Low-temperature fast-curing high-temperature-resistant electrical steel environment-friendly insulating material and preparation method and application thereof

By using a combination of polyimide resin and nano-scale curing agent in electrical steel insulating materials, combined with vacuum degassing treatment, the problems of high-temperature curing and environmental pollution are solved, and the insulation with fast low-temperature curing and high mechanical properties are achieved Material.

CN118931373AInactive Publication Date: 2024-11-12HUBEI WUZHOU NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411173623.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing electrical steel insulating materials consume long time, consume high energy and emit a large amount of VOC during high-temperature curing, resulting in environmental pollution.

Method used

The combination of polyimide resin, nano-scale curing agent, reaction accelerator, solvent and additive is used to spray degassing treatment through a vacuum degassing tower to reduce the curing temperature and time and reduce the emission of volatile organic compounds.

Benefits of technology

It significantly shortens the curing time of insulating materials, reduces VOC emissions, improves the mechanical properties of the materials, and solves the problems of long curing time and unenvironmental protection of traditional insulating coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931373A_ABST
    Figure CN118931373A_ABST
Patent Text Reader

Abstract

The invention discloses a low-temperature fast-curing high-temperature-resistant electrical steel environment-friendly insulating material and a preparation method and application thereof, and relates to the technical field of insulating materials. 10%-20% of a nanoscale curing agent; 1%-5% of a reaction accelerator; 5%-10% of a solvent; 5%-15% of an additive; the nanoscale curing agent comprises nano silicon dioxide, nano zinc oxide and nano aluminum oxide; the insulating material is obtained by spraying and degassing polyimide resin, a nanoscale curing agent, a reaction accelerator, a solvent and an additive in a vacuum degassing tower, the curing temperature of the insulating material is greatly reduced, the curing time of the insulating material is greatly shortened at the same temperature, the emission of volatile organic compounds of the insulating material is reduced by two thirds, and the service life of the insulating material is prolonged. The problems that a traditional insulating coating is long in curing time and not environmentally friendly are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of Internet of Things, and in particular to a low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material and a preparation method and application thereof. Background Art

[0002] The electrical steel insulation materials currently on the market mainly include the following components:

[0003] Resin matrix, commonly epoxy resin, polyester resin, etc., is used to provide basic insulation performance and mechanical strength;

[0004] Curing agent, used to help the resin matrix cure quickly at a certain temperature;

[0005] Fillers, such as graphite and alumina, are used to improve the high temperature resistance of insulating materials;

[0006] Additives, including stabilizers, anti-aging agents, etc., are used to improve the processing properties of materials and extend their service life;

[0007] Solvent, adjusts the processing viscosity of the material to ensure a smooth coating process;

[0008] Traditional electrical steel insulating materials usually need to be cured at higher temperatures, such as an insulating material and its preparation method and application in Chinese patent application with publication number CN115216081A and an insulating material and its preparation method and application in Chinese patent application with publication number CN118165392A. Such insulating materials take a long time to cure and have high energy consumption, which is not ideal in terms of production efficiency and energy consumption. During the high-temperature curing process, a large amount of VOCs will be emitted, causing very serious pollution to the environment. Summary of the invention

[0009] In order to overcome the above-mentioned technical problems, the purpose of the present invention is to provide a low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material and its preparation method and application, so as to solve the problem in the prior art that the existing insulating material has a high curing temperature and a long time, and a large amount of VOC is emitted during the high-temperature curing process, causing environmental pollution.

[0010] The purpose of the present invention can be achieved through the following technical solutions:

[0011] Specifically, the first aspect of the present invention provides a low-temperature, fast-curing, high-temperature resistant electrical steel environmentally friendly insulating material, the components of the insulating material by mass percentage include: polyimide resin, 60-80%; nano-scale curing agent, 10%-20%; reaction accelerator, 1%-5%; solvent, 5%-10%; additives, 5%-15%; the nano-scale curing agent includes nano-silicon dioxide, nano-zinc oxide and nano-aluminum oxide, the polyimide resin, nano-scale curing agent, reaction accelerator, solvent and additive are mixed in a mass ratio to form a mixture, and the mixture is added to a vacuum degassing tower for spray degassing treatment.

[0012] As a further solution of the present invention: the reaction accelerator is prepared by mixing one of dibutyltin dilaurate, tetrabutyl titanate, ferric acetylacetonate, zinc acetate bismuth trichloride or any combination thereof in any proportion.

[0013] As a further embodiment of the present invention: the solvent is an aqueous solvent, a bio-based solvent, a low-volatile organic solvent or an ionic liquid.

[0014] As a further solution of the present invention: the additives include toughening agents, plasticizers, flame retardants and antioxidants.

[0015] The second aspect of the present invention provides a method for preparing the above-mentioned low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material, comprising the following steps:

[0016] S1: Selecting polyimide resin, nano-scale curing agent, reaction accelerator, solvent and additive according to mass ratio;

[0017] S2: Add polyimide resin into a stirring kettle and stir at room temperature for 5-10 minutes;

[0018] S3: Add the nano-scale curing agent into the stirring kettle and stir at room temperature for 20-40 minutes;

[0019] S4: Add the reaction accelerator into the stirred tank and stir at room temperature for 30-50 minutes;

[0020] S5: Add the additive into the stirred tank and stir at room temperature for 40-60 minutes;

[0021] S6: Add the solvent into the stirred tank and stir for 10-20 min at room temperature to form a mixture;

[0022] S7: heating the mixture in the stirred tank to 40-60°C and then conveying it to a vacuum degassing tower;

[0023] S8: Control the vacuum degree in the vacuum degassing tower between 1.33 and 6.65 kPa by a vacuum pump;

[0024] S9: performing spray degassing treatment in a vacuum degassing tower, collecting the degassing mixture, and obtaining an insulating material.

[0025] As a further solution of the present invention: the vacuum degassing tower includes a fixed tower body, the top of the fixed tower body is connected to a sliding tower body, the top surface of the sliding tower body is connected to an input pipe and an outlet pipe, the input pipe is used to transport the mixture, the outlet pipe is used to connect to a vacuum pump, a liquid collecting mechanism is arranged inside the fixed tower body, the bottom surface of the fixed tower body is fixedly connected to a bottom track, and the bottom surface of the bottom track is slidably connected to a storage bucket.

[0026] As a further solution of the present invention: a receiving opening is provided on the top surface of the bottom track near the fixed tower body, and a sliding sealing plate is provided inside the bottom track.

[0027] As a further solution of the present invention: the liquid collecting mechanism includes a rebound cylinder, the interior of the rebound cylinder is fixedly connected with an impact cone, the side of the rebound cylinder is fixedly connected with a fixed foot, and the end of the fixed foot away from the rebound cylinder is fixedly connected to the inner wall of the fixed tower body.

[0028] As a further solution of the present invention: a spray head is fixedly connected to one end of the input pipe close to the inside of the sliding tower body, the diameter of the spray head is smaller than the maximum diameter of the impact cone, and the central axes of the rebound cylinder, the impact cone and the spray head coincide.

[0029] A third aspect of the present invention provides an application of the above-mentioned low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material in electrical steel.

[0030] Beneficial effects of the present invention:

[0031] 1. In the present invention, the insulating material is obtained by spraying and degassing polyimide resin, nano-scale curing agent, reaction accelerator, solvent and additive in a vacuum degassing tower, and the curing temperature is greatly reduced. At the same temperature, the curing time of the insulating material is greatly shortened, and the emission of volatile organic compounds of the insulating material is reduced by two-thirds, solving the problems of long curing time and environmental pollution of traditional insulating coatings.

[0032] 2. In the present invention, the spray head converts the mixture into drops and sprays them vertically. The sprayed drops will automatically fall on the inside of the rebound cylinder under the action of gravity. Since the diameter of the spray head is smaller than the maximum diameter of the impact cone, the rebound cylinder must be larger than the diameter of the spray head. Therefore, the mixture drops sprayed from the spray head can be completely received. In the process of the drops falling in the fixed tower body and the sliding tower body, since the fixed tower body and the sliding tower body are in a negative pressure state, the gas in the drops will inevitably expand and be discharged, thereby achieving a degassing effect, removing the gas in the drops to the greatest extent, thereby enhancing the mechanical properties of the obtained insulating material. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The present invention will be further described below in conjunction with the accompanying drawings.

[0034] Figure 1 This is a flow chart of the preparation method of the low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material of the present invention;

[0035] Figure 2 It is a structural schematic diagram of the vacuum degassing tower in the present invention;

[0036] Figure 3 is a cross-sectional view of a vacuum degassing tower in the present invention;

[0037] Figure 4 It is a structural schematic diagram of the liquid collecting mechanism in the present invention;

[0038] Figure 5 It is a cross-sectional view of the liquid collecting mechanism in the present invention.

[0039] In the figure: 1. fixed tower body; 2. sliding tower body; 21. sliding cylinder; 3. input pipe; 31. sprinkler head; 4. air outlet pipe; 5. bottom track; 51. sealing plate; 52. storage port; 6. storage barrel; 7. liquid collecting mechanism; 71. rebound cylinder; 72. impact cone; 73. fixed foot. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] Example 1

[0042] like Figure 1 and Figure 4 As shown, the present invention discloses a low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material, the mass percentage of the insulating material comprises: polyimide resin, 70%; nano silicon dioxide, 12%; dibutyltin dilaurate, 3%; aqueous solvent, 7%; additives, 8%;

[0043] The polyimide resin, nano-silicon dioxide, dibutyltin dilaurate, aqueous solvent and additives are mixed in a mass ratio to form a mixture, and the mixture is added to a vacuum degassing tower for spray degassing. The specific preparation process of the insulating material includes the following steps:

[0044] S1: Select polyimide resin, nano-silicon dioxide, dibutyltin dilaurate, aqueous solvent and additives according to the mass ratio, for example, 7.0 kg of polyimide resin, 1.2 kg of nano-silicon dioxide, 0.3 kg of dibutyltin dilaurate, 0.7 kg of aqueous solvent and 0.8 kg of additives in total.

[0045] S2: First, add 7.0 kg of polyimide resin into a stirring kettle. The specification and type of the stirring kettle are adaptively selected by those skilled in the art according to the preparation process of the insulating material. Stir at room temperature for 8 minutes.

[0046] S3: Add 1.2 kg of nano-silicon dioxide into the stirring kettle and stir at room temperature for 30 minutes.

[0047] S4: Then, 0.3 kg of dibutyltin dilaurate was added into the stirred tank and stirred at room temperature for 40 min.

[0048] S5: Additives include tougheners, plasticizers, flame retardants and antioxidants. The total weight of the tougheners, plasticizers, flame retardants and antioxidants is 0.8 kg. The mass ratio of the tougheners, plasticizers, flame retardants and antioxidants is 1:1:1:1. Those skilled in the art can also adjust the amounts of the tougheners, plasticizers, flame retardants and antioxidants according to the reaction conditions of the polyimide resin. Before adding them to the stirring tank, the tougheners, plasticizers, flame retardants and antioxidants are mixed, and then the mixed tougheners, plasticizers, flame retardants and antioxidants are added to the stirring tank at the same time, and stirred at room temperature for 50 minutes.

[0049] S6: Finally, 0.7 kg of aqueous solvent was added into the stirred tank and stirred at room temperature for 15 min to form a mixture.

[0050] S7: The mixture in the stirred tank is heated to 40-60° C. and then conveyed to a vacuum degassing tower. Specifically, the mixture can be heated to 50° C., and then conveyed to the vacuum degassing tower through a pipeline.

[0051] S8: The vacuum degree in the vacuum degassing tower is controlled to be between 1.33 and 6.65 kPa by a vacuum pump. It should be noted that the specification and type of the vacuum pump are adaptively selected by technical personnel in this field according to the vacuum degassing tower. The working performance of the vacuum pump should be able to ensure that the vacuum degree in the vacuum degassing tower is maintained between 1.33 and 6.65 kPa. When working, the input end of the vacuum pump is connected to the vacuum degassing tower through a pipeline, and then the vacuum pump is turned on. The vacuum pump will work to suck the air in the vacuum degassing tower, so that the inner cavity space of the vacuum degassing tower forms a negative pressure state.

[0052] S9: Perform spray degassing treatment in a vacuum degassing tower, collect the degassed mixture, and obtain an insulating material. It should be noted that when the mixture is transported to the vacuum degassing tower, since the inner cavity space of the vacuum degassing tower is in a negative pressure state, the vacuum degassing tower will generate a large suction force. Therefore, it is necessary to install an electromagnetic valve on the vacuum degassing tower to control the flow rate of the mixture entering the vacuum degassing tower through the electromagnetic valve to ensure that the mixture can form a spray effect in the vacuum degassing tower.

[0053] When the mixture forms droplets, the contact area between the mixture and the inner cavity space of the vacuum degassing tower is greatly increased, so the air in the mixture can be quickly removed.

[0054] Finally, the prepared insulating material is coated on the surface of the electrical steel, and then the coated electrical steel is placed in a heating furnace at 60° C. for curing, and the performance of the cured insulating material is tested.

[0055] Example 2

[0056] like Figure 1 and Figure 4 As shown, the present invention discloses a low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material, the mass percentage of the insulating material comprises: polyimide resin, 70%; nano zinc oxide, 12%; tetrabutyl titanate, 3%; bio-based solvent, 7%; additives, 8%;

[0057] The polyimide resin, nano zinc oxide, tetrabutyl titanate, bio-based solvent and additives are mixed in a mass ratio to form a mixture, and the mixture is added to a vacuum degassing tower for spray degassing. The specific preparation process of the insulating material includes the following steps:

[0058] S1: Select polyimide resin, nano zinc oxide, tetrabutyl titanate, bio-based solvent and additives according to the mass ratio, for example, 7.0 kg of polyimide resin, 1.2 kg of nano zinc oxide, 0.3 kg of tetrabutyl titanate, 0.7 kg of bio-based solvent and 0.8 kg of additives in total.

[0059] S2: First, add 7.0 kg of polyimide resin into a stirring kettle. The specification and type of the stirring kettle are adaptively selected by those skilled in the art according to the preparation process of the insulating material. Stir at room temperature for 8 minutes.

[0060] S3: Add 1.2 kg of nano zinc oxide into the stirring kettle and stir at room temperature for 30 minutes.

[0061] S4: Then, 0.3 kg of tetrabutyl titanate was added into the stirred tank and stirred at room temperature for 40 min.

[0062] S5: Additives include tougheners, plasticizers, flame retardants and antioxidants. The total weight of the tougheners, plasticizers, flame retardants and antioxidants is 0.8 kg. The mass ratio of the tougheners, plasticizers, flame retardants and antioxidants is 1:1:1:1. Those skilled in the art can also adjust the amounts of the tougheners, plasticizers, flame retardants and antioxidants according to the reaction conditions of the polyimide resin. Before adding them to the stirring tank, the tougheners, plasticizers, flame retardants and antioxidants are mixed, and then the mixed tougheners, plasticizers, flame retardants and antioxidants are added to the stirring tank at the same time, and stirred at room temperature for 50 minutes.

[0063] S6: Finally, 0.7 kg of the bio-based solvent was added to the stirred tank and stirred at room temperature for 15 min to form a mixture.

[0064] S7: The mixture in the stirred tank is heated to 40-60° C. and then conveyed to a vacuum degassing tower. Specifically, the mixture can be heated to 50° C., and then conveyed to the vacuum degassing tower through a pipeline.

[0065] S8: The vacuum degree in the vacuum degassing tower is controlled to be between 1.33 and 6.65 kPa by a vacuum pump. It should be noted that the specification and type of the vacuum pump are adaptively selected by technical personnel in this field according to the vacuum degassing tower. The working performance of the vacuum pump should be able to ensure that the vacuum degree in the vacuum degassing tower is maintained between 1.33 and 6.65 kPa. When working, the input end of the vacuum pump is connected to the vacuum degassing tower through a pipeline, and then the vacuum pump is turned on. The vacuum pump will work to suck the air in the vacuum degassing tower, so that the inner cavity space of the vacuum degassing tower forms a negative pressure state.

[0066] S9: Perform spray degassing treatment in a vacuum degassing tower, collect the degassed mixture, and obtain an insulating material. It should be noted that when the mixture is transported to the vacuum degassing tower, since the inner cavity space of the vacuum degassing tower is in a negative pressure state, the vacuum degassing tower will generate a large suction force. Therefore, it is necessary to install an electromagnetic valve on the vacuum degassing tower to control the flow rate of the mixture entering the vacuum degassing tower through the electromagnetic valve to ensure that the mixture can form a spray effect in the vacuum degassing tower.

[0067] When the mixture forms droplets, the contact area between the mixture and the inner cavity space of the vacuum degassing tower is greatly increased, so the air in the mixture can be quickly removed.

[0068] Finally, the prepared insulating material is coated on the surface of the electrical steel, and then the coated electrical steel is placed in a heating furnace at 60° C. for curing, and the performance of the cured insulating material is tested.

[0069] Example 3

[0070] like Figure 1 and Figure 4As shown, the present invention discloses a low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material, the mass percentage of the insulating material comprises: polyimide resin, 70%; nano-alumina, 12%; acetylacetonate iron, 3%; low-volatile organic solvent, 7%; additives, 8%;

[0071] The polyimide resin, nano-alumina, ferric acetylacetonate, a low-volatile organic solvent and an additive are mixed in a mass ratio to form a mixture, and the mixture is added to a vacuum degassing tower for spray degassing. The specific preparation process of the insulating material includes the following steps:

[0072] S1: Select polyimide resin, nano-alumina, ferric acetylacetonate, low-volatile organic solvent and additives according to the mass ratio, for example, 7.0 kg of polyimide resin, 1.2 kg of nano-alumina, 0.3 kg of ferric acetylacetonate, 0.7 kg of low-volatile organic solvent and 0.8 kg of additives in total.

[0073] S2: First, add 7.0 kg of polyimide resin into a stirring kettle. The specification and type of the stirring kettle are adaptively selected by those skilled in the art according to the preparation process of the insulating material. Stir at room temperature for 8 minutes.

[0074] S3: Add 1.2 kg of nano-alumina into the stirring tank and stir at room temperature for 30 minutes.

[0075] S4: Then 0.3 kg of ferric acetylacetonate was added into the stirred tank and stirred at room temperature for 40 min.

[0076] S5: Additives include tougheners, plasticizers, flame retardants and antioxidants. The total weight of the tougheners, plasticizers, flame retardants and antioxidants is 0.8 kg. The mass ratio of the tougheners, plasticizers, flame retardants and antioxidants is 1:1:1:1. Those skilled in the art can also adjust the amounts of the tougheners, plasticizers, flame retardants and antioxidants according to the reaction conditions of the polyimide resin. Before adding them to the stirring tank, the tougheners, plasticizers, flame retardants and antioxidants are mixed, and then the mixed tougheners, plasticizers, flame retardants and antioxidants are added to the stirring tank at the same time, and stirred at room temperature for 50 minutes.

[0077] S6: Finally, 0.7 kg of low-volatile organic solvent was added into the stirred tank and stirred at room temperature for 15 min to form a mixture.

[0078] S7: The mixture in the stirred tank is heated to 40-60° C. and then conveyed to a vacuum degassing tower. Specifically, the mixture can be heated to 50° C., and then conveyed to the vacuum degassing tower through a pipeline.

[0079] S8: The vacuum degree in the vacuum degassing tower is controlled to be between 1.33 and 6.65 kPa by a vacuum pump. It should be noted that the specification and type of the vacuum pump are adaptively selected by technical personnel in this field according to the vacuum degassing tower. The working performance of the vacuum pump should be able to ensure that the vacuum degree in the vacuum degassing tower is maintained between 1.33 and 6.65 kPa. When working, the input end of the vacuum pump is connected to the vacuum degassing tower through a pipeline, and then the vacuum pump is turned on. The vacuum pump will work to suck the air in the vacuum degassing tower, so that the inner cavity space of the vacuum degassing tower forms a negative pressure state.

[0080] S9: Perform spray degassing treatment in a vacuum degassing tower, collect the degassed mixture, and obtain an insulating material. It should be noted that when the mixture is transported to the vacuum degassing tower, since the inner cavity space of the vacuum degassing tower is in a negative pressure state, the vacuum degassing tower will generate a large suction force. Therefore, it is necessary to install an electromagnetic valve on the vacuum degassing tower to control the flow rate of the mixture entering the vacuum degassing tower through the electromagnetic valve to ensure that the mixture can form a spray effect in the vacuum degassing tower.

[0081] When the mixture forms droplets, the contact area between the mixture and the inner cavity space of the vacuum degassing tower is greatly increased, so the air in the mixture can be quickly removed.

[0082] Finally, the prepared insulating material is coated on the surface of the electrical steel, and then the coated electrical steel is placed in a heating furnace at 60° C. for curing, and the performance of the cured insulating material is tested.

[0083] Example 4

[0084] like Figure 1 and Figure 4 As shown, the present invention discloses a low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material, the mass percentage of the insulating material comprises: polyimide resin, 70%; nano-alumina, 12%; zinc acetate bismuth trichloride, 3%; ionic liquid, 7%; additives, 8%;

[0085] The polyimide resin, nano-alumina, zinc acetate bismuth trichloride, ionic liquid and additives are mixed in a mass ratio to form a mixture, and the mixture is added to a vacuum degassing tower for spray degassing. The specific preparation process of the insulating material includes the following steps:

[0086] S1: Select polyimide resin, nano-alumina, zinc acetate bismuth chloride, and ionic liquid according to the mass ratio. For example, 7.0 kg of polyimide resin, 1.2 kg of nano-alumina, 0.3 kg of zinc acetate bismuth chloride, 0.7 kg of ionic liquid, and a total of 0.8 kg of additives.

[0087] S2: First, add 7.0 kg of polyimide resin into a stirring kettle. The specification and type of the stirring kettle are adaptively selected by those skilled in the art according to the preparation process of the insulating material. Stir at room temperature for 8 minutes.

[0088] S3: Add 1.2 kg of nano-alumina into the stirring tank and stir at room temperature for 30 minutes.

[0089] S4: Then 0.3 kg of zinc acetate bismuth trichloride was added into the stirred tank and stirred at room temperature for 40 min.

[0090] S5: Additives include tougheners, plasticizers, flame retardants and antioxidants. The total weight of the tougheners, plasticizers, flame retardants and antioxidants is 0.8 kg. The mass ratio of the tougheners, plasticizers, flame retardants and antioxidants is 1:1:1:1. Before adding into the stirring tank, the tougheners, plasticizers, flame retardants and antioxidants are mixed. Then the mixed tougheners, plasticizers, flame retardants and antioxidants are added into the stirring tank at the same time and stirred at room temperature for 50 minutes.

[0091] S6: Finally, 0.7 kg of ionic liquid was added into the stirred tank and stirred at room temperature for 15 min to form a mixture.

[0092] S7: The mixture in the stirred tank is heated to 40-60° C. and then conveyed to a vacuum degassing tower. Specifically, the mixture can be heated to 50° C., and then conveyed to the vacuum degassing tower through a pipeline.

[0093] S8: The vacuum degree in the vacuum degassing tower is controlled to be between 1.33 and 6.65 kPa by a vacuum pump. It should be noted that the specification and type of the vacuum pump are adaptively selected by technical personnel in this field according to the vacuum degassing tower. The working performance of the vacuum pump should be able to ensure that the vacuum degree in the vacuum degassing tower is maintained between 1.33 and 6.65 kPa. When working, the input end of the vacuum pump is connected to the vacuum degassing tower through a pipeline, and then the vacuum pump is turned on. The vacuum pump will work to suck the air in the vacuum degassing tower, so that the inner cavity space of the vacuum degassing tower forms a negative pressure state.

[0094] S9: Perform spray degassing treatment in a vacuum degassing tower, collect the degassed mixture, and obtain an insulating material. It should be noted that when the mixture is transported to the vacuum degassing tower, since the inner cavity space of the vacuum degassing tower is in a negative pressure state, the vacuum degassing tower will generate a large suction force. Therefore, it is necessary to install an electromagnetic valve on the vacuum degassing tower to control the flow rate of the mixture entering the vacuum degassing tower through the electromagnetic valve to ensure that the mixture can form a spray effect in the vacuum degassing tower.

[0095] When the mixture forms droplets, the contact area between the mixture and the inner cavity space of the vacuum degassing tower is greatly increased, so the air in the mixture can be quickly removed.

[0096] Finally, the prepared insulating material is coated on the surface of the electrical steel, and then the coated electrical steel is placed in a heating furnace at 60° C. for curing, and the performance of the cured insulating material is tested.

[0097] Comparative Example 1

[0098] It should be noted that the components required for the insulating coating prepared in the comparative example are: epoxy resin, 70%; aluminum powder, 12%; methyltetrahydrophthalic anhydride, 3%; solvent, 7%; additive, 8%;

[0099] The above components are prepared according to the following steps:

[0100] S1: Select epoxy resin, aluminum powder, methyltetrahydrophthalic anhydride, solvent, and additives according to the mass ratio. For example, select 7.0 kg of epoxy resin, 1.2 kg of aluminum powder, 0.3 kg of methyltetrahydrophthalic anhydride, 0.7 kg of solvent, and 0.8 kg of additives in total.

[0101] S2: First, add 7.0 kg of epoxy resin into a stirring tank. The specification and type of the stirring tank are adaptively selected by technicians in this field according to the preparation process of the insulating material. Stir at room temperature for 8 minutes.

[0102] S3: Add 1.2 kg of aluminum powder into the stirred tank and stir at room temperature for 30 min.

[0103] S4: Then, 0.3 kg of methyltetrahydrophthalic anhydride was added into the stirred kettle and stirred at room temperature for 40 min.

[0104] S5: Additives include tougheners, plasticizers, flame retardants and antioxidants. The total weight of the tougheners, plasticizers, flame retardants and antioxidants is 0.8 kg. Before adding them into the stirring tank, the tougheners, plasticizers, flame retardants and antioxidants are mixed. Then the mixed tougheners, plasticizers, flame retardants and antioxidants are added into the stirring tank at the same time and stirred at room temperature for 50 minutes.

[0105] S6: Finally, 0.7 kg of solvent was added into the stirred tank and stirred at room temperature for 15 min to form a mixture.

[0106] S7: The mixture in the stirred tank is heated to 40-60° C. and then conveyed to a vacuum degassing tower. Specifically, the mixture can be heated to 50° C., and then conveyed to the vacuum degassing tower through a pipeline.

[0107] S8: The vacuum degree in the vacuum degassing tower is controlled to be between 1.33 and 6.65 kPa by a vacuum pump. It should be noted that the specification and type of the vacuum pump are adaptively selected by technical personnel in this field according to the vacuum degassing tower. The working performance of the vacuum pump should be able to ensure that the vacuum degree in the vacuum degassing tower is maintained between 1.33 and 6.65 kPa. When working, the input end of the vacuum pump is connected to the vacuum degassing tower through a pipeline, and then the vacuum pump is turned on. The vacuum pump will work to suck the air in the vacuum degassing tower, so that the inner cavity space of the vacuum degassing tower forms a negative pressure state.

[0108] S9: Perform spray degassing treatment in a vacuum degassing tower, collect the degassed mixture, and obtain an insulating material. It should be noted that when the mixture is transported to the vacuum degassing tower, since the inner cavity space of the vacuum degassing tower is in a negative pressure state, the vacuum degassing tower will generate a large suction force. Therefore, it is necessary to install an electromagnetic valve on the vacuum degassing tower to control the flow rate of the mixture entering the vacuum degassing tower through the electromagnetic valve to ensure that the mixture can form a spray effect in the vacuum degassing tower.

[0109] When the mixture forms droplets, the contact area between the mixture and the inner cavity space of the vacuum degassing tower is greatly increased, so the air in the mixture can be quickly removed.

[0110] Finally, the prepared insulating material is coated on the surface of the electrical steel, and then the coated electrical steel is placed in a heating furnace at 60° C. for curing, and the performance of the cured insulating material is tested.

[0111] Comparative Example 2:

[0112] It should be noted that the components required for the insulating coating prepared in the comparative example are: polyimide resin, 70%; nano-silicon dioxide, 12%; dibutyltin dilaurate, 3%; aqueous solvent, 7%; additives, 8%; different from Example 1, step S7 of comparative example 2 does not use a vacuum degassing tower for degassing, but uses a vacuum degasser in the prior art, such as the vacuum degasser produced by Changsha Duoling Environmental Protection Technology Co., Ltd.

[0113] Finally, the prepared insulating material is coated on the surface of the electrical steel, and then the coated electrical steel is placed in a heating furnace at 60° C. for curing, and the performance of the cured insulating material is tested.

[0114] Performance testing method:

[0115] Performance tests include tensile strength test, shear strength test, thermal conductivity test, thermal deformation test, thermal expansion coefficient test, curing temperature test, curing time test and VOC gas emission test.

[0116] The tensile strength test is carried out using a tensile testing machine, specifically, the cured insulating material is placed in the tensile testing machine for a tensile test.

[0117] The shear strength test uses a shear strength testing machine, specifically, the cured insulating material is placed in the shear strength testing machine for shear force testing.

[0118] The thermal conductivity is tested using a thermal conductivity tester, the thermal expansion coefficient is tested using a thermal expansion meter, and the curing temperature and curing time are manually measured by a technician in this field using a counter.

[0119] VOC gas emission detection is carried out using a VOC gas tester.

[0120] The properties of the insulating materials prepared according to the above-mentioned Examples 1-4 and Comparative Examples 1-2 are shown in Table 1 below:

[0121] Table 1 Performance test results of the insulating materials obtained in Examples 1-4 and Comparative Examples 1-2

[0122]

[0123] According to Examples 1-4 and Comparative Example 1, it can be seen that:

[0124] The difference between Examples 1-4 and Comparative Example 1 is that the main materials of Examples 1-4 are polyimide resin and nanoscale curing agent. The nanoscale curing agent can make the polyimide resin react quickly with the reaction accelerator, so that the polyimide resin is quickly cross-linked and cured, which greatly shortens the curing time, and the polyimide resin can be cured at a lower temperature. The curing time of Examples 1-4 is half of the curing time of Comparative Example 1, which can reduce the energy consumption of electrical steel when coating insulating materials. At the same time, when the polyimide resin, nanoscale curing agent and aqueous solvent are cured at low temperature, the volatile VOC gas will also be greatly reduced. The amount of VOC gas volatilized in Examples 1-4 is only one-third of the amount of VOC gas volatilized in Comparative Example 1, which reduces pollution to the environment. In order to complete the curing of the insulating material prepared in Comparative Example 1 within the same time, it is necessary to increase the curing temperature of the insulating material, which will greatly increase the emission of VOC gas, seriously pollute the environment, and is not conducive to the use of insulating materials.

[0125] According to Examples 1-4 and Comparative Example 2, it can be seen that:

[0126] The difference between Example 1-4 and Comparative Example 2 is that Example 1-4 adopts the vacuum degassing tower of the present invention, while Comparative Example 2 adopts the degassing treatment of the prior art. The vacuum degassing tower adopted in Example 1-4 can remove the gas in the prepared insulating material to the greatest extent, thereby improving the tensile strength and shear strength of the prepared insulating material and improving the mechanical properties of the insulating material.

[0127] The insulating material is obtained by spraying and degassing polyimide resin, nano-scale curing agent, reaction accelerator, solvent and additives in a vacuum degassing tower. The curing temperature is greatly reduced. At the same temperature, the curing time of the insulating material is greatly shortened, and the emission of volatile organic compounds of the insulating material is reduced by two-thirds, solving the problems of long curing time and environmental pollution of traditional insulating coatings.

[0128] Example 5

[0129] like Figure 2-Figure 5 As shown, the vacuum degassing tower includes a fixed tower body 1, the top of the fixed tower body 1 is connected to a sliding tower body 2, the top surface of the sliding tower body is connected to an input pipe 3 and an outlet pipe 4, the input pipe 3 is used to transport the mixture, and the end of the input pipe 3 away from the sliding tower body 2 is connected to the stirring kettle, so that when the stirring kettle completes the stirring process, the mixture can be transported to the inner cavity of the vacuum degassing tower through the input pipe 3 for vacuum degassing, and the outlet pipe 4 is used to connect a vacuum pump, and the specifications and types of the vacuum pump are adaptively selected by technical personnel in this field according to the vacuum degree required by the vacuum degassing tower. A liquid collecting mechanism 7 is arranged inside the fixed tower body 1, and a bottom track 5 is fixedly connected to the bottom surface of the fixed tower body 1, and a storage bucket 6 is slidably connected to the bottom surface of the bottom track 5.

[0130] It should be noted that a sliding cylinder 21 is fixedly connected to the bottom surface of the sliding tower body 2, and the sliding cylinder 21 matches the inner cavity of the fixed tower body 1, that is, the sliding cylinder 21 is slidingly and sealingly connected to the fixed tower body 1, and a group of hydraulic push rods (not shown in the figure) can be installed on the outside of the fixed tower body 1, one end of the hydraulic push rod is fixed to the outside of the fixed tower body 1, and the output end of the hydraulic push rod is fixedly connected to the side of the sliding tower body 2. When in use, the hydraulic push rod can be opened, so that the hydraulic push rod can control the height of the sliding tower body 2, that is, control the overall center axis length of the fixed tower body 1 and the sliding tower body 2.

[0131] An ultrasonic transmitter may be installed inside the input pipe 3 , and is used to transmit ultrasonic waves to the mixture inside the input pipe 3 , and detect the air content in the mixture inside the input pipe 3 based on the loss of the ultrasonic waves.

[0132] A height variation curve of the mixture falling in the vacuum degassing tower is generated according to the change in the air content in the mixture inside the input pipe 3, that is, the greater the air content in the mixture inside the input pipe 3, the greater the height of the mixture falling in the vacuum degassing tower is required to ensure that the air can be completely removed from the mixture after passing through the vacuum degassing tower.

[0133] like Figure 2 one Figure 5As shown, a receiving opening 52 is provided on the top surface of the bottom track 5 near the fixed tower body 1, a sliding sealing plate 51 is provided inside the bottom track 5, and a movable groove matching the sealing plate 51 is provided inside the bottom track 5 near the sealing plate 51, and the sealing plate 51 can slide freely in the movable groove. It should also be noted that a hydraulic cylinder is installed inside the movable groove, and the hydraulic cylinder is used to drive the seal 51 so that the sealing plate 51 can automatically slide in the movable groove.

[0134] like Figure 2-Figure 5 As shown, the liquid collecting mechanism 7 includes a rebound cylinder 71, the interior of the rebound cylinder 71 is fixedly connected with an impact cone 72, the side of the rebound cylinder 71 is fixedly connected with a fixed foot 73, the end of the fixed foot 73 away from the rebound cylinder 71 is fixedly connected to the inner wall of the fixed tower body 1, and the end of the input pipe 3 close to the interior of the sliding tower body 2 is fixedly connected with a spray head 31, the diameter of the spray head 31 is smaller than the maximum diameter of the impact cone 72, and the central axis of the rebound cylinder 71, the impact cone 72 and the spray head 31 coincide. When in use, it should be noted that the input pipe 3 can transport the mixture to the spray head 31, and the spray head 31 converts the mixture into droplets and sprays them vertically. The sprayed droplets will automatically fall on the inside of the rebound cylinder 71 under the action of gravity. Since the diameter of the spray head 31 is smaller than the maximum diameter of the impact cone 72, the rebound cylinder 71 must be larger than the diameter of the spray head 31, so it can completely receive the mixture droplets sprayed from the spray head 31 In the process of the droplet falling in the fixed tower body 1 and the sliding tower body 2, since the fixed tower body 1 and the sliding tower body 2 are in a negative pressure state, the gas in the droplet will inevitably expand and be discharged, thereby achieving a degassing effect and removing the gas in the droplet to the greatest extent, thereby enhancing the mechanical properties of the prepared insulating material. When the droplet contacts the impact cone 72, the droplet will further disperse, thereby ensuring that the air inside is completely discharged, and the rebound cylinder 71 limits the dispersion range of the droplet to ensure that the droplet is always inside the rebound cylinder 71. The droplet entering the rebound cylinder 71 will eventually slide down the side wall of the rebound cylinder 71 and the surface of the impact cone 72 and fall into the storage barrel 6. In order to ensure that the droplet can normally slide down the side wall of the rebound cylinder 71 and the surface of the impact cone 72, a layer of polytetrafluoroethylene can be coated on the side wall of the rebound cylinder 71 and the surface of the impact cone 72 to ensure that the droplet of the mixture can smoothly enter the storage barrel 6.

[0135] When one of the storage buckets 6 is full of the mixture, the storage opening 52 is closed by the sealing plate 51, and then another storage bucket 6 is replaced. After the storage opening 52 of the storage bucket 6 is sealed, the sealing plate 51 is opened to ensure that the storage bucket 6 can continue to collect the mixture. During the process of the sealing plate 51 returning, the storage opening 52 will scrape the surface of the sealing plate 51 to prevent the mixture from accumulating.

[0136] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. Low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulation material, characterized in that: The components of the insulating material by mass percentage include: Polyimide resin, 60-80%; Nano-scale curing agent, 10%-20%; Reaction accelerator, 1%-5%; Solvent, 4%-12%; Additives, 5%-15%; The nano-scale curing agent includes one or more of nano-silicon dioxide, nano-zinc oxide and nano-aluminum oxide. The method for preparing the low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material comprises: mixing a polyimide resin, a nano-scale curing agent, a reaction accelerator, a solvent and an additive in a mass ratio to form a mixture, and adding the mixture into a vacuum degassing tower for spray degassing treatment.

2. The low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to claim 1 is characterized in that: The reaction accelerator is one or more of dibutyltin dilaurate, tetrabutyl titanate, ferric acetylacetonate, and zinc acetate bismuth trichloride.

3. The low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to claim 1 is characterized in that: The solvent is an aqueous solvent, a bio-based solvent, a low-volatile organic solvent or an ionic liquid.

4. The low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to claim 1, characterized in that: The additives include tougheners, plasticizers, flame retardants and antioxidants.

5. The method for preparing the low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1: Selecting polyimide resin, nano-scale curing agent, reaction accelerator, solvent and additive according to mass ratio; S2: Add polyimide resin into a stirring kettle and stir at room temperature for 5-10 minutes; S3: Add the nano-scale curing agent into the stirring kettle and stir at room temperature for 20-40 minutes; S4: Add the reaction accelerator into the stirred tank and stir at room temperature for 30-50 minutes; S5: Add the additive into the stirred tank and stir at room temperature for 40-60 minutes; S6: Add the solvent into the stirred tank and stir for 10-20 min at room temperature to form a mixture; S7: heating the mixture in the stirred tank to 40-60°C and then conveying it to a vacuum degassing tower; S8: Control the vacuum degree in the vacuum degassing tower between 1.33-6.65 kPa by a vacuum pump; S9: performing spray degassing treatment in a vacuum degassing tower, collecting the degassing mixture, and obtaining an insulating material.

6. The method for preparing the low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to claim 5, characterized in that: The vacuum degassing tower comprises a fixed tower body (1), the top of the fixed tower body (1) is connected to a sliding tower body (2), the top surface of the sliding tower body is connected to an input pipe (3) and an outlet pipe (4), the input pipe (3) is used to transport a mixture, and the outlet pipe (4) is used to connect to a vacuum pump, a liquid collecting mechanism (7) is arranged inside the fixed tower body (1), the bottom surface of the fixed tower body (1) is fixedly connected to a bottom track (5), and the bottom surface of the bottom track (5) is slidably connected to a storage bucket (6).

7. The method for preparing low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to claim 6, characterized in that: A receiving opening (52) is provided on the top surface of the bottom track (5) near the fixed tower body (1), and a sliding sealing plate (51) is provided inside the bottom track (5).

8. The method for preparing low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to claim 6, characterized in that: The liquid collecting mechanism (7) comprises a rebound cylinder (71), an impact cone (72) is fixedly connected inside the rebound cylinder (71), a fixed foot (73) is fixedly connected to the side of the rebound cylinder (71), and one end of the fixed foot (73) away from the rebound cylinder (71) is fixedly connected to the inner wall of the fixed tower body (1).

9. The method for preparing low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to claim 6, characterized in that: A spray head (31) is fixedly connected to one end of the input pipe (3) close to the inside of the sliding tower body (2); the diameter of the spray head (31) is smaller than the maximum diameter of the impact cone (72); and the central axes of the rebound cylinder (71), the impact cone (72) and the spray head (31) coincide.

10. Use of the low-temperature fast-curing high-temperature resistant electrical steel environmentally friendly insulating material according to any one of claims 1 to 4 in electrical steel.

Citation Information

Patent Citations

  • Highly-efficient degassing tower

    CN108992975A

  • Hydrogen purity improving system and method for degassing hydrogen side sealing oil recharging

    CN112973195A

  • Flame-retardant insulating paint for new energy automobile motor and preparation method of flame-retardant insulating paint

    CN118325461A

  • High-temperature-resistant and chemical-corrosion-resistant insulating paint, enameled wire and preparation method

    CN118421191A

  • Vacuum degassing tank

    CN213994924U