High-temperature-resistant composite coating for electric car and preparation method thereof
By adding modified hollow glass microbeads and alumina to the acrylic resin coating, the problem of degradation of the performance of the coating at high temperatures is solved, and its mechanical and high-temperature resistance is significantly improved, forming a high-temperature composite coating.
Patent Information
- Application Number
- CN202411046855.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Acrylate coatings are prone to degradation under long-term high temperature exposure, such as color changes, reduced gloss, and reduced hardness, resulting in reduced coating performance, and hollow glass microbeads have compatibility challenges with acrylic resins.
Add a variety of high-temperature resistant inorganic fillers, such as hollow glass microbeads, zirconia, and alumina, and through organic modification, it improves its compatibility and interface bonding in acrylic resin, and adopts a specific process The steps and material ratios include mechanical stirring, ultrasonic dispersion, melt extrusion, etc., to form modified fillers to enhance the mechanical and high temperature resistance of the coating.
It significantly improves the mechanical properties and high temperature resistance of acrylic resin composite coatings, enhances the stability and wear resistance of the coatings, and avoids the performance of the coatings under high temperature conditions.
Smart Images

Figure BDA0004973720300000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tram coatings and relates to a high temperature resistant composite coating for trams and a preparation method thereof. Background Art
[0002] Tram paint, as a paint specially used for tram bodies and other auto parts, mainly consists of four components: film-forming substances, pigments, solvents and additives. Film-forming substances are usually natural resins or artificial resins. Their key role is to tightly bond other components to form a tough and complete protective film. Pigments are the outermost covering, mainly carrying the topcoat color of the paint. Solvents and additives work together to promote the smooth construction of the paint on the surface of the car body, improve the chemical properties of the paint, and enhance the gloss of the car body.
[0003] Acrylate resin is a resin synthesized with acrylate or methacrylate as the main raw material. The coating based on this resin is called acrylic coating. Although acrylic coating has certain heat resistance, it may gradually degrade under long-term high temperature exposure, such as color change, reduced gloss, reduced hardness, etc., resulting in a decrease in coating performance.
[0004] Hollow glass microspheres, whose main component is borosilicate, present a unique hollow thin-walled spherical structure. The particle size range is usually between 10 and 250 microns, while the wall thickness is relatively thin, only about 1 to 2 microns. The thin inner wall makes it easy to break. However, hollow glass microspheres have been widely used in civil fields such as coatings, cement, emulsion explosives, and adhesives due to their low density, high strength, excellent thermal insulation properties, and good fluidity and stability. However, when hollow glass microspheres are filled into acrylic resin coating matrix as fillers, there are compatibility challenges due to the significant difference in polarity between the two. Summary of the invention
[0005] The purpose of the present invention is to provide a high temperature resistant composite coating for trams and a preparation method thereof. The present invention significantly improves the mechanical properties and high temperature resistance of the acrylic resin composite coating by adding a variety of high temperature resistant inorganic fillers to the composite coating and organically modifying the composite coating.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing a high temperature resistant composite coating for electric vehicles comprises the following steps:
[0008] Step 1: after methacrylic acid, methyl methacrylate, vinyl acetate and functional monomers are uniformly mixed, an organic solvent is added and heated, an initiator and a modified filler are added and mixed, and then heat-insulated treatment is performed, and the mixture is cooled to room temperature to obtain a modified acrylic resin; the functional monomers are composed of N-hydroxymethyl acrylamide and isooctyl acrylate;
[0009] Step 2: Add a leveling agent, a nano pigment and an auxiliary agent to the modified acrylic resin and stir at high speed, then add an organic solvent and continue stirring and sieve to obtain a high temperature resistant composite coating.
[0010] As a preferred technical solution of the present invention, in step one, the heating temperature is to heat to 65-75°C; the heat preservation treatment is to keep the temperature at 70-75°C for 8-10h; the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, functional monomer, organic solvent, initiator and modified filler is 6-9:15-20:6-7:14-16:70-80:0.8-1.0:2.4-3.0; the functional monomer is a mixture of N-hydroxymethyl acrylamide and isooctyl acrylate in a mass ratio of 1.0-1.5:5-6; the organic solvent is ethyl acetate; the initiator is one or two of azobisisobutyronitrile and benzoyl peroxide.
[0011] As a preferred technical solution of the present invention, in step 2, the high-speed stirring is stirring at a speed of 1000-1200 r / min for 30-45 min; the continued stirring is stirring at a speed of 400-600 r / min for 10-15 min; the sieving is sieving through a 400-mesh sieve; the mass ratio of the modified acrylic resin, leveling agent, nano-pigment, auxiliary agent and organic solvent is 50-55:0.5-0.8:10-12:1-3:30-40; the nano-pigment is pigment red A3B; the leveling agent is one or two of BYK-300 and Evonik TEGO450; the organic solvent is ethyl acetate; the auxiliary agent is silica particles, Therm HPG 6806 or Therm HPG 4000; The present invention and comparative examples are selected ThermHPG 4000.
[0012] The present invention discloses a method for preparing the modified filler, comprising the following steps:
[0013] 1) adding the mixed microbeads into a sodium hydroxide aqueous solution and mechanically stirring the solution, filtering out the liquid to obtain the solid, washing the solid with deionized water, and drying the solid in an oven to obtain a prefabricated filler;
[0014] 2) under an inert atmosphere, adding the prefabricated filler into deionized water for ultrasonic dispersion, adding zirconium oxychloride to adjust the pH of the solution to alkaline, heating the solution, washing the solid, and drying the solid in an oven to obtain a mixed filler;
[0015] 3) After mixing alumina, anhydrous ethanol and p-aminobenzoic acid, add vanillin, heat and stir, filter out the filtrate, wash with ethanol, and dry in an oven to obtain modified alumina;
[0016] 4) placing the terpolymer, mixed filler and modified alumina in a twin-screw extruder for melt extrusion and then granulating to obtain a modified filler; the terpolymer is styrene-vinyl trimethoxysilane-glycidyl methacrylate copolymer.
[0017] As a preferred technical solution of the present invention, in step 1), the mechanical stirring is stirring at a speed of 400-600 r / min for 45-60 min; the washing is washing to neutrality; and the drying is drying at a temperature of 60-70° C. to constant weight.
[0018] As a preferred technical solution of the present invention, in step 1), the mixed microspheres include the following components by weight: 10-20 parts of hollow glass microspheres with a particle size of 30 μm, 18-24 parts of hollow glass microspheres with a particle size of 40 μm, and 20-30 parts of hollow glass microspheres with a particle size of 60 μm; the concentration of the sodium hydroxide aqueous solution is 20-25 g / L; the amount ratio of the hollow glass microspheres to the sodium hydroxide aqueous solution is 2.0-2.4 g: 25 mL; in the scheme of the present invention, after the hollow glass microspheres of different particle sizes are treated with sodium hydroxide, the hollow glass microspheres are connected to more hydroxyl groups and their surfaces are coarsened. The roughened surfaces of the hollow glass microspheres are more easily attached to zirconium oxide, and zirconium oxide is filled on the rough surfaces of the hollow glass microspheres, reducing agglomeration and improving dispersion and uniformity; the hollow glass microspheres have a unique hollow thin-wall structure and are relatively cheap. A layer of special functional material is coated on the surface to form a core-shell hollow structure, reducing the agglomeration of the filler itself.
[0019] As a preferred technical solution of the present invention, in step 2), the inert atmosphere is a nitrogen atmosphere; the ultrasonic dispersion is performed at a power of 100-200W for 45-60min; the pH of the solution is adjusted to alkaline by using ammonia water to adjust the pH of the solution to 9-10; the heating is performed at a temperature of 130-150°C for 3-5h; the washing is performed by washing with deionized water to neutrality; the drying is performed at a temperature of 70-80°C to constant weight; and the mass ratio of the deionized water, the prefabricated filler and the zirconium oxychloride is 30:4-5:2.5-3.0.
[0020] As a preferred technical solution of the present invention, in step 3), the stirring and mixing is stirring at a speed of 600-800r / min for 20-30min; the heating and stirring is stirring at a temperature of 60-75°C for 4-6h; the drying is drying at a temperature of 70-80°C to constant weight; the mass ratio of the aluminum oxide, anhydrous ethanol, p-aminobenzoic acid and vanillin is 13-15:50-55:2.6-3.0:4.0-4.2; in the scheme of the present invention, the imine structure formed by p-aminobenzoic acid and vanillin, combined with the addition of thermal stability and rigid benzene ring structure, can increase the compatibility and high temperature resistance between the aluminum oxide and the acrylate matrix.
[0021] As a preferred technical solution of the present invention, in step 4), the temperature of the melt extrusion is 180-210°C; the mass ratio of the terpolymer, the mixed filler and the modified alumina is 7-10:2.8-3.2:6-8.
[0022] The present invention discloses a method for preparing the terpolymer, comprising the following steps:
[0023] Styrene, vinyl trimethoxysilane and glycidyl methacrylate are placed in ethyl acetate, an initiator is added, the mixture is heated, and the ethyl acetate is removed to obtain a terpolymer; the terpolymer contains a large amount of benzene ring structures, silicone structures and epoxy groups, which can act as a compatibilizer to increase the compatibility of fillers and play a role in reinforcing composite coatings.
[0024] As a preferred technical solution of the present invention, the heating treatment is heating at a temperature of 70-75°C for 3-4h; the initiator is azobisisobutyronitrile; the mass ratio of styrene, vinyltrimethoxysilane, glycidyl methacrylate, ethyl acetate and initiator is 10-14:3.0-3.5:4.0-4.3:60-70:0.35-0.40.
[0025] Beneficial effects of the present invention:
[0026] The present invention introduces high temperature resistant fillers such as hollow glass microspheres, zirconium oxide, aluminum oxide, etc. into the composite coating, and organically modifies the fillers to increase their compatibility in the acrylic resin composite coating, improve the interface bonding force between the fillers and the components, and significantly improve the mechanical properties and high temperature resistance of the acrylic resin composite coating. DETAILED DESCRIPTION
[0027] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0028] Example 1
[0029] A method for preparing a high temperature resistant composite coating for electric vehicles comprises the following steps:
[0030] Step 1: After methacrylic acid, methyl methacrylate, vinyl acetate and functional monomer are uniformly mixed, an organic solvent is added and the temperature is raised to 65°C, an initiator and a modified filler are added and mixed, and the mixture is kept at 70°C for 8 hours, and cooled to room temperature to obtain a modified acrylic resin; wherein the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, functional monomer, organic solvent, initiator and modified filler is 6:15:6:14:70:0.8:2.4; the functional monomer is prepared by mixing N-hydroxymethyl acrylamide and isooctyl acrylate in a mass ratio of 1.0:5; the organic solvent is ethyl acetate; and the initiator is azobisisobutyronitrile;
[0031] Step 2: Add a leveling agent, a nano-pigment and an auxiliary agent to the modified acrylic resin, stir at a speed of 1000 r / min for 30 minutes, add an organic solvent, stir at a speed of 400 r / min for 10 minutes, and then pass through a 400-mesh sieve to obtain a high-temperature resistant composite coating; wherein the mass ratio of the modified acrylic resin, the leveling agent, the nano-pigment, the auxiliary agent and the organic solvent is 50:0.5:10:1:30; the nano-pigment is pigment red A3B; the leveling agent is BYK-300; the auxiliary agent is silica particles; and the organic solvent is ethyl acetate.
[0032] The preparation method of the modified filler comprises the following steps:
[0033] 1) adding mixed microbeads to a sodium hydroxide aqueous solution, stirring at a speed of 400 r / min for 45 minutes, filtering out the liquid to obtain the solid, washing with deionized water until neutral, placing in an oven, and drying at a temperature of 60° C. to a constant weight to obtain a prefabricated filler; wherein the mixed microbeads include the following components by weight: 10 parts of hollow glass microbeads with a particle size of 30 μm, 18 parts of hollow glass microbeads with a particle size of 40 μm, and 20 parts of hollow glass microbeads with a particle size of 60 μm; the concentration of the sodium hydroxide aqueous solution is 20 g / L; the amount ratio of the hollow glass microbeads to the sodium hydroxide aqueous solution is 2.0 g:25 mL;
[0034] 2) under a nitrogen atmosphere, adding the prefabricated filler to deionized water and ultrasonically treating at 100 W for 45 min, adding zirconium oxychloride, adjusting the pH of the solution to 9 with ammonia water, heating at 130° C. for 3 h, washing the solid with deionized water until neutral, placing it in an oven, and drying it at 70° C. to constant weight to obtain a mixed filler; wherein the mass ratio of the deionized water, the prefabricated filler and the zirconium oxychloride is 30:4:2.5;
[0035] 3) After stirring alumina, anhydrous ethanol and p-aminobenzoic acid at a speed of 600 r / min for 20 minutes, vanillin is added and stirred at a temperature of 60° C. for 4 hours, the filtrate is filtered off and washed with anhydrous ethanol for 3 times, and dried in an oven at a temperature of 70° C. to constant weight to obtain modified alumina; wherein the mass ratio of the alumina, anhydrous ethanol, p-aminobenzoic acid and vanillin is 13:50:2.6:4.0;
[0036] 4) placing the terpolymer, mixed filler and modified alumina in a twin-screw extruder, melt-extrude at 180° C., and granulate to obtain a modified filler; wherein the mass ratio of the terpolymer, mixed filler and modified alumina is 7:2.8:6.
[0037] The preparation method of the terpolymer comprises the following steps:
[0038] Styrene, vinyl trimethoxysilane and glycidyl methacrylate are placed in ethyl acetate, azobisisobutyronitrile is added and heated at 70°C for 3 hours, and the ethyl acetate is removed to obtain a terpolymer; wherein the mass ratio of styrene, vinyl trimethoxysilane, glycidyl methacrylate, ethyl acetate and azobisisobutyronitrile is 10:3.0:4.0:60:0.35.
[0039] Example 2
[0040] A method for preparing a high temperature resistant composite coating for electric vehicles comprises the following steps:
[0041] Step 1: After methacrylic acid, methyl methacrylate, vinyl acetate and functional monomer are uniformly mixed, an organic solvent is added and the temperature is raised to 68°C, an initiator and a modified filler are added and mixed, and the mixture is kept at 72°C for 8.5 hours, and cooled to room temperature to obtain a modified acrylic resin; wherein the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, functional monomer, organic solvent, initiator and modified filler is 7:17:6.3:14.7:73:0.85:2.6; the functional monomer is prepared by mixing N-hydroxymethyl acrylamide and isooctyl acrylate in a mass ratio of 1.2:5.3; the organic solvent is ethyl acetate; and the initiator is azobisisobutyronitrile;
[0042] Step 2: Add a leveling agent, a nano-pigment and an auxiliary agent to the modified acrylic resin, stir at a speed of 1050 r / min for 35 minutes, add an organic solvent, stir at a speed of 460 r / min for 12 minutes, and then pass through a 400-mesh sieve to obtain a high-temperature resistant composite coating; wherein the mass ratio of the modified acrylic resin, the leveling agent, the nano-pigment, the auxiliary agent and the organic solvent is 52:0.6:10.7:1.7:33; the nano-pigment is pigment red A3B; the leveling agent is BYK-300; the auxiliary agent is silica particles; and the organic solvent is ethyl acetate.
[0043] The preparation method of the modified filler comprises the following steps:
[0044] 1) adding mixed microbeads to a sodium hydroxide aqueous solution, stirring at a speed of 460 r / min for 50 min, filtering out the liquid and taking out the solid, washing with deionized water until neutral, placing in an oven, and drying at a temperature of 63° C. to a constant weight to obtain a prefabricated filler; wherein the mixed microbeads include the following components by weight: 13 parts of hollow glass microbeads with a particle size of 30 μm, 20 parts of hollow glass microbeads with a particle size of 40 μm, and 23 parts of hollow glass microbeads with a particle size of 60 μm; the concentration of the sodium hydroxide aqueous solution is 22 g / L; the amount ratio of the hollow glass microbeads to the sodium hydroxide aqueous solution is 2.1 g:25 mL;
[0045] 2) under nitrogen atmosphere, adding the prefabricated filler to deionized water and ultrasonically treating at 130 W for 50 min, adding zirconium oxychloride, adjusting the pH of the solution to 9.3 with ammonia water, heating at 137° C. for 3.7 h, washing the solid with deionized water until neutral, placing it in an oven, and drying it at 73° C. to constant weight to obtain a mixed filler; wherein the mass ratio of the deionized water, the prefabricated filler and the zirconium oxychloride is 30:4.3:2.7;
[0046] 3) After stirring alumina, anhydrous ethanol and p-aminobenzoic acid at a speed of 660 r / min for 23 min, vanillin was added and stirred at a temperature of 65° C. for 4.5 h, the filtrate was filtered off and washed with anhydrous ethanol for 3 times, and dried in an oven at a temperature of 73° C. to constant weight to obtain modified alumina; wherein the mass ratio of the alumina, anhydrous ethanol, p-aminobenzoic acid and vanillin is 13.7:52:2.7:4.1;
[0047] 4) placing the terpolymer, mixed filler and modified alumina in a twin-screw extruder, melt-extrude at 190° C., and granulate to obtain a modified filler; wherein the mass ratio of the terpolymer, mixed filler and modified alumina is 8:2.9:6.7.
[0048] The preparation method of the terpolymer comprises the following steps:
[0049] Styrene, vinyl trimethoxysilane and glycidyl methacrylate are placed in ethyl acetate, azobisisobutyronitrile is added and heated at 72°C for 3.5 hours, and the ethyl acetate is removed to obtain a terpolymer; wherein the mass ratio of styrene, vinyl trimethoxysilane, glycidyl methacrylate, ethyl acetate and azobisisobutyronitrile is 11:3.2:4.1:63:0.37.
[0050] Example 3
[0051] A method for preparing a high temperature resistant composite coating for electric vehicles comprises the following steps:
[0052] Step 1: After methacrylic acid, methyl methacrylate, vinyl acetate and functional monomer are uniformly mixed, an organic solvent is added and the temperature is raised to 72°C, an initiator and a modified filler are added and mixed, and the mixture is kept at 73°C for 9.5 hours, and then cooled to room temperature to obtain a modified acrylic resin; wherein the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, functional monomer, organic solvent, initiator and modified filler is 8:18:6.7:15.3:77:0.9:2.8; the functional monomer is a mixture of N-hydroxymethyl acrylamide and isooctyl acrylate in a mass ratio of 1.3:5.6; the organic solvent is ethyl acetate; and the initiator is azobisisobutyronitrile;
[0053] Step 2: Add a leveling agent, a nano-pigment and an auxiliary agent to the modified acrylic resin, stir the mixture at a speed of 1130 r / min for 40 minutes, add an organic solvent, stir the mixture at a speed of 530 r / min for 13 minutes, and then pass the mixture through a 400-mesh sieve to obtain a high-temperature resistant composite coating; wherein the mass ratio of the modified acrylic resin, the leveling agent, the nano-pigment, the auxiliary agent and the organic solvent is 53:0.7:11.3:2.3:37; the nano-pigment is pigment red A3B; the leveling agent is BYK-300; the auxiliary agent is silica particles; and the organic solvent is ethyl acetate.
[0054] The preparation method of the modified filler comprises the following steps:
[0055] 1) adding the mixed microbeads to a sodium hydroxide aqueous solution, stirring at a speed of 530 r / min for 55 min, filtering out the liquid and taking out the solid, washing with deionized water until neutral, placing in an oven, and drying at a temperature of 67° C. to a constant weight to obtain a prefabricated filler; wherein the mixed microbeads include the following components by weight: 17 parts of hollow glass microbeads with a particle size of 30 μm, 22 parts of hollow glass microbeads with a particle size of 40 μm, and 27 parts of hollow glass microbeads with a particle size of 60 μm; the concentration of the sodium hydroxide aqueous solution is 23 g / L; the amount ratio of the hollow glass microbeads to the sodium hydroxide aqueous solution is 2.3 g:25 mL;
[0056] 2) under a nitrogen atmosphere, adding the prefabricated filler to deionized water and ultrasonically treating at a power of 165 W for 55 minutes, adding zirconium oxychloride, adjusting the pH of the solution to 9.7 with ammonia water, heating at 145° C. for 4.5 hours, washing the solid with deionized water until it is neutral, placing it in an oven, and drying it at 77° C. to constant weight to obtain a mixed filler; wherein the mass ratio of the deionized water, the prefabricated filler and the zirconium oxychloride is 30:4.7:2.8;
[0057] 3) After stirring alumina, anhydrous ethanol and p-aminobenzoic acid at a speed of 730 r / min for 25 min, vanillin was added and stirred at a temperature of 70° C. for 5.5 h, the filtrate was filtered off and washed with anhydrous ethanol for 3 times, and dried in an oven at a temperature of 77° C. to constant weight to obtain modified alumina; wherein the mass ratio of the alumina, anhydrous ethanol, p-aminobenzoic acid and vanillin is 14.5:53:2.9:4.1;
[0058] 4) placing the terpolymer, mixed filler and modified alumina in a twin-screw extruder, melt-extrude at 200° C., and granulate to obtain a modified filler; wherein the mass ratio of the terpolymer, mixed filler and modified alumina is 9:3.1:7.3.
[0059] The preparation method of the terpolymer comprises the following steps:
[0060] Styrene, vinyl trimethoxysilane and glycidyl methacrylate are placed in ethyl acetate, azobisisobutyronitrile is added and heated at 73°C for 3.5 hours, and the ethyl acetate is removed to obtain a terpolymer; wherein the mass ratio of styrene, vinyl trimethoxysilane, glycidyl methacrylate, ethyl acetate and azobisisobutyronitrile is 13:3.3:4.2:67:0.38.
[0061] Example 4
[0062] A method for preparing a high temperature resistant composite coating for electric vehicles comprises the following steps:
[0063] Step 1: After methacrylic acid, methyl methacrylate, vinyl acetate and functional monomer are uniformly mixed, an organic solvent is added and the temperature is raised to 75°C, an initiator and a modified filler are added and mixed, and the mixture is kept at 75°C for 10 hours, and cooled to room temperature to obtain a modified acrylic resin; wherein the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, functional monomer, organic solvent, initiator and modified filler is 9:20:7:16:80:1.0:3.0; the functional monomer is a mixture of N-hydroxymethyl acrylamide and isooctyl acrylate in a mass ratio of 1.5:6; the organic solvent is ethyl acetate; and the initiator is azobisisobutyronitrile;
[0064] Step 2: Add a leveling agent, a nano-pigment and an auxiliary agent to the modified acrylic resin, stir at a speed of 1200 r / min for 45 minutes, add an organic solvent, stir at a speed of 600 r / min for 15 minutes, and then pass through a 400-mesh sieve to obtain a high-temperature resistant composite coating; wherein the mass ratio of the modified acrylic resin, the leveling agent, the nano-pigment, the auxiliary agent and the organic solvent is 55:0.8:12:3:40; the nano-pigment is pigment red A3B; the leveling agent is BYK-300; the auxiliary agent is silica particles; and the organic solvent is ethyl acetate.
[0065] The preparation method of the modified filler comprises the following steps:
[0066] 1) adding mixed microbeads to a sodium hydroxide aqueous solution, stirring at a speed of 600 r / min for 60 min, filtering out the liquid to obtain the solid, washing with deionized water until neutral, placing in an oven, and drying at a temperature of 70° C. to a constant weight to obtain a prefabricated filler; wherein the mixed microbeads include the following components by weight: 20 parts of hollow glass microbeads with a particle size of 30 μm, 24 parts of hollow glass microbeads with a particle size of 40 μm, and 30 parts of hollow glass microbeads with a particle size of 60 μm; the concentration of the sodium hydroxide aqueous solution is 25 g / L; the amount ratio of the hollow glass microbeads to the sodium hydroxide aqueous solution is 2.4 g:25 mL;
[0067] 2) under a nitrogen atmosphere, adding the prefabricated filler to deionized water and ultrasonicating at a power of 200 W for 60 minutes, adding zirconium oxychloride, adjusting the pH of the solution to 10 with ammonia water, heating at a temperature of 150° C. for 5 hours, washing the solid with deionized water until it is neutral, placing it in an oven, and drying it at a temperature of 80° C. to a constant weight to obtain a mixed filler; wherein the mass ratio of the deionized water, the prefabricated filler and the zirconium oxychloride is 30:5:3.0;
[0068] 3) After stirring alumina, anhydrous ethanol and p-aminobenzoic acid at a speed of 800 r / min for 30 minutes, vanillin is added and stirred at a temperature of 75° C. for 6 hours, the filtrate is filtered off and washed with anhydrous ethanol for 3 times, and placed in an oven at a temperature of 80° C. to dry to constant weight to obtain modified alumina; wherein the mass ratio of the alumina, anhydrous ethanol, p-aminobenzoic acid and vanillin is 15:55:3.0:4.2;
[0069] 4) placing the terpolymer, mixed filler and modified alumina in a twin-screw extruder, melt-extrude at 210° C., and granulate to obtain a modified filler; wherein the mass ratio of the terpolymer, mixed filler and modified alumina is 10:3.2:8.
[0070] The preparation method of the terpolymer comprises the following steps:
[0071] Styrene, vinyl trimethoxysilane and glycidyl methacrylate are placed in ethyl acetate, azobisisobutyronitrile is added and heated at 75°C for 4 hours, and the ethyl acetate is removed to obtain a terpolymer; wherein the mass ratio of styrene, vinyl trimethoxysilane, glycidyl methacrylate, ethyl acetate and azobisisobutyronitrile is 14:3.5:4.3:70:0.4.
[0072] Comparative Examples 1-3
[0073] Compared with Example 4, the difference between Comparative Examples 1-3 is that the components of the mixed filler are as shown in Table 1; the other components, preparation steps and parameters are the same.
[0074] Table 1
[0075]
[0076] Comparative Example 4
[0077] Compared with Example 4, the difference of Comparative Example 4 is that step 1) is not performed, mixed microbeads are used instead of prefabricated fillers, and the other components, preparation steps and parameters are the same.
[0078] Comparative Example 5
[0079] Compared with Example 4, Comparative Example 5 is different in that step 2) is not performed, prefabricated fillers are used instead of mixed fillers, and the remaining components, preparation steps and parameters are the same.
[0080] Comparative Example 6
[0081] Compared with Example 4, Comparative Example 6 is different in that p-aminobenzoic acid is not used, and the remaining components, preparation steps and parameters are the same.
[0082] Comparative Example 7
[0083] Compared with Example 4, Comparative Example 7 is different in that vanillin is not used, and the other components, preparation steps and parameters are the same.
[0084] Comparative Example 8
[0085] Compared with Example 4, Comparative Example 8 is different in that vinyltrimethoxysilane is not used, and the remaining components, preparation steps and parameters are the same.
[0086] Comparative Example 9
[0087] Compared with Example 4, Comparative Example 9 is different in that glycidyl methacrylate is not used, and the other components, preparation steps and parameters are the same.
[0088] Comparative Example 10
[0089] Compared with Example 4, Comparative Example 10 is different in that no terpolymer is used, and the other components, preparation steps and parameters are the same.
[0090] The composite coatings prepared in Examples 1-4 and Comparative Examples 1-10 were subjected to the following performance tests, respectively. The test results are shown in Table 2.
[0091] Impact resistance test: GB / T 1732-2020 for impact resistance test.
[0092] High temperature resistance test: Test the impact strength of the film after baking at 150°C for 100 hours;
[0093] Table 2
[0094] Impact strength (kg cm) Impact strength after baking (kg cm) Example 1 58 53 Example 2 57 52 Example 3 55 50 Example 4 60 55 Comparative Example 1 42 35 Comparative Example 2 46 38 Comparative Example 3 48 41 Comparative Example 4 46 37 Comparative Example 5 40 33 Comparative Example 6 47 40 Comparative Example 7 48 41 Comparative Example 8 41 34 Comparative Example 9 39 32 Comparative Example 10 35 27
[0095] From the test results in Table 2, it can be seen that compared with Comparative Examples 1-10, the composite coatings prepared in Examples 1-4 of the present invention have excellent mechanical properties and high temperature resistance.
[0096] The present invention uses hollow glass microspheres with different particle sizes to reinforce each other and fill gaps, thereby increasing the density of the structure after the coating is cured, improving the mechanical properties and high temperature resistance of the coating, and then using sodium hydroxide to roughen the hollow glass microspheres with different particle sizes, so that the surface of the composite hollow glass microspheres is rougher and more active hydroxyl groups are introduced. By generating uniformly distributed zirconium oxide on the surface of the hollow glass microspheres, the rough surface of the hollow glass microspheres plays a similar "anchoring" role to the zirconium oxide, increasing the bonding force between the two, and the zirconium oxide can coat the hollow glass microspheres, while introducing more hydroxyl groups, reducing the agglomeration phenomenon between particles, improving the thermal stability and wear resistance of the coating, and overcoming the phenomenon that the hollow glass microspheres are crushed due to extrusion due to direct addition.
[0097] Next, the present invention loads p-aminobenzoic acid in the porous structure of alumina. The p-aminobenzoic acid can form a chemical bond with vanillin, and an imine structure and a benzene ring structure with good thermal stability are introduced into the porous structure of alumina. The dispersibility and compatibility of alumina in acrylic resin coatings are increased through organic modification.
[0098] Finally, the present invention melt-extrudes the terpolymer, mixed filler and modified alumina. The organosilicon structure of the terpolymer can further improve the mechanical properties and high temperature resistance of the coating after curing. The terpolymer can also be used as a compatibilizer. The epoxy group thereof is used to form a bridge between the mixed filler and the modified alumina. The carbon-carbon double bond can significantly increase the compatibility and dispersibility of the mixed filler and the modified alumina in the system, thereby reinforcing the composite coating and improving its high temperature resistance.
[0099] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a high temperature resistant composite coating for electric vehicles, characterized in that: The preparation method comprises the following steps: Step 1: after methacrylic acid, methyl methacrylate, vinyl acetate and functional monomers are uniformly mixed, an organic solvent is added and heated, an initiator and a modified filler are added and mixed, and then heat-insulated treatment is performed, and the mixture is cooled to room temperature to obtain a modified acrylic resin; the functional monomers are composed of N-hydroxymethyl acrylamide and isooctyl acrylate; Step 2: adding a leveling agent, a nano pigment and an auxiliary agent to the modified acrylic resin and stirring at high speed, then adding an organic solvent and continuing stirring and sieving to obtain a high temperature resistant composite coating; Wherein, the preparation method of the modified filler comprises the following steps: 1) adding the mixed microbeads into a sodium hydroxide aqueous solution and mechanically stirring the solution, filtering out the liquid and obtaining the solid, washing the solid with deionized water, and drying the solid in an oven to obtain a prefabricated filler; 2) Under an inert atmosphere, the prefabricated filler is added to deionized water for ultrasonic dispersion, zirconium oxychloride is added to adjust the pH of the solution to alkaline, the solution is heated, the solid is washed, and the solid is placed in an oven for drying to obtain a mixed filler; 3) After mixing alumina, anhydrous ethanol and p-aminobenzoic acid, add vanillin, heat and stir, filter out the filtrate, wash with ethanol, and dry in an oven to obtain modified alumina; 4) placing the terpolymer, mixed filler and modified alumina in a twin-screw extruder for melt extrusion and granulation to obtain a modified filler; the terpolymer is styrene-vinyl trimethoxysilane-glycidyl methacrylate copolymer.
2. The method for preparing a high temperature resistant composite coating for electric vehicles according to claim 1, characterized in that: In step one, the heating temperature is to heat to 65-75°C; the heat preservation treatment is to keep the temperature at 70-75°C for 8-10h; the mass ratio of methacrylic acid, methyl methacrylate, vinyl acetate, functional monomer, organic solvent, initiator and modified filler is 6-9:15-20:6-7:14-16:70-80:0.8-1.0:2.4-3.0; the functional monomer is a mixture of N-hydroxymethyl acrylamide and isooctyl acrylate in a mass ratio of 1.0-1.5:5-6; the organic solvent is ethyl acetate; the initiator is one or two of azobisisobutyronitrile and benzoyl peroxide.
3. The method for preparing a high temperature resistant composite coating for electric vehicles according to claim 1, characterized in that: In step 2, the high-speed stirring is stirring at a speed of 1000-1200 r / min for 30-45 min; the continued stirring is stirring at a speed of 400-600 r / min for 10-15 min; the screening is through a 400-mesh sieve; the mass ratio of the modified acrylic resin, leveling agent, nano-pigment, auxiliary agent and organic solvent is 50-55:0.5-0.8:10-12:1-3:30-40; the leveling agent is one or two of BYK-300 and Evonik TEGO450; the auxiliary agent is silicon dioxide particles; and the organic solvent is ethyl acetate.
4. The method for preparing a high temperature resistant composite coating for electric vehicles according to claim 1, characterized in that: In step 1), the mechanical stirring is stirring at a speed of 400-600 r / min for 45-60 min; the washing is washing until neutral; The drying step is drying at 60-70° C. to a constant weight.
5. The method for preparing a high temperature resistant composite coating for electric vehicles according to claim 1, characterized in that: In step 1), the mixed microspheres include the following components by weight: 10-20 parts of hollow glass microspheres with a particle size of 30 μm, 18-24 parts of hollow glass microspheres with a particle size of 40 μm, and 20-30 parts of hollow glass microspheres with a particle size of 60 μm; the concentration of the sodium hydroxide aqueous solution is 20-25 g / L; and the usage ratio of the hollow glass microspheres to the sodium hydroxide aqueous solution is 2.0-2.4 g:25 mL.
6. The method for preparing a high temperature resistant composite coating for electric vehicles according to claim 1, characterized in that: In step 2), the inert atmosphere is a nitrogen atmosphere; the ultrasonic dispersion is performed at a power of 100-200 W for 45-60 min; the pH of the solution is adjusted to alkaline by using ammonia water to adjust the pH of the solution to 9-10; the heating is performed at a temperature of 130-150° C. for 3-5 h; the washing is performed by washing with deionized water to neutrality; the drying is performed at a temperature of 70-80° C. to constant weight; and the mass ratio of deionized water, prefabricated filler and zirconium oxychloride is 30:4-5:2.5-3.
0.
7. The method for preparing a high temperature resistant composite coating for electric vehicles according to claim 1, characterized in that: In step 3), the stirring and mixing is stirring at a speed of 600-800 r / min for 20-30 min; the heating and stirring is stirring at a temperature of 60-75°C for 4-6 h; the drying is drying at a temperature of 70-80°C to constant weight; the mass ratio of the aluminum oxide, anhydrous ethanol, p-aminobenzoic acid and vanillin is 13-15:50-55:2.6-3.0:4.0-4.
2.
8. The method for preparing a high temperature resistant composite coating for electric vehicles according to claim 1, characterized in that: In step 4), the temperature of the melt extrusion is 180-210° C.; the mass ratio of the terpolymer, the mixed filler and the modified alumina is 7-10:2.8-3.2:6-8.
9. A high temperature resistant composite coating for electric vehicles prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Cathode electrophoresis paint with antistatic and antifreezing functions and manufacturing method thereof
CN104725910A
Heat-resistant and wear-resistant aluminum alloy wood grain transfer printing sectional material
CN108102524A
Inorganic fireproof thermal insulation coating and preparation method thereof
CN112409830A
Automotive water-based sound insulation damping coating with high damping performance and preparation method thereof
CN115197623A
Temperature-resistant thermal insulation coating for metal surface
CN115637084A
Cited By
High-strength UV ink and preparation method thereof
CN120272047A
Application of environment-friendly cyclohexanone peroxide curing agent composition in high-speed rail putty
CN121271301A