Aramid fiber composite modified waterborne epoxy coating and preparation method thereof
By using high shear force and peristaltic pump technology in water-based epoxy coatings to disperse aramid fibers evenly, the problem of difficult dispersion and agglomeration of aramid fibers in water-based coatings is solved, and the corrosion resistance and salt spray resistance of the coating are improved , enhances the protection effect of steel.
Patent Information
- Application Number
- CN202411082510.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-08
AI Technical Summary
During the use of existing water-based epoxy anticorrosion coatings, pinholes and defects are prone to occur after moisture evaporation and curing, which leads to infiltration of corrosive media, reducing the anticorrosion effect of steel, and it is difficult to disperse aramid fibers evenly in the coating, resulting in agglomeration and reduction. Anti-corrosion performance.
By dispersing aramid fibers into the aqueous phase under the action of dispersant and high shear force, and dropping the pre-dispersed aramid fiber aqueous solution using a peristaltic pump to make it evenly wrap on the surface of the emulsion particles to avoid agglomeration and form A dense passivation layer fills the defects in the coating and improves corrosion resistance.
Effectively fill pinholes and defects in the coating, enhance the shielding and salt spray resistance of the coating, extend the time when corrosion liquid penetrates to the surface of the metal substrate, and improve the corrosion resistance of the coating.
Smart Images

Figure CN118931323A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-corrosion coatings, and in particular to an aramid fiber composite modified waterborne epoxy coating and a preparation method thereof. Background Art
[0002] Since steel is susceptible to oxidation, corrosion and other problems, applying anti-corrosion coatings on the surface of steel is a widely used and most effective protective technology. In recent years, environmentally friendly water-based epoxy polymer anti-corrosion coatings have emerged. However, during the use of water-based coatings, pinholes and defects will inevitably appear after the water evaporates and solidifies into a film. In the later stage, it is very easy to cause the infiltration of corrosive media such as water molecules, oxygen molecules, and chloride ions in the environment, causing rust on the steel. Therefore, adding various synergistic materials to water-based coatings is a key issue in improving the long-term anti-corrosion performance of coatings.
[0003] Among various synergistic materials, aramid fiber stands out due to its good chemical corrosion resistance, high specific strength and modulus, and low specific density. In addition, fibrous aramid can fill the pinholes and defects formed by the coating, shield the penetration of corrosive media, and form a dense passivation layer on the surface of the metal substrate.
[0004] In the currently published preparation methods of aramid fiber reinforced waterborne epoxy anticorrosive coatings, such as CN106336775A, aramid fibers are usually added directly into a container and ground with the pigment and filler components in the coating. However, aramid fibers have good chemical stability and are not easy to interact with other media, which easily leads to agglomeration in the coating and inability to disperse evenly, resulting in gaps between emulsion particles, which in turn causes the corrosive medium to penetrate into the coating along the gaps, reducing the anticorrosive effect of the coating. Summary of the invention
[0005] In view of the problems of the prior art, the present invention provides an aramid fiber composite modified water-based epoxy coating and a preparation method thereof. First, the aramid fiber is dispersed into the water phase under the action of a dispersant and high shear force, and then the emulsifier, epoxy resin, and cosolvent are heated to melt, and the dispersion is started. The pre-dispersed aramid fiber aqueous solution is dripped by a peristaltic pump, and the aramid fiber can be evenly wrapped on the surface of the emulsion particles during the phase inversion process, thereby completing the dispersion of the aramid fiber in the epoxy emulsion and avoiding the occurrence of agglomeration. By using the method of the present invention, the aramid fiber can effectively fill the pinholes and defects that appear after the water evaporates and solidifies into a film, reduce the gaps between the emulsion particles, and improve the shielding performance of the coating against water vapor, salt spray resistance, and corrosion resistance.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A kind of aramid fiber composite modified waterborne epoxy coating, the raw material composition of which comprises two components A and B, wherein the component A comprises, by weight, 40-60 parts of aramid fiber modified epoxy emulsion, 10-70 parts of pigments and fillers, 0.1-3 parts of anti-flash rust agent, 0.1-5 parts of dispersant, 2-3 parts of film-forming aid, 1-3 parts of defoamer, 1-3 parts of thickener, 1-2 parts of wetting agent, and 10-50 parts of water; wherein the component B comprises, by weight, 10-40 parts of curing agent and 5-20 parts of propylene glycol methyl ether; the mass ratio of the components A and B is 100:30-40.
[0008] The aramid fiber modified epoxy emulsion is prepared according to the following method:
[0009] (1) Add 1-10 parts of aramid fiber, 0.1-1 parts of dispersant, and 50-90 parts of water into a jacketed reactor, open the condensation water, and disperse at 25° C. and 2000-4500 r / min for 2-6 hours to obtain a dispersed aramid fiber aqueous solution.
[0010] (2) Add 40-60 parts of epoxy resin, 4-8 parts of emulsifier, and 6-12 parts of cosolvent into a jacketed reactor, heat to 60-80°C until melted, start dispersion, stir evenly at a speed of 1000-2000 r / min, maintain the material temperature at 60-65°C, start the peristaltic pump, and add 30-60 parts of aramid fiber aqueous solution at a speed of 1-2 ml / min. After the addition is completed, stir at a speed of 1000-1500 r / min for 15-30 minutes, and obtain the aramid fiber modified epoxy emulsion after filtering.
[0011] The present invention further provides a method for preparing the above-mentioned aramid fiber composite modified waterborne epoxy coating, the specific steps comprising:
[0012] S1: Preparation of component A: Add aramid fiber modified epoxy emulsion, pigment filler, anti-rust agent, dispersant, film-forming aid, defoamer, thickener, wetting agent and water into the reactor according to the proportion, grind to a fineness of less than 25 μm, filter the material and obtain component A;
[0013] S2: Preparation of component B: Add curing agent and propylene glycol methyl ether into the reactor according to the ratio, stir and mix at a speed of 500-1000 rpm / min, filter the material to obtain component B;
[0014] S3: Component A and component B are mixed evenly in a mass ratio of 100:30-40, and filtered to obtain an aramid fiber composite modified water-based epoxy coating.
[0015] Preferably, the epoxy resin is selected from bisphenol A epoxy resin; more preferably, it is selected from one or more of E51, E44, and E20 epoxy resins.
[0016] Preferably, the aramid fiber is a para-aramid fiber; more preferably, the aramid fiber has a diameter between 10-100 nm and an aspect ratio of about 3000.
[0017] Preferably, the emulsifier is a non-ionic emulsifier of polyetheramine grafted modified epoxy resin, and the preparation method is as follows:
[0018] Weigh 2-5 parts of E51 epoxy resin, 1-5 parts of polyethylene glycol with a molecular weight of 3500-6000, 0.5-2 parts of polyetheramine with a molecular weight of 2000-4000, and 0.01-0.03 parts of tetrafluoroboric acid by weight; add E51 epoxy resin and polyethylene glycol into a reactor, heat to 100-110° C., drop all of tetrafluoroboric acid within 1-2 hours, keep warm at 100-110° C. for reaction for 3-4 hours, add polyetheramine, heat to 120-140° C., continue to react for 4-6 hours, and obtain a non-ionic emulsifier for polyetheramine grafted modified epoxy resin.
[0019] Preferably, the co-solvent is selected from one or more of propylene glycol methyl ether, propylene glycol butyl ether and acetone.
[0020] Preferably, the pigment filler is selected from one or more of titanium dioxide, talcum powder, barium sulfate, red iron, zinc phosphate, strontium chrome yellow and mica powder.
[0021] Preferably, the dispersant is selected from one or more of dodecyl sulfonates, alkyl alcohol polyoxyethylene ethers, polyacrylates, and polycarboxylates.
[0022] Preferably, the film-forming aid is selected from one or more of dipropylene glycol methyl ether, propylene glycol methyl ether and dipropylene glycol butyl ether.
[0023] Preferably, the defoaming agent is selected from one or more of polyether blocks, silicones, and mineral oils.
[0024] Preferably, the thickener is selected from one or more of cellulose, polyacrylic acid, inorganic thickener and polyurethane.
[0025] Preferably, the curing agent is selected from one or more of Huntsman 3986, Hexion 6870, and Allnex 613W.
[0026] The flash rust preventer is not specially selected and can be prepared or purchased using existing technology. Preferably, it can be one or more of CK-20, CK-35, and HY-72.
[0027] The wetting agent is not specially selected and can be prepared or purchased using existing technology. Preferably, it can be one or more of TEGO-245, TEGO-270, and TEGO280.
[0028] Beneficial effects of the present invention:
[0029] The present invention adopts aramid fiber to modify the waterborne epoxy coating, effectively enhancing the anti-corrosion and salt spray resistance of the coating. Aramid fiber, as a reinforcing material, can fill the pinholes and defects that appear in the coating after the water evaporates and solidifies into a film, shielding the entry of corrosive media. Secondly, due to the multi-layer coating of aramid fiber, the external corrosive medium needs a longer time to pass through the protective film of the aramid fiber, increasing the difficulty of the corrosive liquid penetrating into the surface of the metal substrate. Aramid fiber is mainly para-aramid fiber and meta-aramid fiber. Para-aramid fiber has the characteristics of high strength and high modulus, high temperature resistance and corrosion resistance, and has a large specific surface area, high surface energy, good dispersibility, water retention rate, and excellent flame retardant performance. In addition, the mystery of aramid nanofiber film formation is good in dimensional stability and insulation, and can form a uniform suspension with water, which is easy to spray.
[0030] The present invention utilizes high-speed shear force to disperse aramid fibers in the water phase in advance. During the phase inversion process, as the system changes from water-in-oil to oil-in-water, the aramid fibers more evenly wrap the emulsion particles, thereby completing the dispersion of the aramid fibers in the water-based epoxy emulsion and avoiding the occurrence of agglomeration.
[0031] The process flow and principle adopted by the invention are relatively simple, highly operable, environmentally friendly, pollution-free, and highly repeatable, and can realize large-scale industrial continuous production.
[0032] The present invention preferably uses a special emulsifier, which is prepared by modifying a polyetheramine grafted epoxy resin, retains the epoxy group, has good compatibility with the epoxy resin, and can participate in the curing of the latex film-forming process to further increase the cross-linking density of the coating.
[0033] The present invention limits the amount of aramid fiber added in the preparation method. When the added amount is too low, it is insufficient to fill the defects generated when the water-based coating is cured to form a film in the later stage, and the improvement of the anti-corrosion performance of the water-based epoxy coating is relatively limited. When the added amount is too high, the excessive aramid fiber is difficult to disperse, and the excess aramid fiber will always be free outside the system, causing certain damage to the performance of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The aramid fiber aqueous solution dispersed in Example 2;
[0035] Figure 2 This is the Fourier infrared transform image of the emulsifier for polyetheramine grafted epoxy resin;
[0036] Figure 3 is a TEM image of the aramid fiber aqueous solution in Example 2;
[0037] Figure 4TEM image of aramid fiber modified epoxy emulsion in Example 2;
[0038] Figure 5 It is a comparison chart of the salt spray resistance results of Comparative Example 1 and Example 2. DETAILED DESCRIPTION
[0039] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0040] The para-aramid fiber is produced by Shandong Jufang New Materials Co., Ltd., with a diameter between 10-100nm and an aspect ratio of about 3000.
[0041] Example 1
[0042] Prepare the emulsifier:
[0043] Weigh 2 parts of E51 epoxy resin, 1 part of 4000 molecular weight polyethylene glycol, 0.5 parts of 3000 molecular weight polyetheramine, and 0.01 parts of tetrafluoroboric acid; add E51 epoxy resin and polyethylene glycol into a reactor, heat to 100°C, add all the tetrafluoroboric acid dropwise within 1 hour, keep the reaction at 100°C for 3 hours, add polyetheramine, heat to 120°C, and continue the reaction for 4 hours to obtain a non-ionic emulsifier for polyetheramine grafted modified epoxy resin.
[0044] Preparation of aramid fiber modified epoxy emulsion:
[0045] (1) According to weight, 2 parts of aramid fiber, 50 parts of water, and 0.2 parts of dispersant are weighed, condensed water is turned on, and dispersed at 25° C. and 3000 r / min for 4 hours to obtain a dispersed aramid fiber aqueous solution, wherein the aramid fiber is para-aramid fiber.
[0046] (2) In parts by weight, 50 parts of E20 epoxy resin, 5 parts of emulsifier and 8.5 parts of cosolvent were added into a jacketed reactor and heated to 80°C until melted. Then, the dispersion was started and stirred evenly at a speed of 1500 r / min. The material temperature was maintained at 60°C. The peristaltic pump was started and 46.5 parts of aramid fiber aqueous solution were added dropwise at a speed of 2 ml / min. After the addition was completed, the mixture was stirred at a speed of 1500 r / min for 30 min and filtered to obtain an aramid fiber-modified epoxy emulsion.
[0047] Preparation of aramid fiber composite modified waterborne epoxy coating:
[0048] The amount of each component is as shown in the following table, by weight. Accurately weigh component 1, add it to the dispersion tank, add 2-5 in sequence while stirring, and disperse at 1000rpm for 5 minutes. Add components 6-14 in sequence while stirring, disperse at 1000rpm for 10 minutes, add zirconium beads, grind at high speed to a fineness of less than 25 microns, filter and set aside to obtain component A. Accurately weigh components 15 and 16, mix and stir evenly, filter, and obtain component B. Mix and stir components A and B in a mass ratio of 100:32, filter, and obtain a water-based epoxy coating composite modified with aramid fiber.
[0049] Serial number of each component Material Name Weight 1 water 18.0 2 Propylene glycol methyl ether 2.0 3 Dispersant TEGO 760W 1.2 4 Wetting agent TEGO 270 0.2 5 Defoamer TEGO 810 0.1 6 Titanium dioxide 10.3 7 Iron Red 0.8 8 Zinc phosphate 4.0 9 Mica powder 3.0 10 talcum powder 7.0 11 Barium sulfate 10.0 12 Aramid fiber modified epoxy emulsion 40.0 13 Thickener TEGO 3060 1.3 14 Anti-flash rust agent CK-20 2.1 15 Curing agent 3986 16.0 16 Propylene glycol methyl ether 16.0
[0050] Example 2
[0051] Prepare the emulsifier:
[0052] Weigh 2 parts of E51 epoxy resin, 2 parts of 4000 molecular weight polyethylene glycol, 1 part of 2000 molecular weight polyetheramine, and 0.02 parts of tetrafluoroboric acid; add E51 epoxy resin and polyethylene glycol into a reactor, heat to 100°C, add all the tetrafluoroboric acid dropwise within 1 hour, keep the reaction at 100°C for 3 hours, add polyetheramine, heat to 120°C, and continue the reaction for 4 hours to obtain a non-ionic emulsifier for polyetheramine grafted modified epoxy resin.
[0053] Preparation of aramid fiber modified epoxy emulsion:
[0054] (1) By weight, 4 parts of aramid fiber, 50 parts of water, and 0.4 parts of dispersant are weighed, condensed water is turned on, and dispersed at 25° C. and 3000 r / min for 4 hours to obtain a dispersed aramid fiber aqueous solution, wherein the aramid fiber is para-aramid fiber.
[0055] (2) In parts by weight, 55 parts of E20 epoxy resin, 6 parts of emulsifier and 9 parts of cosolvent were added into a jacketed reactor, heated to 80°C until melted, and then the dispersion was started. The mixture was stirred evenly at a speed of 1500 r / min, and the material temperature was maintained at 60°C. The peristaltic pump was started, and 45 parts of aramid fiber aqueous solution were added dropwise at a speed of 2 ml / min. After the addition was completed, the mixture was stirred at a speed of 1500 r / min for 30 min, and the aramid fiber-modified epoxy emulsion was obtained after filtration.
[0056] Preparation of aramid fiber composite modified waterborne epoxy coating:
[0057] The amount of each component is as shown in the following table, weigh 1 accurately, add it to the dispersion tank, add 2-5 in sequence while stirring, and disperse at 1000rpm for 5 minutes. Add 6-14 in sequence while stirring, disperse at 1000rpm for 10 minutes, add zirconium beads, grind at high speed to a fineness of less than 25 microns, filter and set aside to obtain component A. Weigh 15 and 16 accurately, mix and stir evenly, filter, and obtain component B. Mix and stir components A and B evenly in a mass ratio of 100:32, filter, and obtain a water-based epoxy coating composite modified with aramid fiber.
[0058] Serial number of each component Material Name Weight 1 water 18.0 2 Propylene glycol methyl ether 2.0 3 Dispersant TEGO 760W 1.2 4 Wetting agent TEGO 270 0.2 5 Defoamer TEGO 810 0.1 6 Titanium dioxide 10.3 7 Iron Red 0.8 8 Zinc phosphate 4.0 9 Mica powder 3.0 10 talcum powder 7.0 11 Barium sulfate 10.0 12 Aramid fiber modified epoxy emulsion 40.0 13 Thickener TEGO 3060 1.3 14 Anti-flash rust agent CK-20 2.1 15 Curing agent 3986 16.0 16 Propylene glycol methyl ether 16.0
[0059] Example 3
[0060] Prepare the emulsifier:
[0061] Weigh 2 parts of E51 epoxy resin, 1 part of 6000 molecular weight polyethylene glycol, 0.5 parts of 2000 molecular weight polyetheramine, and 0.01 parts of tetrafluoroboric acid; add E51 epoxy resin and polyethylene glycol into a reactor, heat to 100°C, add all the tetrafluoroboric acid dropwise within 1 hour, keep the reaction at 100°C for 3 hours, add polyetheramine, heat to 120°C, and continue the reaction for 4 hours to obtain a non-ionic emulsifier for polyetheramine grafted modified epoxy resin.
[0062] Preparation of aramid fiber modified epoxy emulsion:
[0063] (1) By weight, 6 parts of aramid fiber, 50 parts of water, and 0.6 parts of dispersant are weighed, condensed water is turned on, and dispersed at 25° C. and 3000 r / min for 4 hours to obtain a dispersed aramid fiber aqueous solution, wherein the aramid fiber is para-aramid fiber.
[0064] (2) In parts by weight, 50 parts of E20 epoxy resin, 5 parts of emulsifier and 8.5 parts of cosolvent were added into a jacketed reactor, heated at 80°C until melted, and then the dispersion was started. The mixture was stirred evenly at a speed of 1500 r / min, and the material temperature was maintained at 60°C. The peristaltic pump was started, and 46.5 parts of aramid fiber aqueous solution were added dropwise at a speed of 2 ml / min. After the addition was completed, the mixture was stirred at a speed of 1500 r / min for 30 min, and the aramid fiber-modified epoxy emulsion was obtained after filtration.
[0065] Preparation of aramid fiber composite modified waterborne epoxy coating:
[0066] The amount of each component is as shown in the following table, weigh 1 accurately, add it to the dispersion tank, add 2-5 in sequence while stirring, and disperse at 1000rpm for 5 minutes. Add 6-14 in sequence while stirring, disperse at 1000rpm for 10 minutes, add zirconium beads, grind at high speed to a fineness of less than 25 microns, filter and set aside to obtain component A. Weigh 15 and 16 accurately, mix and stir evenly, filter, and obtain component B. Mix and stir components A and B evenly in a mass ratio of 100:32, filter, and obtain a water-based epoxy coating composite modified with aramid fiber.
[0067] Example 4
[0068] Prepare the emulsifier:
[0069] Weigh 2 parts of E51 epoxy resin, 1 part of 4000 polyethylene glycol, 0.5 parts of 4000 molecular weight polyetheramine, and 0.01 parts of tetrafluoroboric acid; add E51 epoxy resin and polyethylene glycol into a reactor, heat to 100°C, add all the tetrafluoroboric acid dropwise within 1 hour, keep the reaction at 100°C for 3 hours, add polyetheramine, heat to 120°C, and continue the reaction for 4 hours to obtain a non-ionic emulsifier for polyetheramine grafted modified epoxy resin.
[0070] Preparation of aramid fiber modified epoxy emulsion:
[0071]
[0072]
[0073] (1) By weight, 8 parts of aramid fiber, 50 parts of water, and 0.8 parts of dispersant are weighed, condensed water is turned on, and dispersed at 25° C. and 3000 r / min for 4 hours to obtain a dispersed aramid fiber aqueous solution, wherein the aramid fiber is para-aramid fiber.
[0074] (2) In parts by weight, 40 parts of E20 epoxy resin, 5 parts of emulsifier and 8 parts of cosolvent were added into a jacketed reactor, heated at 80°C until melted, and then the dispersion was started. The mixture was stirred evenly at a speed of 1500 r / min, and the material temperature was maintained at 60°C. The peristaltic pump was started, and 60 parts of aramid fiber aqueous solution were added dropwise at a speed of 2 ml / min. After the addition was completed, the mixture was stirred at a speed of 1500 r / min for 30 min, and the aramid fiber-modified epoxy emulsion was obtained after filtration.
[0075] Preparation of aramid fiber composite modified waterborne epoxy coating:
[0076] The amount of each component is as shown in the following table, weigh 1 accurately, add it to the dispersion tank, add 2-5 in sequence while stirring, and disperse at 1000rpm for 5 minutes. Add 6-14 in sequence while stirring, disperse at 1000rpm for 10 minutes, add zirconium beads, grind at high speed to a fineness of less than 25 microns, filter and set aside to obtain component A. Weigh 15 and 16 accurately, mix and stir evenly, filter, and obtain component B. Mix and stir components A and B evenly in a mass ratio of 100:32, filter, and obtain a water-based epoxy coating composite modified with aramid fiber.
[0077]
[0078]
[0079] Comparative Example 1
[0080] The difference from Example 2 is that aramid fiber is not added, and the rest of the composition and preparation process are exactly the same.
[0081] Performance Testing
[0082] The adhesion is determined by cross-cut test according to GB / T 9286-2021;
[0083] Determine the water resistance of paint film according to GB / T 1733-1993;
[0084] Determination of the salt spray resistance of the paint film according to GB / T 1771-2007;
[0085] Determine the impact resistance of paint film according to GB / T 1732-1993;
[0086] The paint film hardness was measured in accordance with GB / T 6739-2006.
[0087] Table 1 shows the experimental data under different implementation schemes.
[0088] The test results are shown in Table 1 below:
[0089] Test items Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Appearance Flat, smooth Flat, smooth Flat, smooth Surface wrinkles Flat, smooth Adhesion Level 0 Level 0 Level 0 Level 0-1 Level 0 Water resistance 10 days 15 days 15 days 3 days 7 days Salt spray resistant 400h 800h 776h 344h 320h Shock resistance >50cm >60cm >60cm >40cm >50cm hardness H 2H 2H HB HB
[0090] As described in the above table, it can be seen from the comparison between the embodiment and the comparative example that the technical solution of the present invention is adopted to complete the dispersion of aramid fiber in water-based epoxy emulsion and avoid the occurrence of agglomeration. In Example 2, the water-based epoxy coating modified by aramid fiber has water resistance ≥15 days, salt spray resistance ≥800h, and impact resistance>60cm, and the performance is better than that of comparative example 1. This is because aramid fiber, as a reinforcing material, can fill the pinholes and defects that appear in the coating after the film is solidified due to water evaporation, and shield the entry of corrosive media. Secondly, due to the multi-layer coating of aramid fiber, the external corrosive medium needs a longer time to pass through the protective film of aramid fiber, which increases the difficulty of corrosive liquid penetrating into the surface of the metal substrate. However, as the amount of aramid fiber added gradually increases, the appearance of the coating appears wrinkled, and the adhesion, salt spray resistance and other properties also decrease. This is because when the addition amount is too high, too much aramid fiber is difficult to disperse, and the excess aramid fiber will always be free outside the system, causing certain damage to the performance of the coating.
[0091] As shown in the figure, Figure 2 This is the emulsifier spectrum of polyetheramine grafted modified epoxy resin, the characteristic peak of epoxy group is 830cm -1 and 915cm -1 It also exists and retains the epoxy group, which has good compatibility with epoxy resin. In the later emulsion curing film forming process, it can participate in the curing film and increase the crosslinking density of the coating. The NH peak in polyetheramine is 3312cm -1 The absence of this indicates that the reaction is complete and has no effect on the later storage stability.
[0092] The description of the above embodiments is only used to help understand the method of the present invention and its core idea. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features disclosed herein.
Claims
1. A aramid fiber composite modified waterborne epoxy coating, characterized in that: The raw material composition comprises two components, A and B, wherein the A component comprises, by weight, 40-60 parts of aramid fiber modified epoxy emulsion, 10-70 parts of pigments and fillers, 0.1-3 parts of anti-flash rust agent, 0.1-5 parts of dispersant, 2-3 parts of film-forming aid, 1-3 parts of defoamer, 1-3 parts of thickener, 1-2 parts of wetting agent, and 10-50 parts of water; wherein the B component comprises, by weight, 10-40 parts of curing agent and 5-20 parts of propylene glycol methyl ether; the mass ratio of the A and B components is 100:30-40; The aramid fiber modified epoxy emulsion is prepared according to the following method: (1) Add 1-10 parts of aramid fiber, 0.1-1 parts of dispersant, and 50-90 parts of water into a jacketed reactor, open condensation water, and disperse at 25° C. and 2000-4500 r / min for 2-6 hours to obtain a dispersed aramid fiber aqueous solution; (2) Add 40-60 parts of epoxy resin, 4-8 parts of emulsifier, and 6-12 parts of cosolvent into a jacketed reactor, heat to 60-80°C until melted, start dispersion, stir evenly at a speed of 1000-2000 r / min, maintain the material temperature at 60-65°C, start the peristaltic pump, and add 30-60 parts of aramid fiber aqueous solution at a speed of 1-2 ml / min. After the addition is completed, stir at a speed of 1000-1500 r / min for 15-30 minutes, and obtain the aramid fiber modified epoxy emulsion after filtering.
2. The aramid fiber composite modified waterborne epoxy coating according to claim 1, characterized in that: The epoxy resin is selected from bisphenol A epoxy resin.
3. The aramid fiber composite modified waterborne epoxy coating according to claim 1, characterized in that: The epoxy resin is selected from one or more of E51, E44 and E20 epoxy resins.
4. The aramid fiber composite modified waterborne epoxy coating according to claim 1, characterized in that: The aramid fiber is para-aramid fiber.
5. The aramid fiber composite modified waterborne epoxy coating according to claim 1 or 4, characterized in that: The diameter of the aramid fiber is between 10-100 nm.
6. The aramid fiber composite modified waterborne epoxy coating according to claim 1, characterized in that: The emulsifier is a non-ionic emulsifier of polyetheramine grafted modified epoxy resin, and the preparation method is as follows: Weigh 2-5 parts of E51 epoxy resin, 1-5 parts of polyethylene glycol with a molecular weight of 3500-6000, 0.5-2 parts of polyetheramine with a molecular weight of 2000-4000, and 0.01-0.03 parts of tetrafluoroboric acid by weight; add E51 epoxy resin and polyethylene glycol into a reactor, heat to 100-110° C., drop all of tetrafluoroboric acid within 1-2 hours, keep warm at 100-110° C. for reaction for 3-4 hours, add polyetheramine, heat to 120-140° C., continue to react for 4-6 hours, and obtain a non-ionic emulsifier for polyetheramine grafted modified epoxy resin.
7. The aramid fiber composite modified waterborne epoxy coating according to claim 1, characterized in that: The cosolvent is selected from one or more of propylene glycol methyl ether, propylene glycol butyl ether and acetone; The pigment filler is selected from one or more of titanium dioxide, talcum powder, barium sulfate, iron red, zinc phosphate, strontium chrome yellow, and mica powder; The dispersant is selected from one or more of dodecyl sulfonates, alkyl alcohol polyoxyethylene ethers, polyacrylates, and polycarboxylates; The film-forming aid is selected from one or more of dipropylene glycol methyl ether, propylene glycol methyl ether, and dipropylene glycol butyl ether; The defoamer is selected from one or more of polyether block, silicone, and mineral oil; The thickener is selected from one or more of cellulose, polyacrylic acid, inorganic thickener, and polyurethane; The curing agent is selected from one or more of Huntsman 3986, Hexion 6870, and Allnex 613W.
8. The aramid fiber composite modified waterborne epoxy coating according to claim 1, characterized in that: The flash rust preventer is one or more of CK-20, CK-35, and HY-72; the wetting agent is one or more of TEGO-245, TEGO-270, and TEGO280.
9. The method for preparing the aramid fiber composite modified waterborne epoxy coating according to claim 1, characterized in that: The specific steps include: S1: Preparation of component A: Add aramid fiber modified epoxy emulsion, pigment filler, anti-rust agent, dispersant, film-forming aid, defoamer, thickener, wetting agent and water into the reactor according to the proportion, grind to a fineness of less than 25 μm, filter the material and obtain component A; S2: Preparation of component B: Add curing agent and propylene glycol methyl ether into the reactor according to the ratio, stir and mix at a speed of 500-1000 rpm / min, filter the material to obtain component B; S3: Component A and component B are mixed evenly in a mass ratio of 100:30-40, and filtered to obtain an aramid fiber composite modified water-based epoxy coating.
Citation Information
Patent Citations
Method of using block polyether to prepare epoxy emulsion
CN101585922A
Aramid nano-fiber corrosion-resistant environmentally-friendly coating material and preparation method thereof
CN106336775A
Preparation method of aqueous epoxy basalt scale anticorrosive paint
CN106978041A
Waterborne fluorocarbon insulation paint modified by aramid fibers and preparation method thereof
CN109401462A