High-temperature-resistant fireproof facing coating

By using a combination coating of organic adhesive, lightweight thermal insulation filler and refractory fiber on the steel structure, the existing fire-resistant coatings have been solved and the problem of insufficient smoke generation and decorative properties are insufficient at high temperatures, achieving efficient thermal insulation and good decorative properties and high-durability high-temperature and fire-resistant effects.

CN118931290APending Publication Date: 2024-11-12SICHUAN FIRE RES INST OF MEM
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410988133.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing fire-resistant coatings are prone to smoke in high-temperature environments, the expansion layer is susceptible to mechanical damage, and lacks decorative and durability, making it difficult to meet the high-temperature fire-proof performance requirements of steel structures.

Method used

Using a combination of organic adhesives, light heat-insulating fillers, refractory fibers, refractory fillers and additives, high-temperature fire-resistant finish coatings, including acrylic emulsions, expanded perlites, aluminum silicate fibers and alumina, The components are equally composed of a homogeneous mixture by stirring and filtration.

Benefits of technology

It achieves effective heat insulation in high temperature environments, maintains good decorative effect and high durability, avoids smoke release, ensures environmental safety, and improves the fire resistance and service life of the steel structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931290A_ABST
    Figure CN118931290A_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant fireproof facing coating which comprises an organic adhesive, a light heat insulation filler, refractory fibers, a refractory filler and an auxiliary agent. The concrete proportion is as follows: 33 parts of the organic adhesive, 38 parts of the light heat insulation filler, 16 parts of the refractory fiber, 8 parts of the refractory filler and 5 parts of the assistant. The organic adhesive comprises an acrylic emulsion and a silicone acrylic emulsion, the light heat insulation filler comprises expanded perlite, expanded vermiculite and hollow glass beads, the refractory fibers comprise aluminum silicate fibers and basalt fibers, the refractory filler comprises aluminum oxide, silica powder and titanium dioxide, and the auxiliaries comprise a flatting agent, a dispersing agent and a preservative. The high-temperature-resistant fireproof facing coating disclosed by the invention not only has excellent fireproof performance and high-temperature-resistant performance, but also has good decorative performance and durability, and is suitable for fireproof protection of buildings and industrial steel structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fireproof coating, in particular to a high temperature resistant fireproof finishing coating. Background Art

[0002] In the construction engineering and industrial fields, the use of steel structures is becoming more and more common. However, steel structures are prone to lose strength at high temperatures, resulting in structural instability or even collapse. Therefore, in order to improve the fire resistance of steel structures, fire retardant coatings are usually applied on their surfaces. Most of the existing fire retardant coatings are intumescent fire retardant coatings, which protect the substrate by expanding at high temperatures to form an insulating layer. However, intumescent fire retardant coatings will produce a large amount of smoke under high temperature conditions, and their intumescent layers are susceptible to mechanical damage, affecting their fire resistance. In addition, existing fire retardant coatings also have certain deficiencies in terms of decorativeness and durability. Therefore, it is particularly important to develop a non-intumescent steel structure fire retardant coating with excellent fire resistance, high temperature resistance, good decorativeness and strong durability. Summary of the invention

[0003] The purpose of the present invention is to provide a high temperature resistant fireproof finishing paint.

[0004] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0005] The present invention comprises an organic adhesive, a lightweight heat-insulating filler, a refractory fiber, a refractory filler and an auxiliary agent. In parts by weight, the high-temperature resistant fireproof finishing coating contains 33 parts of the organic adhesive, 38 parts of the lightweight heat-insulating filler, 16 parts of the refractory fiber, 8 parts of the refractory filler and 5 parts of the auxiliary agent.

[0006] Furthermore, the organic adhesive includes acrylic emulsion and silicone acrylic emulsion, the lightweight thermal insulation filler includes expanded perlite, expanded vermiculite and hollow glass microspheres, the refractory fiber includes aluminum silicate fiber and basalt fiber, the refractory filler includes alumina, silica powder and titanium dioxide, and the additives include BYK-310, Solplus D540 and ActicideMBS.

[0007] Preferably, by volume, the ratio of acrylic emulsion to silicone acrylic emulsion is 1:8; the ratio of expanded perlite, expanded vermiculite and hollow glass microspheres is 2:2:3; the ratio of aluminum silicate fiber to basalt fiber is 1:4; the ratio of alumina, silica powder and titanium dioxide is 1:1:4; the ratio of BYK-310, Solplus D540 and Acticide MBS is 1:1:2.

[0008] The preparation method of the high temperature resistant fireproof finishing coating of the present invention comprises the following steps:

[0009] S1: weigh each component material according to the ratio;

[0010] S2: Pour the organic binder into the mixing container and start the mixer; gradually add the lightweight thermal insulation filler, refractory fiber, refractory filler and additives, and continue stirring to ensure uniform mixing; stirring time: 20-30 minutes, stirring speed: 500-1000rpm;

[0011] S3: Filter the mixed paint through a sieve to remove impurities and unmixed particles.

[0012] The beneficial effects of the present invention are:

[0013] The present invention is a high temperature resistant fireproof finishing coating, and compared with the prior art, the present invention has the following advantages:

[0014] Excellent fireproof performance: This coating can effectively insulate in high temperature environments, preventing the temperature of the steel structure from rising rapidly, thereby improving its fire resistance limit.

[0015] Good decorative properties: This coating not only has fireproof function, but also has good decorative effect and can meet the aesthetic requirements of building decoration.

[0016] High durability: This paint is not easy to age in high temperature environment, has a long service life, and can maintain its fireproof and decorative properties for a long time in harsh environment.

[0017] Environmental protection: This paint does not contain toxic and harmful substances, meets environmental protection requirements, and will not release a large amount of harmful smoke when a fire occurs, ensuring environmental safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a sample detection diagram of the present invention;

[0019] Figure 2 It is the specific heat capacity spectrum of the samples of the present invention. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0021] The present invention comprises an organic adhesive, a lightweight heat-insulating filler, a refractory fiber, a refractory filler and an auxiliary agent. In parts by weight, the high-temperature resistant fireproof finishing coating contains 33 parts of the organic adhesive, 38 parts of the lightweight heat-insulating filler, 16 parts of the refractory fiber, 8 parts of the refractory filler and 5 parts of the auxiliary agent.

[0022] Furthermore, the organic adhesive includes acrylic emulsion and silicone acrylic emulsion, the lightweight thermal insulation filler includes expanded perlite, expanded vermiculite and hollow glass microspheres, the refractory fiber includes aluminum silicate fiber and basalt fiber, the refractory filler includes alumina, silica powder and titanium dioxide, and the additives include BYK-310, Solplus D540 and ActicideMBS.

[0023] Preferably, by volume, the ratio of acrylic emulsion to silicone acrylic emulsion is 1:8; the ratio of expanded perlite, expanded vermiculite and hollow glass microspheres is 2:2:3; the ratio of aluminum silicate fiber to basalt fiber is 1:4; the ratio of alumina, silica powder and titanium dioxide is 1:1:4; the ratio of BYK-310, Solplus D540 and Acticide MBS is 1:1:2.

[0024] The preparation method of the high temperature resistant fireproof finishing coating of the present invention comprises the following steps:

[0025] S1: weigh each component material according to the ratio;

[0026] S2: Pour the organic binder into the mixing container and start the mixer; gradually add the lightweight thermal insulation filler, refractory fiber, refractory filler and additives, and continue stirring to ensure uniform mixing; stirring time: 20-30 minutes, stirring speed: 500-1000rpm;

[0027] S3: Filter the mixed paint through a sieve to remove impurities and unmixed particles.

[0028] The high temperature resistant fireproof finishing coating of the present invention is tested by a thermal conductivity meter, a differential scanning calorimeter, and an ultraviolet visible spectrophotometer. The monitoring items include thermal conductivity (500°C, 600°C, 700°C, 800°C, 900°C, 1000°C), density, specific heat capacity, emissivity, and absorption coefficient. The test samples are as follows: Figure 1 As shown, the specific heat capacity test spectrum is as follows Figure 2 The test results are shown in the following table:

[0029]

[0030] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A high temperature resistant fireproof finishing coating, characterized in that: It includes organic adhesive, lightweight thermal insulation filler, refractory fiber, refractory filler and additives. In parts by weight, the high-temperature resistant fireproof finishing coating contains 33 parts of the organic adhesive, 38 parts of the lightweight thermal insulation filler, 16 parts of the refractory fiber, 8 parts of the refractory filler and 5 parts of the additive.

2. The high temperature resistant fireproof finishing coating according to claim 1, characterized in that: The organic adhesive includes acrylic emulsion and silicone acrylic emulsion, the lightweight thermal insulation filler includes expanded perlite, expanded vermiculite and hollow glass microspheres, the refractory fiber includes aluminum silicate fiber and basalt fiber, the refractory filler includes alumina, silica powder and titanium dioxide, and the additives include BYK-310, Solplus D540 and Acticide MBS.

3. The high temperature resistant fireproof finishing coating according to claim 2, characterized in that: By volume ratio, the ratio of acrylic emulsion to silicone acrylic emulsion is 1:8; the ratio of expanded perlite, expanded vermiculite and hollow glass microspheres is 2:2:3; the ratio of aluminum silicate fiber to basalt fiber is 1:4; the ratio of alumina, silica powder and titanium dioxide is 1:1:4; the ratio of BYK-310, Solplus D540 and Acticide MBS is 1:1:

2.

4. The high temperature resistant fireproof finishing coating according to claim 3, characterized in that: The preparation method of the high temperature resistant fireproof finishing coating comprises the following steps: S1: weigh each component material according to the ratio; S2: Pour the organic binder into the mixing container and start the mixer; gradually add the lightweight thermal insulation filler, refractory fiber, refractory filler and additives, and continue stirring to ensure uniform mixing; stirring time: 20-30 minutes, stirring speed: 500-1000rpm; S3: Filter the mixed paint through a sieve to remove impurities and unmixed particles.

Citation Information

Patent Citations

  • Indoor coating with sound absorption function

    CN105153853A

  • Thermal insulation heat-preservation paint coating used for building external wall

    CN106700695A

  • Waterproof heat-insulation exterior wall coating and preparation method thereof

    CN108329780A

  • Tunnel stain-resistant decorative fireproof coating as well as preparation method and application thereof

    CN116162385A

  • Dry mixture for fire-protective coating

    RU2660154C1