength range of 800 nm to 1100 nm is 10% or less (ii) The average transmittance in the wavelength range of 460 nm to 580 nm is 80% or more (iii) A first cutoff wavelength having a transmittance of 50% in the wavelength range of 680 nm to 780 nm (iv) It has a second cutoff wavelength with a transmittance of 50% within the wavelength range of 320 nm to 380 nm.
5. The composition (D) according to claim 4, wherein the transmission spectrum further satisfies the following requirement (v), (v) The standard deviation of the transmittance in the wavelength range of 900 nm to 1100 nm is 0.5% or less.
6. An optical film formed from the composition (D) according to claim 1.
7. A layer (D1) formed from the composition (D) according to claim 1, wherein the transmission spectrum satisfies the following requirements (I) to (V), (I) The average transmittance in the wavelength range of 460nm to 580nm is 80% or more (II) The average transmittance in the wavelength range of 800 nm to 1100 nm is 5% or less (III) A third cutoff wavelength having a transmittance of 50% in the wavelength range of 680 nm to 730 nm (IV) A fourth cutoff wavelength having a transmittance of 50% in the wavelength range of 340 nm to 400 nm (V) The maximum value of the transmittance at a wavelength of 950 nm is 1% or less. 8 . An optical filter comprising a layer ( D1 ) formed from the composition (D) according to claim 1 .
9. An optical filter comprising: A layer (D1) formed from the composition (D) according to claim 1; and The layer (D2) is formed by a composition (D2) containing a pigment (C) other than the compound (A), and at least one selected from a polymer (B2-1) and a curable compound (B2-2) that is cured by light or heat.
10. The optical filter according to claim 8, comprising a dielectric multilayer film.
11. An optical element comprising the optical filter according to any one of claims 8 to 10. 12 . A solid-state imaging device comprising the optical filter according to claim 8 .
13. A camera module comprising the optical filter according to any one of claims 8 to 10.
14. A composition (D), wherein The composition (D) contains: a light absorbing compound (A) containing a phosphonic acid component and a copper component, and a polymer (B1) containing a polyarylate. The solid content of the composition (D) is 15% to 85% by mass. The content of the polymer (B1) in the composition (D) is 5% to 70% by mass. The content of the polymer (B1) is 0.5 to 6 parts by mass based on 1 part by mass of the compound (A).
Citation Information
Patent Citations
Process for production of composite panel
JP1978055330A
Preparation of heat-resistant resin
JP1982049621A
Fuzzy inference control method
JP1993040505A
Optical compensation element, manufacturing method thereof, liquid crystal display device and liquid crystal projector
JP2007072163A
Near infrared ray cut filter and device comprising the same
JP2011100084A