A method for improving high temperature performance of shotcrete

By using a combination of silicone rubber tackifying insulation and spray concrete slurry under high rock temperature environments, the bonding insulation layer and locking structure are formed, which solves the poor bonding performance and crack resistance of spray concrete at high rock temperatures. The poor problem has achieved the improvement of high bonding, low rebound and crack resistance, ensuring the stability and safety of the tunnel structure.

CN117645450BActive Publication Date: 2024-12-06JIANGSU CHINA CONSTR COMMERCIAL CONCRETE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311612069.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-12-06
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

Under high rock temperature environment, the mechanical properties and durability of jet concrete are deteriorated at an accelerated manner, resulting in its loss of support in tunnel support, affecting the stability and safety of tunnel structure. The existing technology cannot effectively improve its high temperature stability and Adhesion properties.

Method used

The combination of silicone rubber tackifying insulation and sprayed concrete slurry is used to form a tackifying insulation layer and locking structure, which improves the high-temperature stability, bonding and crack resistance of sprayed concrete. Through silicone rubber and ceramic hollow micro The synergistic effect of beads, phenyl silicone oil and fibers forms a bridge structure to enhance adhesion and thermal insulation.

Benefits of technology

Significantly reduce the rebound rate of jet concrete, improve its crack resistance and mechanical properties at high rock temperatures, extend its service life, and ensure the stability and safety of the tunnel structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a method for improving the high temperature performance of shotcrete, and belongs to the technical field of highway tunnel engineering. The method comprises the following steps: S1. Applying a silicone rubber thickening and heat-insulating agent on the high temperature rock surface to form a thickening and heat-insulating layer; S2. Spraying the shotcrete slurry onto the high temperature rock surface coated with the thickening and heat-insulating layer. Before the shotcrete slurry is sprayed, the present invention first applies a layer of thickening and heat-insulating layer with excellent adhesion, heat insulation and water resistance on the high temperature rock surface, which provides effective adhesion and layered heat insulation before the shotcrete slurry contacts the rock surface; at the same time, fibers are used to bridge the thickening and heat-insulating layer and the shotcrete slurry, and after the shotcrete slurry is sprayed onto the rock surface, the concrete is tightly bonded, which effectively solves the problem that the traditional shotcrete is not suitable for high rock temperature conditions, has poor high temperature stability, poor bonding performance, and high spraying rebound rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of highway tunnel engineering, and in particular relates to a method for improving the high temperature performance of shotcrete. Background Art

[0002] In some major projects, tunnels and large underground projects are inevitably involved. Due to the complex geological conditions, tunnels are gradually developing in the direction of longer, larger and deeper. The high rock temperature of tunnels is also becoming increasingly prominent. For example, the highest rock temperature of Sangzhuling Tunnel is as high as 89.9℃, and the highest rock temperature of some hydropower station diversion tunnels can reach more than 105℃. High rock temperature has a huge adverse effect on the mechanical properties, durability and safety of concrete supporting tunnels. Sprayed concrete is a kind of fast-setting concrete used to reinforce and protect structures or rock surfaces. This technology uses a spraying machine, compressed air or other power to spray a certain mix of cement, sand, gravel and admixtures through a nozzle onto the sprayed surface. The concrete reinforcement material is formed by solidification and hardening in a short time. Unlike traditional on-site cast concrete, sprayed concrete does not require formwork and vibration, has the advantages of fast construction speed and high early strength, and has a very wide range of applicability. In tunnel engineering, shotcrete has been widely used. However, if the temperature of the surrounding rock is too high and cannot be reduced to room temperature in a short period of time, the shotcrete needs to be firmly bonded to the rock, which will cause the concrete to be affected by the high temperature, causing the mechanical properties and durability of the shotcrete to deteriorate rapidly and lose its supporting function, thus affecting the stability and safety of the tunnel structure.

[0003] The main reason why shotcrete is easy to deteriorate under high rock temperature conditions is that traditional shotcrete has poor high temperature stability, insufficient adhesion to surrounding rock, and high rebound rate. Shotcrete is in direct contact with high-temperature surrounding rock, which accelerates the cement hydration reaction. The hydration product is generated too quickly to diffuse evenly, and a large amount of it accumulates on the surface of cement particles to prevent water from entering the core, reducing the internal density, affecting or destroying the concrete hardening process, and affecting the later strength development of concrete; at the same time, concrete loses water faster in high temperature environment, and the shrinkage increases, causing volume deformation, which together cause serious loss of bonding performance between concrete and surrounding rock, high rebound rate, and easy cracking; in addition, the relatively frequent thermal expansion and cold contraction of the surrounding rock of high-rock temperature tunnels causes small cracks on the surface of the surrounding rock, which are pulled outward at high temperature. In addition, the temperature difference between the surrounding rock and shotcrete generates thermal stress, which easily generates stress inside the shotcrete and then cracks, affecting the bonding effect and durability of the concrete.

[0004] In summary, the comprehensive performance of shotcrete in high rock temperature tunnel environment is easily significantly reduced due to the influence of working conditions, and the technical means for simply improving the performance of shotcrete in the existing technology are relatively simple and cannot achieve good results.

[0005] Therefore, it is of great significance to provide a method to improve the comprehensive performance of shotcrete in high rock temperature environment. Summary of the invention

[0006] In view of the deficiencies of the above-mentioned prior art, the present invention provides a method for improving the high-temperature performance of shotcrete. On the one hand, a thermal insulating bonding layer is utilized to improve the high-temperature resistance of shotcrete and its bonding with high-temperature rock surface, thereby reducing the rebound rate. On the other hand, the high-temperature stability, bonding performance and crack resistance of shotcrete itself are improved. Under the combined effect of the above two aspects, shotcrete has the characteristics of high bonding, low rebound and excellent crack resistance in a high rock temperature environment, thereby solving the problems of poor bonding performance, high rebound rate, poor crack resistance and low strength of traditional shotcrete in a high rock temperature environment.

[0007] To achieve the above purpose, the specific technical solutions of the present invention are as follows:

[0008] A method for improving the high temperature performance of shotcrete comprises the following steps:

[0009] S1. Apply silicone rubber adhesion-enhancing heat-insulating agent on the high-temperature rock surface to form an adhesion-enhancing heat-insulating layer;

[0010] The silicone rubber adhesion-enhancing heat-insulating agent comprises the following components: α,ω-dihydroxy polydimethylsiloxane, 3-aminopropyl triethoxysilane, silane-modified silica powder, ceramic hollow microspheres, phenyl silicone oil, a crosslinking agent and a catalyst;

[0011] S2. spraying the shotcrete slurry onto the high-temperature rock surface coated with the adhesion-enhancing heat-insulating layer;

[0012] The sprayed concrete slurry comprises the following components in parts by weight: 380-450 parts of cementitious materials, 800-850 parts of modified ceramsite, 700-750 parts of sand, 3-5 parts of nano calcium carbonate, 0.6-1 part of polyurethane, 0.2-0.4 part of aramid fiber, 0.1-0.3 part of hydroxyethyl cellulose, 0.05-0.08 part of triethylamine, 1-3 parts of 3-aminopropyl triethoxysilane, 4-6 parts of tridecyl trimethyl ammonium bromide, 4-7 parts of admixture, and 160-175 parts of water.

[0013] The present invention adopts liquid silicone rubber with excellent high temperature stability and bonding performance, and cooperates with ceramic hollow microspheres to improve thermal insulation, silane-modified silica powder to improve water resistance and strength, and phenyl silicone oil cooperates with liquid silicone rubber to improve high temperature stability. With the cooperation of various components, the silicone rubber thickening and thermal insulation agent of the present invention has excellent bonding, thermal insulation and water resistance in a high temperature environment. By brushing a layer of silicone rubber thickening and thermal insulation agent on the high temperature rock surface before spraying the concrete slurry, the bonding effect between the sprayed concrete and the high temperature rock surface can be strengthened, and at the same time, the heat conducted from the high temperature rock surface to the sprayed concrete can be reduced, and the influence of high temperature on the sprayed concrete can be reduced; in addition, the pre-coated silicone rubber thickening and thermal insulation agent can achieve penetration, filling and repair of tiny cracks on the surface of the surrounding rock, and lock them firmly. The certain toughness of the material itself can alleviate the transmission of the outward pulling force of the surrounding rock at high temperature to the sprayed concrete. More importantly, under the joint bridging effect of polyurethane, aramid fiber, triethylamine and tridecyltrimethylammonium bromide, a tight interlocking structure can be formed between the silicone rubber viscosity enhancing insulation agent of the present invention and the shotcrete slurry, further strengthening the bonding effect between the shotcrete and the high-temperature rock surface, and weakening the deterioration effect of the high-temperature rock surface on the performance of the shotcrete.

[0014] Under the catalytic action of triethylamine, the polyurethane wrapped on the surface of the aramid fiber solidifies to form polyurethane wrapped aramid fiber. When the shotcrete slurry is sprayed onto the high-temperature rock surface coated with silicone rubber thickening and thermal insulation agent, the curing polyurethane wrapped aramid fiber and the curing silicone rubber thickening and thermal insulation agent combine with each other. Because the two are both organic polymers, and with the enhanced catalytic activity of tridecyltrimethylammonium bromide, one end of the polyurethane wrapped aramid fiber can be firmly locked in the silicone rubber thickening and thermal insulation layer, and the other end is tightly bonded to the concrete to form a bridging structure, which can greatly reduce the rebound rate of the shotcrete.

[0015] Aramid fiber has the properties of soft texture, light weight, high strength, and excellent high temperature resistance, but the surface of aramid fiber is relatively smooth, has high hydrophobicity, and has weak bonding with cement base. Under the catalytic action of triethylamine, the polyurethane wrapped on the surface of the aramid fiber is cured, a tiny uneven polyurethane cured film is formed on the fiber surface, a mechanical anchor point is formed between the fiber and the cement base, and the bonding force between the aramid fiber and the cement base can be effectively enhanced; at the same time, the alkaline property of the triethylamine can promote the hydration product at the interface of the aramid fiber and the concrete to form a more compact structure, effectively improving the interface bonding force and adhesion between the fiber and the cement base; the polyurethane cured film has excellent elasticity and toughness, helps to absorb the shrinkage and deformation of the concrete, thereby reducing the risk of cracking; in addition, under the strengthening bonding effect of 3-aminopropyltriethoxysilane and the micro-aggregate, volcanic ash activity and crystal nucleus action of nano calcium carbonate, the density of the concrete cement slurry is enhanced and the amount of hydrated calcium silicate gel is increased, the aramid fiber-mortar interface transition zone is improved, the bonding performance between the aramid fiber and the cement base is further improved, and the density of the interface transition zone is improved. The bonded and reinforced aramid fibers in shotcrete are like a large number of fine tendons, forming overlaps in the shotcrete, reducing the rebound rate of the shotcrete, further enhancing the high-temperature stability, and effectively regulating the microcracks caused by the shrinkage, drying shrinkage and temperature changes of the concrete. It can effectively reduce the probability of cracks in the concrete and greatly improve the crack resistance of the shotcrete.

[0016] The present invention effectively improves the adhesion between the sprayed concrete and the liquid silicone rubber by adding 3-aminopropyltriethoxysilane to the sprayed concrete slurry and utilizing the amino group in the 3-aminopropyltriethoxysilane to react with the hydroxyl group in the silicone rubber. Adding 3-aminopropyltriethoxysilane to the silicone rubber tackifying and heat insulating agent can provide a stable network structure, improve the high temperature resistance of the silicone rubber, increase its stability in a high rock temperature environment, and further improve the adhesion between the silicone rubber and the high rock temperature rock, and between the silicone rubber bonding insulation layer and the sprayed concrete.

[0017] Preferably, within 30 minutes after the silicone rubber tackifying heat insulating agent is applied, and within 5 minutes after the shotcrete slurry is prepared, the shotcrete slurry is sprayed onto the high-temperature rock surface coated with the tackifying heat insulating layer. By controlling the spraying time of the shotcrete slurry, the curing polyurethane and the curing silicone rubber tackifying heat insulating agent can be combined.

[0018] Preferably, in step S1, the amount of the silicone rubber tackifying heat insulating agent applied is 0.5-0.8 kg / m 2 .

[0019] Preferably, in step S1, the mass ratio of the α,ω-dihydroxypolydimethylsiloxane, 3-aminopropyltriethoxysilane, silane-modified silica powder, ceramic hollow microspheres, phenyl silicone oil, cross-linking agent and catalyst is (10-14): (0.6-1): (2-3): (3-5): (0.3-0.6): (0.5-1): (0.1-0.3).

[0020] Preferably, in step S1, the silane-modified silica powder is formed by modifying silica powder with methyltrimethoxysilane. Methyltrimethoxysilane has a hydrophobic functional group (methyl group) and a silicophilic functional group (methoxy group), which is connected to the surface of silica particles through the silicophilic functional group, so that the silane-modified silica powder can have a hydrophobic functional group; adding a silica filler with a hydrophobic functional group to the silicone rubber thickening and heat-insulating agent can greatly increase the content of the non-polar phase (hydrophobic phase) in the liquid silicone rubber, hinder the penetration of water molecules, and further improve the water resistance of the thickening and heat-insulating layer, so that it maintains a better performance in the sprayed concrete containing water, and the introduction of silica powder also has a significant effect on the strength of the liquid silicone rubber.

[0021] Preferably, in step S1, the crosslinking agent is methyltributylacetonato silane and / or vinyltributylacetonato silane, and the catalyst includes at least one of dibutyltin dilaurate, monobutyltin triisooctoate, dibutyltin diacetate, and tetrabutyltin.

[0022] Preferably, in step S2, the modified ceramsite has a particle size of 5 to 10 mm, a water absorption rate of ≤8%, and a thermal conductivity of ≤0.50 W / K·m.

[0023] The modified ceramsite is obtained by soaking natural ceramsite in 5% to 10% polyacrylate emulsion for 3 to 6 hours and then drying it.

[0024] High temperature environment will cause the water in concrete to evaporate quickly. Ceramic aggregate has good thermal insulation, but it is easy to absorb water. The evaporation of water plus the absorption of water by ceramsite will affect the hydration of concrete and cause cracking. Coating ceramsite with polymer emulsion can form a continuous film on the surface of ceramsite, reduce the water absorption rate of ceramsite, reduce water penetration, and improve the adhesion between ceramsite and cement base, improve the density of shotcrete and reduce the rebound rate.

[0025] Preferably, the method for preparing the shotcrete slurry comprises the following steps:

[0026] M1. Weigh each component by weight;

[0027] M2. The polyurethane is mixed with aramid fiber, hydroxyethyl cellulose and triethylamine are added, and the mixture is stirred evenly. After standing for 40 to 60 minutes, 3-aminopropyl triethoxysilane and nano-calcium carbonate are added, and the mixture is stirred evenly. Then, the cementitious material, modified ceramsite, sand, admixture, water and tridecyl trimethyl ammonium bromide are added, and the mixture is stirred evenly to obtain the sprayed concrete slurry.

[0028] Preferably, the polyurethane is a solvent-based polyurethane with a solid content of 30% to 40% and a viscosity of 2000 to 3000 mpa·s.

[0029] In the preparation method of the shotcrete slurry of the present invention, polyurethane and aramid fiber are firstly mixed, and the polyurethane is wrapped on the surface of the aramid fiber. Then, under the dispersion of hydroxyethyl cellulose and the catalytic action of triethylamine, the polyurethane wrapped on the surface of the aramid fiber is cured to form an uneven polyurethane cured film on the surface of the aramid fiber. When the polyurethane is not completely cured, 3-aminopropyl triethoxysilane and nano-calcium carbonate are added. Through the strengthening bonding effect of 3-aminopropyl triethoxysilane and the micro-aggregate, volcanic ash activity and crystal nucleation effect of the nano-calcium carbonate, the density of the concrete cement slurry is enhanced and the amount of hydrated calcium silicate gel is increased, the aramid fiber-mortar interface transition zone is improved, the bonding performance between the aramid fiber and the cement base is further improved, and the density of the interface transition zone is improved.

[0030] Preferably, the preparation method of the silicone rubber tackifying heat insulating agent comprises the following steps:

[0031] Pour the α,ω-dihydroxy polydimethylsiloxane and phenyl silicone oil into a double planetary mixer, stir evenly, and add ceramic hollow microspheres at a speed of 1000-1400rpm / min. When the material temperature rises to 110°C, reduce the speed to 600-800rpm / min, open the vacuum valve, continue stirring and dehydrating for 2.5h, and then discharge the material; after cooling the above semi-finished product to room temperature, add the cross-linking agent and disperse it evenly, then add silane-modified silica powder and 3-aminopropyltriethoxysilane in an inert gas atmosphere, stir at high speed for 20min under vacuum, then add the catalyst, stir evenly to obtain the silicone rubber viscosity-enhancing heat-insulating agent, and seal it for standby use.

[0032] Compared with the prior art, the present invention is beneficial in that:

[0033] (1) Before spraying concrete slurry, the present invention first applies a layer of adhesion-enhancing heat-insulating layer with excellent adhesion, heat insulation and water resistance on the high-temperature rock surface, thereby providing effective adhesion and layered heat insulation before the sprayed concrete slurry contacts the rock surface; at the same time, fibers are used to bridge the adhesion-enhancing heat-insulating layer and the sprayed concrete slurry. After the sprayed concrete slurry is sprayed onto the rock surface, the concrete is tightly bonded, and the high temperature environment of the high-temperature rock surface can promote the cross-linking and curing of liquid silicone rubber, locking the sprayed concrete, thereby effectively solving the problems that traditional sprayed concrete is not suitable for high rock temperature conditions, has poor high temperature stability, poor adhesion performance, and a high spray rebound rate.

[0034] (2) The present invention realizes the gradient transfer of high rock temperature and weakens the deterioration effect of high rock temperature conditions on the performance of shotcrete through the following two improvements: first, the excellent thermal insulation of the viscosity-enhancing insulation layer is used to reduce heat conduction; second, high-temperature resistant thermal insulation materials such as expanded clay and polyurethane aramid fiber are introduced into the shotcrete slurry to improve the high-temperature resistance and thermal insulation performance of the shotcrete.

[0035] (3) The present invention uses polyurethane to wrap aramid fiber. Under the catalytic action of triethylamine, polyurethane is cured on the surface of aramid fiber, and combined with 3-aminopropyl triethoxysilane and nano calcium carbonate, the bonding performance between aramid fiber and cement base is improved from both physical and chemical viscosity enhancement, and the elasticity, toughness and dispersibility of aramid fiber are improved; in addition, tridecyl trimethyl ammonium bromide is used to increase the catalytic activity, and the curing polyurethane wrapping aramid fiber and the curing silicone rubber viscosity-enhancing heat-insulating agent are promoted to be tightly interlocked to form a bridge structure. Through the above measures, the fine reinforcement overlap effect of aramid fiber in concrete is fully utilized, the rebound rate of shotcrete is greatly reduced, the high temperature stability is enhanced, the microcracks caused by concrete shrinkage and temperature shrinkage are reduced, and the crack resistance and mechanical properties of shotcrete are greatly improved. DETAILED DESCRIPTION

[0036] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The method for improving the high temperature performance of shotcrete of the present invention comprises the following steps:

[0038] S1. Apply silicone rubber adhesion-enhancing heat-insulating agent on the high-temperature rock surface to form an adhesion-enhancing heat-insulating layer;

[0039] The silicone rubber adhesion-enhancing heat-insulating agent comprises the following components: α,ω-dihydroxy polydimethylsiloxane, 3-aminopropyl triethoxysilane, silane-modified silica powder, ceramic hollow microspheres, phenyl silicone oil, a crosslinking agent and a catalyst;

[0040] S2. spraying the shotcrete slurry onto the high-temperature rock surface coated with the adhesion-enhancing heat-insulating layer;

[0041] The sprayed concrete slurry comprises the following components in parts by weight: 380-450 parts of cementitious materials, 800-850 parts of modified ceramsite, 700-750 parts of sand, 3-5 parts of nano calcium carbonate, 0.6-1 part of polyurethane, 0.2-0.4 part of aramid fiber, 0.1-0.3 part of hydroxyethyl cellulose, 0.05-0.08 part of triethylamine, 1-3 parts of 3-aminopropyl triethoxysilane, 4-6 parts of tridecyl trimethyl ammonium bromide, 4-7 parts of admixture, and 160-175 parts of water.

[0042] The modified ceramsite has a particle size of 5 to 10 mm, a water absorption rate of ≤8%, and a thermal conductivity of ≤0.50 W / K·m. The modified ceramsite is obtained by soaking natural ceramsite in 5% to 10% polyacrylate emulsion for 3 to 6 hours and then drying it.

[0043] In the following examples and comparative examples, the viscosity of α,ω-dihydroxypolydimethylsiloxane is in the range of 20000 to 40000 mPa·s; the silane-modified silica powder is obtained by modifying silica powder with methyltrimethoxysilane, and has a particle size of 1000 to 2000 mesh; the purity of 3-aminopropyltriethoxysilane is ≥98.0%, and the density is 0.94 to 0.95 g / cm 3 The average particle size of nano calcium carbonate is 60-80nm, the purity is ≥98%, and the pH value is 8.6; the polyurethane is a solvent-based polyurethane with a solid content of 30%-40% and a viscosity of 2000-3000mpa•s; the sand is natural river sand with a fineness modulus of 2.6-3.0 and a mud content of less than 2.5%; the initial setting time of the alkali-free liquid accelerator is ≤8min, the final setting time is ≤18min, and the dosage is 6% of the mass of the cementitious material; the aramid fiber is chopped aramid fiber; the cement is ordinary Portland cement with a specification of P•O 42.5R.

[0044] Example 1

[0045] This embodiment provides a method for improving the high temperature performance of shotcrete, comprising the following steps:

[0046] S1. Spray water on the high-temperature rock surface to wash away the floating powder on the surface, and then apply silicone rubber viscosity-enhancing heat-insulating agent on the high-temperature rock surface. The amount of silicone rubber viscosity-enhancing heat-insulating agent applied is 0.5kg / m 2 , forming an adhesion-enhancing heat-insulating layer;

[0047] S2. After the silicone rubber thickening and heat-insulating agent is applied, let it stand for 20 to 30 minutes. Then, within 5 minutes after the shotcrete slurry is prepared, load the prepared shotcrete slurry into the sprayer, use high-pressure air to transport the shotcrete slurry to the nozzle, and introduce alkali-free liquid quick-setting agent into the nozzle. The shotcrete slurry is sprayed from the nozzle at high speed onto the high-temperature rock surface coated with the thickening and heat-insulating layer.

[0048] The steps of preparing the silicone rubber tackifying heat insulating agent are as follows:

[0049] N1. Weigh α,ω-dihydroxypolydimethylsiloxane, 3-aminopropyltriethoxysilane, silane-modified silica powder, ceramic hollow microspheres, phenyl silicone oil, methyltributylidene oxime silane and dibutyltin dilaurate in a mass ratio of 10:0.6:3:5:0.6:0.5:0.1;

[0050] N2. Pour α,ω-dihydroxypolydimethylsiloxane and phenyl silicone oil into a dual planetary power mixer, start stirring, and add ceramic hollow microspheres at a speed of 1200rpm / min. When the material temperature rises to 110℃, reduce the speed to 700rpm / min, open the vacuum valve and continue stirring and dehydrating for 2.5h. After cooling to room temperature, add methyl tributylidene silane and stir evenly. Then, add silane-modified silica powder and 3-aminopropyltriethoxysilane under N2 protection, and then stir at a speed of 2000rpm / min for 20min under vacuum conditions. Finally, add dibutyltin dilaurate and stir evenly to obtain the silicone rubber thickening and heat-insulating agent, which is sealed for standby use.

[0051] The steps of preparing shotcrete slurry are as follows:

[0052] M1. Weigh the following components in parts by weight: 340 parts of cement, 60 parts of fly ash, 800 parts of modified ceramsite, 700 parts of sand, 5 parts of nano calcium carbonate, 1 part of solvent-based polyurethane, 0.4 parts of aramid fiber, 0.3 parts of hydroxyethyl cellulose, 0.08 parts of triethylamine, 3 parts of 3-aminopropyl triethoxysilane, 6 parts of tridecyltrimethylammonium bromide, 4 parts of water reducer, and 160 parts of water;

[0053] M2. Mix polyurethane with aramid fiber, add hydroxyethyl cellulose and triethylamine, stir evenly, let stand for 40 to 60 minutes, then add 3-aminopropyltriethoxysilane and nano-calcium carbonate, mix at a speed of 100 to 140 rpm / min for 90 to 120 seconds, then add cement, fly ash, ceramsite, sand, water reducer, water and tridecyltrimethylammonium bromide, mix at a speed of 40 to 60 rpm / min for 20 to 30 seconds to obtain the shotcrete slurry.

[0054] Example 2

[0055] The heat-resistant low-carbon concrete of this embodiment is basically the same as that of embodiment 1, except that:

[0056] In step S1, the amount of silicone rubber thickening and heat insulating agent applied is 0.8 kg / m 2 ;

[0057] The preparation method of silicone rubber tackifying heat insulating agent is as follows:

[0058] N1. Weigh α,ω-dihydroxypolydimethylsiloxane, 3-aminopropyltriethoxysilane, silane-modified silica powder, ceramic hollow microspheres, phenyl silicone oil, vinyltributylidene oxime silane and dibutyltin diacetate in a mass ratio of 14:1:2:3:0.3:1:0.3;

[0059] N2. Pour α,ω-dihydroxypolydimethylsiloxane and phenyl silicone oil into a dual planetary power mixer, start stirring, and add ceramic hollow microspheres at a speed of 1200rpm / min. When the material temperature rises to 110℃, reduce the speed to 700rpm / min, open the vacuum valve and continue stirring and dehydrating for 2.5h. After cooling to room temperature, add vinyl trisbutyl ketoxime silane and stir evenly. Then, add silane-modified silica powder and 3-aminopropyltriethoxysilane under N2 protection, and then stir at a speed of 2000rpm / min for 20min under vacuum conditions. Finally, add dibutyltin diacetate and stir evenly to obtain the silicone rubber thickening and heat-insulating agent, which is sealed for standby use.

[0060] The shotcrete slurry includes the following components in parts by weight: 390 parts of cement, 40 parts of fly ash, 850 parts of modified ceramsite, 750 parts of sand, 3 parts of nano calcium carbonate, 0.6 parts of solvent-based polyurethane, 0.2 parts of aramid fiber, 0.1 parts of hydroxyethyl cellulose, 0.05 parts of triethylamine, 1 part of 3-aminopropyltriethoxysilane, 4 parts of tridecyltrimethylammonium bromide, 7 parts of water reducer, and 175 parts of water.

[0061] Comparative Example 1

[0062] The method of Comparative Example 1 is substantially the same as that of Example 1, except that the method of this comparative example is as follows:

[0063] S1. Spray water on the high-temperature rock surface to wash away the floating powder on the surface;

[0064] S2. Within 5 minutes after the preparation of the shotcrete slurry is completed, the prepared shotcrete slurry is loaded into the sprayer, and the shotcrete slurry is transported to the nozzle by high-pressure air, and an alkali-free liquid quick-setting agent is introduced into the nozzle. The shotcrete slurry is sprayed from the nozzle at high speed onto the high-temperature rock surface.

[0065] That is, compared with Example 1, the comparative example did not spray the silicone rubber viscosity-enhancing heat-insulating agent on the high-temperature rock surface.

[0066] Comparative Example 2

[0067] The method of Comparative Example 2 is substantially the same as that of Example 1, except that the silicone rubber adhesion enhancing and heat insulating agent lacks silane-modified silica powder and ceramic hollow microspheres.

[0068] Comparative Example 3

[0069] The method of Comparative Example 3 is substantially the same as that of Example 1, except that the sprayed concrete slurry lacks solvent-based polyurethane, triethylamine and tridecyltrimethylammonium bromide.

[0070] Comparative Example 4

[0071] The method of Comparative Example 4 is substantially the same as that of Example 1, except that 3-aminopropyltriethoxysilane is absent in the sprayed concrete slurry.

[0072] Test example

[0073] The sprayed concrete of Examples 1 to 2 and Comparative Examples 1 to 4 were tested for thermal conductivity, rebound, mechanical properties and early crack resistance performance indicators. The wet spraying method was used in accordance with Appendix L of GBT50086-2015 "Technical Specifications for Rock and Soil Anchors and Sprayed Concrete Support Engineering" to form the number and size of test blocks required for mechanical properties, crack resistance and other tests. When forming the thermal conductivity, rebound, compressive strength and crack resistance flat plate test specimens, silicone rubber viscosity-enhancing insulation agent was first applied to the rock surface or the test mold, and then the test specimens were formed by wet spraying. In the test method, the compressive strength and early crack resistance performance indicators refer to GB / T50081-2019 "Standard for Test Methods of Physical and Mechanical Properties of Ordinary Concrete" and GB / T50082-2009 "Standard for Test Methods of Long-term Performance and Durability of Ordinary Concrete" respectively; the thermal conductivity test refers to the method in GB / T 10294-2008 "Determination of Steady-state Thermal Resistance and Related Characteristics of Insulating Materials Protective Plate Hot Plate Method", and the test instrument is IMDRY3001-II Concrete Thermal Conductivity Meter for testing; according to the method mentioned in Appendix G of JGJ / T372-2016 "Technical Code for Application of Shotcrete", the rebound index is measured. The compressive strength test mold, crack resistance flat plate, and rebound test plate test mold are continuously maintained at a temperature of 80℃±2℃ for specimen preparation and test environment. The test results are shown in Table 1.

[0074] Table 1 Shotcrete performance test results

[0075]

[0076] From the data in Table 1, it can be seen that under high temperature working conditions, the thermal conductivity of the sprayed concrete of Examples 1 to 2 of the present invention is within 0.2, and the rebound rate is less than 3.5%, which is much lower than the rebound rate of 15% to 20% or more of ordinary sprayed concrete. The 1d compressive strength reaches 23.7 to 23.9 MPa, and the 1d reaches more than 48% of the 28d strength ratio, and the later strength growth is more guaranteed. In terms of crack resistance, the total cracking area per unit area is 46 to 58 mm 2 / m 2 The cracks on the slab are almost invisible to the naked eye, and the crack resistance level of the slab is the highest level V. The test data of the embodiment show that the sprayed concrete of the present invention has excellent heat insulation and high temperature resistance, strength and crack resistance, and can significantly reduce the rebound rate.

[0077] Compared with Example 1, Comparative Example 1 did not spray silicone rubber thickening and heat-insulating agent on the high-temperature rock surface. Because there is no silicone rubber thickening and heat-insulating agent to provide excellent layered insulation effect and bonding force, when the shotcrete is sprayed onto the high-temperature panel, the cement hydration reaction is accelerated, but a large amount of hydration products accumulate on the surface of cement particles to organize water to enter the inner core, affecting the concrete hardening process, and the strength of 1d and 28d is significantly reduced, and the rebound rate is increased by 6.3 percentage points. In addition, under high temperature conditions, the concrete loses water faster, the shrinkage deformation of the concrete is aggravated, the total cracking area per unit area increases, and the concrete crack resistance is reduced, and finally it is reduced to Grade IV.

[0078] Compared with Example 1, the thermal conductivity of the concrete in Comparative Example 2 is increased by 38%, and the thermal insulation performance is reduced. In terms of other technical indicators, the rebound rate is increased, the total cracking area per unit area is increased, and the final crack resistance grade is V, which is close to the boundary of Grade IV. Ceramic hollow microspheres can further improve the thermal insulation performance of silicone rubber and improve the high temperature stability of shotcrete, while silane-modified silica powder can improve the water resistance and strength of silicone rubber, reduce the effect of initial moisture in shotcrete on silicone rubber and improve the adhesion of silicone rubber. This shows that under the synergistic cooperation of ceramic hollow microspheres, silane-modified silica powder and other components, the silicone rubber tackifying thermal insulation agent of the present invention has excellent adhesion, thermal insulation and water resistance under high temperature environment.

[0079] Compared with Example 1, solvent-based polyurethane, triethylamine and tridecyltrimethylammonium bromide were not added to the shotcrete slurry in Comparative Example 3. The rebound rate of Comparative Example 3 was increased to 6.2%, and the compressive strength index was slightly reduced, and the flat plate crack resistance grade was reduced to Grade IV. This shows that by adding solvent-based polyurethane and triethylamine to treat the fiber, the bonding force of aramid fiber in concrete can be effectively increased, and the anti-cracking reinforcement effect of aramid fiber can be improved. At the same time, with the effect of tridecyltrimethylammonium bromide, a tight interlocking structure can be formed between the silicone rubber viscosity-enhancing insulation agent and the shotcrete slurry, further strengthening the bonding effect between the shotcrete and the high-temperature rock surface, greatly reducing the rebound rate of the shotcrete, and giving full play to the performance improvement effect of aramid fiber in concrete under high temperature conditions. The concrete rebound rate of Comparative Example 4 is 1.7 percentage points higher than that of Example 1, which indicates that by adding 3-aminopropyltriethoxysilane to the shotcrete slurry, the amino group in 3-aminopropyltriethoxysilane can be used to react with the hydroxyl group in the silicone rubber, thereby effectively improving the adhesion between the shotcrete and the liquid silicone rubber, thereby reducing the rebound rate of the shotcrete.

[0080] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for improving the high temperature performance of shotcrete, It is characterized in that The following steps are involved: S1. Apply silicone rubber adhesion-enhancing heat-insulating agent on the high-temperature rock surface to form an adhesion-enhancing heat-insulating layer; The silicone rubber adhesion-enhancing heat-insulating agent comprises the following components: α,ω-dihydroxy polydimethylsiloxane, 3-aminopropyl triethoxysilane, silane-modified silica powder, ceramic hollow microspheres, phenyl silicone oil, a crosslinking agent and a catalyst; S2. spraying the shotcrete slurry onto the high-temperature rock surface coated with the adhesion-enhancing heat-insulating layer; The sprayed concrete slurry comprises the following components in parts by weight: 380-450 parts of cementitious materials, 800-850 parts of modified ceramsite, 700-750 parts of sand, 3-5 parts of nano calcium carbonate, 0.6-1 part of polyurethane, 0.2-0.4 part of aramid fiber, 0.1-0.3 part of hydroxyethyl cellulose, 0.05-0.08 part of triethylamine, 1-3 parts of 3-aminopropyl triethoxysilane, 4-6 parts of tridecyl trimethyl ammonium bromide, 4-7 parts of admixture, and 160-175 parts of water.

2. A method for improving the high temperature performance of shotcrete according to claim 1, It is characterized in that Within 30 minutes after the silicone rubber adhesion-enhancing heat-insulating agent is applied, and within 5 minutes after the shotcrete slurry is prepared, the shotcrete slurry is sprayed onto the high-temperature rock surface coated with the adhesion-enhancing heat-insulating layer.

3. A method for improving high temperature performance of shotcrete according to claim 1, It is characterized in that In step S1, the amount of silicone rubber thickening and heat-insulating agent applied is 0.5-0.8 kg / m 2 .

4. A method for improving high temperature performance of shotcrete according to claim 1, It is characterized in that In step S1, the mass ratio of the α,ω-dihydroxypolydimethylsiloxane, 3-aminopropyltriethoxysilane, silane-modified silica powder, ceramic hollow microspheres, phenyl silicone oil, cross-linking agent and catalyst is (10-14): (0.6-1): (2-3): (3-5): (0.3-0.6): (0.5-1): (0.1-0.3).

5. A method for improving high temperature performance of shotcrete according to claim 1, It is characterized in that In step S1, the silane-modified silica powder is prepared by modifying silica powder with methyltrimethoxysilane.

6. A method for improving high temperature performance of shotcrete according to claim 1, It is characterized in that In step S1, the crosslinking agent is methyltributylacetonato silane and / or vinyltributylacetonato silane, and the catalyst includes at least one of dibutyltin dilaurate, monobutyltin triisooctoate, dibutyltin diacetate, and tetrabutyltin.

7. A method for improving high temperature performance of shotcrete according to claim 1, It is characterized in that In step S2, the modified ceramsite has a particle size of 5 to 10 mm, a water absorption rate of ≤8%, and a thermal conductivity of ≤0.50 W / K·m.

8. A method for improving high temperature performance of shotcrete according to claim 1, It is characterized in that The preparation method of the shotcrete slurry comprises the following steps: M1. Weigh each component by weight; M2. The polyurethane is mixed with aramid fiber, hydroxyethyl cellulose and triethylamine are added, and the mixture is stirred evenly. After standing for 40 to 60 minutes, 3-aminopropyl triethoxysilane and nano-calcium carbonate are added, and the mixture is stirred evenly. Then, the cementitious material, modified ceramsite, sand, admixture, water and tridecyl trimethyl ammonium bromide are added, and the mixture is stirred evenly to obtain the sprayed concrete slurry.

9. A method for improving high temperature performance of shotcrete according to claim 1, It is characterized in that The preparation method of the silicone rubber tackifying heat insulating agent comprises the following steps: Pour the α,ω-dihydroxy polydimethylsiloxane and phenyl silicone oil into a mixer, stir evenly, and add ceramic hollow microspheres at a speed of 1000-1400 rpm / min. When the material temperature rises to 110°C, reduce the speed to 600-800 rpm / min, open the vacuum valve, continue stirring and dehydrating for 2.5 hours, and then discharge the material; after cooling the above semi-finished product to room temperature, add a cross-linking agent and disperse it evenly, then add silane-modified silica powder and 3-aminopropyltriethoxysilane in an inert gas atmosphere, stir evenly under vacuum, add a catalyst, and stir evenly to obtain the silicone rubber viscosity-enhancing thermal insulation agent.

Citation Information

Patent Citations

  • Ceramsite dual-doped shotcrete for high-temperature tunnel rock surfaces

    CN102718443A

  • Heat-insulating composite material and preparation method thereof

    CN111423728A

  • Deep well high-temperature roadway high-strength heat-insulation supporting structure and construction method

    CN113958344A

  • Environment-friendly energy-saving thermal insulation sealant as well as preparation method and application thereof

    CN115029101A

  • High-strength and high-toughness thermal-insulation functional sprayed concrete for occurrence high-temperature hot water tunnel

    CN116283145A