High-thermal-conductivity insulating nano functional coating as well as preparation method and application thereof
By combining the modified resin and the modified boron nitride nanosheets, an aqueous coating is formed, which solves the problem of insufficient thermal conductivity of the aluminum alloy insulation layer, and achieves a highly thermal conductivity and environmentally friendly coating, which is suitable for the heat dissipation needs of electronic equipment.
Patent Information
- Application Number
- CN202411078343.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the thermal conductivity of the insulating layer on the surface of the aluminum alloy is insufficient, resulting in unsatisfactory heat dissipation performance. The anodizing method has problems such as single color, difficulty in repairing and easy corrosion. Nanofunctional coatings also have shortcomings in hardness and wear resistance. And the filler has poor compatibility with the matrix.
Using a combination of modified resin dispersion and modified boron nitride nanosheets, the water-based coating is formed by self-made modified resin and modified boron nitride nanosheets to ensure uniform distribution of nanofillers, forming a continuous thermal conductivity network, and improving the coating. Thermal conductivity and the agglomeration of polymer particles is controlled by hydrophilic groups, which improves the fluidity and density of the coating.
It realizes a dense, uniform and flat coating, improves the thermal conductivity of the insulating layer, meets the high requirements of modern electronic equipment for heat dissipation and insulation performance, and is an environmentally friendly water-based coating, suitable for industrial production.
Smart Images

Figure BDA0004983002750000081 
Figure BDA0004983002750000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coatings, and in particular relates to a high thermal conductivity insulating nano functional coating and a preparation method thereof. Background Art
[0002] With the continuous improvement of integration technology and microelectronic packaging technology, the size of electronic components has been miniaturized and the power has increased, making it difficult to quickly dissipate the heat generated during operation, resulting in the continuous increase in the operating temperature of highly integrated electronic devices, which not only causes energy consumption, but also seriously affects their service life. Among them, the heat dissipation performance of the packaging substrate has the greatest impact on the heat dissipation effect of electronic devices. At present, packaging substrates are mostly prepared using metal substrates. Aluminum alloy has become the preferred material for packaging substrates in the current electronic and electrical industry due to its high specific strength, excellent thermal conductivity, and good decorative properties. Although aluminum alloy has excellent thermal conductivity, the insulating layer on the surface of the aluminum alloy in the packaging substrate generally has insufficient thermal conductivity, resulting in unsatisfactory heat dissipation performance.
[0003] The anodizing method can prepare a dense crystalline aluminum oxide coating on the surface of aluminum alloy, which is expected to improve the breakdown voltage and thermal conductivity of the insulating layer and meet the development requirements of the electronic and electrical industry. However, this method has the following disadvantages: First, the color selectivity is relatively single; second, in the early stage of anodizing of aluminum alloy, the dense and non-porous oxide coating is thin and easily scratched due to collision or scratching. Since anodizing relies on electrolysis, it is more difficult to repair scratches; third, as anodizing proceeds, the oxide coating will further thicken. At this time, under the influence of stress and volume expansion in the coating, microcracks will appear in the coating. Due to the increase of local current in the microcracks, the dissolution rate of the oxide film at this location increases, resulting in micropores. The presence of micropores makes it easy to be penetrated by corrosive substances in a corrosive environment, eventually causing pitting of the aluminum alloy.
[0004] Nano-functional coatings are a type of coating with special functions prepared using nanotechnology. They can avoid the shortcomings of the above-mentioned anodizing process, such as single color, difficulty in repair, and pitting corrosion, as much as possible in metal surface treatment. Their relatively simple preparation process can also achieve energy conservation and emission reduction. However, there is a certain degree of difficulty in introducing nanomaterials into the coating system, mainly because the coating system is diversified and compatibility has become a difficulty. In addition, they still have some shortcomings in hardness and wear resistance.
[0005] Patent CN110964228B uses an in-situ growth method to prepare heterogeneous structure thermal conductive filler silicon carbide-boron nitride nanosheets, and reduces the interface thermal resistance introduced by directly doped boron nitride nanosheets and silicon carbide through the close bonding force generated by chemical bonds, constructs an efficient thermal conductive path in the epoxy resin, and achieves high thermal conductivity and high performance of epoxy resin composite materials; however, since the coating pays more attention to the compatibility between the filler and the matrix than the composite material, the compatibility of the filler and the epoxy resin matrix in this method needs to be improved. Patent CN116285229B treats hexagonal boron nitride nanosheets by self-polymerizing dopamine, realizes the stripping and modification of hexagonal boron nitride nanosheets, and then strengthens the compatibility with epoxy resin by grafting dopamine. The dopamine used in this method is relatively expensive and is not suitable for large-scale industrial production. Summary of the invention
[0006] In order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a high thermal conductivity insulating nano-functional coating and a preparation method and application thereof. The coating can obtain a dense, uniform and smooth coating, and the nano-filler can form a continuous thermal conductive network in the coating, which is expected to improve the thermal conductivity of the insulating layer and meet the development requirements of the electronic and electrical industry.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is:
[0008] The first aspect of the present invention provides a high thermal conductivity insulating nano functional coating, which comprises the following raw materials by weight: 50-70 parts of a modified resin dispersion, 1-5 parts of a defoaming agent, 2-4 parts of triethylamine and 40-50 parts of a modified boron nitride nanosheet dispersion;
[0009] The molecular formula of the modified resin in the modified resin dispersion is:
[0010] NCO-(R 1 -NHCOOCH 2 C(CH 3 COOH)CH 2 OOCNH-R 1 -N(CH 2 COOCH)-R 2 -(CH2COOCH)NR 1 )-NCO;
[0011] R 1 =-(S 1 -NH-COO-CH 2 CH 2 CH 2 CH 2 -OOC-NH-S 1 ) a -;
[0012] R 2 =-CH 2 O-(C 6 H 4 C(CH 3 ) 2 C 6 H 4 CH 2 CH(OH)CH 2 ) b -OC 6 H 4 C(CH 3 ) 2 C 6 H 4 OCH 2 -;
[0013] S 1 =-(C 6 H 3 (CH 3 )-NHCOO-S 2 -OOCNH) c -C 6 H 3 (CH 3 )-;
[0014] S2 is a polybutadiene chain.
[0015] In some embodiments, the preparation steps of the modified resin dispersion are as follows:
[0016] S1, stirring toluene diisocyanate, hydroxyl-terminated polybutadiene and a catalyst at 70-80° C. for 60-80 minutes under nitrogen protection to obtain a prepolymer 1;
[0017] S2, stirring dimethylolpropionic acid, epoxy resin, acetone and hydroxypropyl methacrylate to obtain a mixed solution;
[0018] S3, stirring the prepolymer 1 of step S1, 1,4-butanediol and acetone for 50-70 minutes to obtain prepolymer 2;
[0019] S4, take the prepolymer 2 of step S3, heat it to 140-160°C, add all the mixed solutions of step S2, keep it warm for 4-6 hours, then cool it to 60-70°C to obtain a modified resin, then slowly add deionized water at a stirring speed of 700-900 rpm, stir for 40-60 minutes, and obtain the modified resin dispersion.
[0020] In some embodiments, the hydroxy-terminated polybutadiene in step S1 has an average functionality of 2-3 and a number average molecular weight of 2500-3000.
[0021] In some embodiments, the molar ratio of toluene diisocyanate to hydroxyl-terminated polybutadiene in the prepolymer 1 in step S1 is (1.52-1.7):1.
[0022] In some embodiments, the catalyst in step S1 is one or more of organotin, organoaluminum or organozinc.
[0023] In some embodiments, the molar ratio of prepolymer 1 to 1,4-butanediol in step S3 is 1:(0.53-0.58).
[0024] High thermal conductivity insulating nano-functional coatings are of great significance for meeting the high requirements of modern electronic equipment for heat dissipation and insulation performance. Taking environmental protection needs into consideration, the present invention uses water as a dispersion medium and forms polymer nanoparticles with narrow and uniform particle size distribution through a self-made modified resin dispersion. The polymer nanoparticles are matched with the size of modified boron nitride nanosheets to facilitate close contact between the two parties, satisfying the two conditions of uniform distribution of nanofillers in the polymer and close contact between polymer particles and nanofillers, so that the water-based coating can obtain a dense, uniform and smooth coating after water evaporation, and the nanofillers can form a continuous thermal conductive network in the coating to improve the thermal conductivity of the coating.
[0025] Due to the high-temperature use environment caused by high power, the cured resin will become hard due to oxidative degradation if placed under such conditions for a long time, and when stress is applied to the installed circuit board, it is easy to crack and deform, resulting in reduced application reliability. In the preparation process of the modified resin dispersion, since the hydrophilic monomer chain extender needs to be added in the prepolymerization stage, it brings certain restrictions to the structure of the main chain, so that the polymer nanoparticles will form agglomerates, affecting the coating. The present invention avoids the formation of agglomerates of polymer particles by specifically selecting the type of hydrophilic group and its amount in this system, improves the fluidity of the coating, and enables the polymer particles to diffuse and fuse with each other during the gradual evaporation of water, overcomes the brush marks and stitch marks produced during the coating process of the water-based coating, and the orange peel and sagging phenomena produced during the curing process, and forms a dense and uniform coating film.
[0026] In some embodiments, the preparation steps of the modified boron nitride nanosheet dispersion are as follows:
[0027] The boron nitride nanosheets, hydrazine carbonate and deionized water are first stirred at a rotation speed of 300-400 rpm for 40-60 minutes, and then dispersed by 10-20 kHz ultrasound for 10-20 minutes to obtain a modified boron nitride nanosheet dispersion.
[0028] In some embodiments, the mass ratio of the boron nitride nanosheets to hydrazine carbonate is 1:(2-3).
[0029] The second aspect of the present invention provides a method for preparing a high thermal conductive insulating nano functional coating, the preparation steps are as follows:
[0030] The modified boron nitride nanosheet dispersion and the modified resin dispersion are stirred at 60-70°C and 800-1000 rpm for 70-90 minutes, then cooled to 40-50°C, the speed is reduced to 400-600 rpm, triethylamine is added and stirred for 40-60 minutes, and finally a defoamer is added at room temperature and stirred for 10-30 minutes to obtain the high thermal conductive insulating nano functional coating.
[0031] A third aspect of the present invention provides an application of a high thermal conductivity insulating nano functional coating in a packaging substrate.
[0032] Boron nitride nanosheets are usually directly added to organic solvents or water, and a dispersion is prepared by ultrasonic action. Since the coating of the present invention is an environmentally friendly water-based coating, and the stability and dispersibility of the aqueous dispersion of boron nitride nanosheets are poor, the present invention modifies the boron nitride nanosheets to obtain a stable dispersion that is not easy to agglomerate, and the groups on the modified boron nitride nanosheets can react with -NCO in the modified resin dispersion, so that the polymer particles can be close to the nanosheets, and the nanosheets and the polymer are closely stacked, so that the obtained coating is dense, uniform and smooth, and the nanosheets can form a continuous thermal conductive network in the coating.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. The present invention provides a high thermal conductivity insulating nano-functional coating that can meet the high requirements of modern electronic equipment for heat dissipation and insulation performance.
[0035] 2. The high thermal conductivity insulating nano-functional coating provided by the present invention is an environmentally friendly water-based coating. By making a self-made modified resin dispersion and modified boron nitride nanosheets, the water-based coating can obtain a dense, uniform and smooth coating after the water evaporates, and the nanofiller can form a continuous thermal conductive network in the coating to improve the thermal conductivity of the coating.
[0036] 3. In the preparation process of the modified resin dispersion, the present invention avoids the formation of polymer particles agglomerates by regulating the hydrophilic groups, and enables the chains of the polymer particles to diffuse and fuse with each other during the gradual evaporation of water, thereby forming a dense and uniform coating film. DETAILED DESCRIPTION
[0037] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following examples and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0038] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments are described as follows:
[0039] Hydroxyl-terminated polybutadiene was purchased from Shandong Zibo Qilong Chemical Co., Ltd., with a functionality of 2.2 and Mn = 2700;
[0040] Epoxy resin was purchased from Guangzhou Dongfeng Chemical Industry Co., Ltd., model E20;
[0041] Boron nitride nanosheets were purchased from Suzhou Napu Material Technology Co., Ltd.
[0042] Preparation Example 1
[0043] The preparation steps of modified resin dispersion-A are as follows:
[0044] S1. Under nitrogen protection and 75°C, 3.2 mol of toluene diisocyanate, 2 mol of hydroxy-terminated polybutadiene and 0.1 mol of dibutyltin dilaurate were stirred for 70 min to obtain prepolymer 1.
[0045] S2, 1.1 mol of dimethylolpropionic acid, 1.2 mol of epoxy resin, 300 mL of acetone and 0.2 mol of hydroxypropyl methacrylate were stirred to obtain a mixed solution;
[0046] S3, 8 mol of the prepolymer 1 prepared in step S1, 4.4 mol of 1,4-butanediol and 1300 mL of acetone were stirred for 60 min to obtain a prepolymer 2;
[0047] S4, take 3 mol of prepolymer 2 from step S3, heat it to 150°C, add all the mixed solution from step S2, keep it warm for 5 hours, then cool it to 65°C to obtain a modified resin, and then heat it at 800rp m At a stirring speed of , deionized water is slowly added, the deionized water accounting for 30% of the total mass, and after stirring for 50 minutes, the modified resin dispersion-A is obtained.
[0048] Preparation Example 2
[0049] The preparation steps of modified resin dispersion-B are as follows:
[0050] The difference between this preparation example and preparation example 1 is that the amount of terminal hydroxyl polybutadiene used in step S1 is 3 mol.
[0051] Preparation Example 3
[0052] The preparation steps of modified resin dispersion-C are as follows:
[0053] The difference between this preparation example and preparation example 1 is that the amount of terminal hydroxyl polybutadiene used in step S1 is 3.6 mol.
[0054] Preparation Example 4
[0055] The preparation steps of modified resin dispersion-D are as follows:
[0056] The difference between this preparation example and preparation example 1 is that the amount of 1,4-butanediol used in step S3 is 4 mol.
[0057] Preparation Example 5
[0058] The preparation steps of modified resin dispersion-E are as follows:
[0059] The difference between this preparation example and preparation example 1 is that the amount of 1,4-butanediol used in step S3 is 4.6 mol.
[0060] Preparation Example 6
[0061] The preparation steps of modified boron nitride nanosheet dispersion-A are as follows:
[0062] 10 g of boron nitride nanosheets, 25 g of hydrazine carbonate and 80 g of deionized water were first stirred at a rotation speed of 650 rpm for 50 min, and then dispersed by 12 kHz ultrasound for 15 min to obtain a modified boron nitride nanosheet dispersion-A.
[0063] Preparation Example 7
[0064] The preparation steps of modified boron nitride nanosheet dispersion-B are as follows:
[0065] The difference between this preparation example and preparation example 6 is that the amount of hydrazine carbonate used is 15 g.
[0066] Preparation Example 8
[0067] The preparation steps of modified boron nitride nanosheet dispersion-C are as follows:
[0068] The difference between this preparation example and preparation example 6 is that the amount of hydrazine carbonate used is 35 g.
[0069] Preparation Example 9
[0070] The preparation steps of boron nitride nanosheet dispersion are as follows:
[0071] The difference between this preparation example and preparation example 6 is that the amount of hydrazine carbonate used is 0 g.
[0072] Example 1
[0073] A high thermal conductivity insulating nano functional coating comprises the following raw materials in parts by weight: 60 parts of modified resin dispersion-A, 3 parts of tributyl phosphate, 3 parts of triethylamine and 45 parts of modified boron nitride nano sheet dispersion-A.
[0074] The preparation method of the high thermal conductive insulating nano functional coating in this embodiment comprises the following steps:
[0075] The modified boron nitride nanosheet dispersion-A and the modified resin dispersion-A were stirred at 65°C and 900 rpm for 80 minutes, then cooled to 45°C, the speed was reduced to 500 rpm, triethylamine was added and stirred for 50 minutes, and finally tributyl phosphate was added at room temperature and stirred for 20 minutes to obtain the high thermal conductive insulating nano functional coating.
[0076] Example 2
[0077] A high thermal conductivity insulating nano functional coating comprises the following raw materials in parts by weight: 55 parts of modified resin dispersion-A, 1 part of tributyl phosphate, 1 part of triethylamine and 40 parts of modified boron nitride nano sheet dispersion-A.
[0078] The preparation method of the high thermal conductive insulating nano functional coating in this embodiment comprises the following steps:
[0079] The modified boron nitride nanosheet dispersion-A and the modified resin dispersion-A were stirred at 60°C and 800 rpm for 90 minutes, then cooled to 40°C, the speed was reduced to 400 rpm, triethylamine was added and stirred for 40 minutes, and finally tributyl phosphate was added at room temperature and stirred for 10 minutes to obtain the high thermal conductive insulating nano functional coating.
[0080] Example 3
[0081] A high thermal conductivity insulating nano functional coating comprises the following raw materials in parts by weight: 65 parts of modified resin dispersion-A, 4 parts of defoamer, 4 parts of triethylamine and 50 parts of modified boron nitride nano sheet dispersion-A.
[0082] The preparation method of the high thermal conductive insulating nano functional coating in this embodiment comprises the following steps:
[0083] The modified boron nitride nanosheet dispersion-A and the modified resin dispersion-A were stirred at 70°C and 1000 rpm for 70 minutes, then cooled to 50°C, the speed was reduced to 600 rpm, triethylamine was added and stirred for 60 minutes, and finally tributyl phosphate was added at room temperature and stirred for 30 minutes to obtain the high thermal conductive insulating nano functional coating.
[0084] Example 4
[0085] This embodiment provides a high thermal conductivity insulating nano-functional coating and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified resin dispersion-A in the raw material is replaced by an equal amount of modified resin dispersion-B.
[0086] Example 5
[0087] This embodiment provides a high thermal conductivity insulating nano-functional coating and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified resin dispersion-A in the raw material is replaced by an equal amount of modified resin dispersion-C.
[0088] Example 6
[0089] This embodiment provides a high thermal conductivity insulating nano-functional coating and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified resin dispersion-A in the raw material is replaced by an equal amount of modified resin dispersion-D.
[0090] Example 7
[0091] This embodiment provides a high thermal conductivity insulating nano-functional coating and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified resin dispersion-A in the raw material is replaced by an equal amount of modified resin dispersion-E.
[0092] Example 8
[0093] This embodiment provides a high thermal conductivity insulating nano-functional coating and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified boron nitride nanosheet dispersion-A in the raw material is replaced by an equal portion of modified boron nitride nanosheet dispersion-B.
[0094] Example 9
[0095] This embodiment provides a high thermal conductivity insulating nano-functional coating and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified boron nitride nanosheet dispersion-A in the raw material is replaced by an equal portion of modified boron nitride nanosheet dispersion-C.
[0096] Comparative Example 1
[0097] This comparative example provides a high thermal conductivity insulating nano-functional coating and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified boron nitride nanosheet dispersion-A in the raw material is replaced by an equal portion of boron nitride nanosheet dispersion.
[0098] Performance Testing
[0099] Experimental sample preparation:
[0100] The nano-functional coatings of each embodiment were coated on an aluminum plate to prepare a sample, and the coating thickness was 1 mm. After the coating was completely cured at 60° C., the sample was subjected to the following test:
[0101] Thermal conductivity test:
[0102] The thermal conductivity of the sample coating was measured using a thermal conductivity analyzer. The instrument used was TPS2500S from Swedish Hot Disk Company, which complies with the "GB T32064-2015" standard. The transient heat source method was used to measure the thermal conductivity of the coating, and the probe model was 5465.
[0103] Table 1 Performance test results
[0104]
[0105]
[0106] It can be seen from the data in Table 1 that the high thermal conductive insulating nano-functional coatings of Examples 1-3 have excellent thermal conductivity; it can be seen from Examples 1 and 4-7 that the preparation process of the modified resin dispersion has a certain influence on the thermal conductivity effect, and the possible reason is that its preparation process affects the size compatibility of the polymer nanoparticles and the size of the modified boron nitride nanosheets; it can be seen from Example 1 and Examples 8-9 and Comparative Example 1 that the modified boron nitride nanosheets can effectively improve the thermal conductivity, and the possible reason is that the modified boron nitride nanosheet dispersion is more stable and uniform, and can be tightly stacked with the polymer particles, so that the obtained coating is dense, uniform and smooth, forming a continuous thermal conductive network in the coating.
[0107] The embodiments described above do not impose any form of limitation on the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A high thermal conductivity insulating nano functional coating, characterized in that: The invention comprises the following raw materials by weight: 50-70 parts of modified resin dispersion, 1-5 parts of defoamer, 2-4 parts of triethylamine and 40-50 parts of modified boron nitride nanosheet dispersion; The molecular formula of the modified resin in the modified resin dispersion is: NCO-(R1-NHCOOCH2C(CH3COOH)CH2OOCNH-R1-N(CH2COOCH)-R2-(CH 2COOCH)N-R1)-NCO; R1=-(S1-NH-COO-CH2CH2CH2CH2-OOC-NH-S1) a -; R2=-CH2O-(C6H4C(CH3)2C6H4CH2CH(OH)CH2) b -OC6H4C(CH3)2C6H4OCH2-; <h2 style=";text-align:left;direction:ltr">S1 = (C6H3(CH3)-NHCOO-S2-OOCNH)<h2 style=";text-align:left;direction:ltr"> c <h2 style=";text-align:left;direction:ltr"> -C6H3(CH3)-; S2 is a polybutadiene chain.
2. The high thermal conductivity and insulation nano-functional coating according to claim 1, characterized in that: The preparation steps of the modified resin dispersion are as follows: S1, stirring toluene diisocyanate, hydroxyl-terminated polybutadiene and a catalyst at 70-80° C. for 60-80 minutes under nitrogen protection to obtain a prepolymer 1; S2, stirring dimethylolpropionic acid, epoxy resin, acetone and hydroxypropyl methacrylate to obtain a mixed solution; S3, stirring the prepolymer 1 of step S1, 1,4-butanediol and acetone for 50-70 minutes to obtain prepolymer 2; S4, take the prepolymer 2 of step S3, heat it to 140-160°C, add all the mixed solutions of step S2, keep it warm for 4-6 hours, then cool it to 60-70°C to obtain a modified resin, then slowly add deionized water at a stirring speed of 700-900 rpm, stir for 40-60 minutes, and obtain the modified resin dispersion.
3. The high thermal conductivity insulating nano functional coating according to claim 2, characterized in that: The average functionality of the hydroxy-terminated polybutadiene in step S1 is 2-3, and the number average molecular weight is 2500-3000.
4. The high thermal conductivity insulating nano functional coating according to claim 3, characterized in that: In the step S1, the molar ratio of toluene diisocyanate to terminal hydroxyl polybutadiene in the prepolymer 1 is (1.52-1.7):
1.
5. The high thermal conductivity and insulation nano-functional coating according to claim 2, characterized in that: The catalyst in step S1 is one or more of organic tin, organic aluminum or organic zinc.
6. The high thermal conductivity insulating nano functional coating according to claim 2, characterized in that: In the step S3, the molar ratio of the prepolymer 1 to 1,4-butanediol is 1:(0.53-0.58).
7. The high thermal conductivity and insulation nano-functional coating according to claim 1, characterized in that: The preparation steps of the modified boron nitride nanosheet dispersion are as follows: The boron nitride nanosheets, hydrazine carbonate and deionized water are first stirred at a rotation speed of 300-400 rpm for 40-60 minutes, and then dispersed by 10-20 kHz ultrasound for 10-20 minutes to obtain a modified boron nitride nanosheet dispersion.
8. The high thermal conductivity and insulation nano-functional coating according to claim 7, characterized in that: The mass ratio of the boron nitride nanosheets to hydrazine carbonate is 1:(2-3).
9. A method for preparing the high thermal conductive insulating nano functional coating according to any one of claims 1 to 8, characterized in that: The preparation steps are as follows: The modified boron nitride nanosheet dispersion and the modified resin dispersion are stirred at 60-70°C and 800-1000 rpm for 70-90 minutes, then cooled to 40-50°C, the speed is reduced to 400-600 rpm, triethylamine is added and stirred for 40-60 minutes, and finally a defoamer is added at room temperature and stirred for 10-30 minutes to obtain the high thermal conductive insulating nano functional coating.
10. Use of the high thermal conductivity insulating nano-functional coating according to any one of claims 1 to 8 or the high thermal conductivity insulating nano-functional coating obtained by the preparation method according to claim 9 in a packaging substrate.
Citation Information
Patent Citations
A silicon carbide-boron nitride nanosheet heterogeneous filler and its preparation method, and an epoxy resin thermally conductive composite material and its preparation method.
CN110964228B
A ceramic toughening epoxy resin for halogen-free copper clad laminates and its preparation method
CN116285229B
Preparing method for high-temperature-resistant heat conducting water-based insulating paint
CN105838203A
Boron nitride nanosheet enhanced heat conductive insulating waterborne coating as well as preparation and use methods thereof
CN107641424A