Graphene-based organic silicon / epoxy resin composite heavy anti-corrosion coating and preparation method thereof

Through the conductive network framework structure of graphene-based silicone/epoxy resin composite coating, the corrosion problem of metal substrates in high-temperature acid gas environment in cement clinker production line is solved, providing an efficient corrosion-resistant coating, and extending the equipment Service life.

CN118931379AInactive Publication Date: 2024-11-12安徽芜湖海螺建筑安装工程有限责任公司 +1

Patent Information

Application Number
CN202411179590.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing temperature-resistant and anti-corrosion coatings are easy to decompose in the high-temperature acid gas environment of the cement clinker production line, with poor adhesion, low mechanical strength, short service life, and cannot effectively prevent corrosion of metal substrates.

Method used

Use graphene-based silicone/epoxy resin composite heavy anticorrosion coating to form a conductive network framework through conductive polymer modified graphene powder, carbon nanofibers, nanosilicon oxide and other materials, reduce the use of zinc powder/aluminum powder, and improve coating The wear resistance, high temperature resistance and corrosion resistance of the layer.

Benefits of technology

It provides a new type of coating with strong bonding power and corrosion resistance to metal substrates. It can be used for a long time in a high temperature environment of 200-350℃, effectively protects the metal substrate of clinker production equipment in the cement industry, and fills in the long-term use of corrosion protection. Blanks of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931379A_ABST
    Figure CN118931379A_ABST
Patent Text Reader

Abstract

The invention relates to a graphene-based organic silicon / epoxy resin composite heavy anti-corrosion coating and a preparation method thereof. The coating is composed of a component A and a component B, the component A is prepared from organic silicon / epoxy resin composite resin, a cosolvent, graphene powder, carbon nano tube / fiber, nano silicon oxide, nano aluminum oxide, nano silicon carbide, nano niobium carbide, nano PTFE fine powder, zinc powder, aluminum powder, a dispersing agent, a defoaming agent and an anti-flash-rust additive, and the component B is prepared from a cosolvent and a curing agent. According to the invention, the conductive stone polymer is utilized to modify the graphene powder, the carbon nanofibers have the effects of conductivity, high temperature resistance and corrosion resistance, and a conductive network skeleton is formed, so that the use amount of zinc powder / aluminum powder is reduced; the nano silicon oxide, the nano zinc oxide, the nano titanium oxide, the silicon carbide and the niobium carbide can achieve the effects of wear resistance, high temperature resistance and corrosion resistance. The novel high-temperature-resistant / wear-resistant graphene-based organic silicon / epoxy resin composite heavy anti-corrosion coating has the advantages of being high in binding force with a metal base material and resistant to corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an injection mold, and in particular to a graphene-based organic silicon / epoxy resin composite heavy-duty anticorrosive coating and a preparation method thereof. Background Art

[0002] Practical research has proved that the key to the "low-carbon emission" transformation of the cement industry lies in achieving low-carbon and energy-saving production in the cement clinker production process. However, the "low-carbon emission reduction" transformation of the cement clinker production line will cause great changes in the actual production conditions, and ultimately make the anti-corrosion measures in each link of the original production line unable to meet the requirements of the new working conditions, thus causing different types and degrees of corrosion.

[0003] For example, the use of technologies such as "co-treatment of cement kilns" and "alternative fuel technology" to carry out low-carbon emission reduction transformation of cement kiln clinker production lines can indeed observe corrosion conditions different from those caused by the operation of traditional cement kiln clinker production lines during operation. Taking Conch Kawasaki's CKK gasifier, Jinyu Finland JYF's "garbage to fire", and Huaxin Holcim HXH's "multi-point coordination" technology as examples, due to the need to deal with domestic and production waste, a variety of harmful elements such as alkali, chlorine, and sulfur will be introduced in addition. Moreover, since most of the garbage is an organic medium with a high moisture content, during the garbage treatment process, the unremoved moisture enters the kiln in a gaseous state and occupies the space of the original hot air, which also has a potential impact on the balanced operation of the kiln system. In addition, in order to reduce other emissions such as nitrogen oxides, it is necessary to introduce an SNR denitrification system that requires a large amount of ammonia water into the cement clinker production line, thereby exacerbating the ammonia corrosion phenomenon of the production line. The final result is that the original anti-corrosion measures fail early, resulting in corrosion of the equipment in the form of chemical erosion and crusting.

[0004] In short, since the cement clinker production line adopts energy-saving and emission-reduction measures such as desulfurization and denitrification treatment, coordinated disposal, etc., it will cause changes in the internal working conditions, forming a high-temperature acidic and alkaline corrosion environment that is very easy to cause corrosion to metal materials, making the original anti-corrosion measures fail early. However, the existing heat-resistant anti-corrosion coatings on the market are very easy to decompose in the cement clinker production and operation environment, have poor adhesion to the substrate, low mechanical strength, and a very short service life. Therefore, so far, there are few corresponding ready-made coatings on the market for high-temperature anti-corrosion coatings for cement clinker production lines. Summary of the invention

[0005] The purpose of the present invention is to solve the problems of the above-mentioned prior art, to solve the problems of long-term heat resistance and corrosion protection of metal substrates of production lines in high temperature (temperature of 200-400°C) acidic gas environments in the cement industry, and to provide a new type of high temperature resistant / wear-resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating and its preparation technology.

[0006] The technical solution adopted by the present invention to solve the technical problem is: a graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating, which is composed of two components, A and B. Component A is composed of silicone / epoxy resin composite resin, co-solvent, graphene powder, carbon nanotubes / fibers, nano-silicon oxide, nano-aluminum oxide, nano-silicon carbide, nano-niobium carbide, nano-PTFE fine powder, zinc powder, aluminum powder, dispersant, defoaming agent and anti-flash rust additive, and component B is composed of co-solvent and curing agent. The specific coating formula is as follows in parts by weight:

[0007] Component A:

[0008] Silicone resin: 10-45wt.%

[0009] Epoxy resin: 5-20wt.%

[0010] Cosolvent: 5-20wt.%

[0011] Conductive polymer modified graphene powder: 0.1-2wt.%

[0012] Carbon nanotubes / fibers: 1-10wt.%

[0013] Nano zinc oxide: 1-10wt.%

[0014] Nano titanium oxide: 1-10wt.%

[0015] Nano silicon oxide: 1-10wt.%

[0016] Silicon carbide: 1-10wt.%

[0017] Niobium carbide: 1-10wt.%

[0018] Zinc powder / aluminum powder: 5-25wt.%

[0019] Dispersant: 0.2-3wt.%

[0020] Defoamer: 0.2-3wt.%

[0021] Anti-flash rust additive: 0.2-3wt.%

[0022] Component B:

[0023] Cosolvent: 5-15wt.%

[0024] Curing agent: 3-10wt.%

[0025] Add component B to component A, and cure at room temperature to 70°C or under ultraviolet light for 2-5 hours to prepare a new type of high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating;

[0026] The silicone resin is one or more of pure silicone resin, modified silicone resin (methyl silicone containing methoxy groups), silicone polyester resin, silicone alkyd resin, silicone acrylic resin and silicone epoxy resin;

[0027] The epoxy resin is one or more of bisphenol A epoxy resin, bisphenol S epoxy resin, and epoxy novolac resin;

[0028] The co-solvent is one or more of methanol, ethanol, toluene, xylene, n-butanol, 1,4-butanediol, acetone, ethylene glycol butyl ether, ethyl acetate, propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, and dipropylene glycol butyl ether.

[0029] The conductive polymer modified graphene powder is a composite of one or more conductive polymers selected from polyaniline (PANI), poly(3,4-ethylenedioxythiophene) (PEDOT), polyethylenedioxythiophene-polystyrene sulfonate (PEDOT:PSS) and few-layer graphene powder.

[0030] The carbon nanotube / fiber may be one or both of carbon nanotube and carbon nanofiber, wherein the carbon nanotube is one or both of carboxylated and amino-treated single-walled nanotube or multi-walled carbon nanotube.

[0031] The particle size of the nano zinc oxide is about 100-500nm; the particle size of the nano titanium oxide is about 10-100nm; the particle size of the nano silicon oxide is about 10-100nm; the particle size of the silicon carbide and niobium carbide is 1-10μm; the zinc powder / aluminum powder is one or both of zinc powder and aluminum powder.

[0032] The dispersant is one or more of a polyurethane dispersant, an acrylic dispersant, and an acetylene alcohol dispersant.

[0033] The defoaming agent is one or more of a mineral oil defoaming agent and a silicon defoaming agent (organic silicon, modified silicon polyether, polydimethylsiloxane (PDMS) and a mixture of silicon dioxide).

[0034] The anti-flash rust additive is one or more of cationic salts (sodium nitrite, sodium molybdate, strontium chromate, zinc phosphate, strontium phosphosilicate, aluminum tripolyphosphate, zinc aluminum phosphate + zinc molybdate) or organic polymer amine anti-flash rust additives.

[0035] The curing agent is one or more of polyamide 650, polyamide 651, polyamide 910, phenolic amine T-31, polythiol QE-340M, polythiol GPM-800, ethylenediamine, hexamethylenediamine, diethylenetriamine, tetraethylenepentamine, diethylaminopropylamine, 4,4′-diaminodiphenyl sulfone, m-phenylenediamine, tetraethyl orthosilicate, silane coupling agent KH-560, KH-550.

[0036] A method for preparing a graphene-based organosilicon / epoxy resin composite heavy-duty anticorrosion coating, wherein the method for preparing the novel high-temperature-resistant / wear-resistant graphene-based organosilicon / epoxy resin composite heavy-duty anticorrosion coating is characterized by comprising the following steps:

[0037] 1) Preparation of conductive polymer modified graphene powder

[0038] The few-layer graphene and conductive polymer powder (one or more of PANI, PEDOT, PEDOT:PSS) are matched according to the mass ratio, and the two are evenly mixed by high-energy ball milling. The method is characterized in that before ball milling, the balls, the tank and the sample to be milled are heated at 60°C, and then the few-layer graphene powder and the conductive polymer powder are pre-mixed at a mass ratio of 5-1:1, and then the mixture is put into an agate ball mill tank, agate balls and anhydrous ethanol are added, and the material-liquid ratio and the ball-to-material ratio are controlled to be 1:3-5: and 4-6:1 respectively, and ball milling is carried out with a planetary ball mill, and then vacuum drying is carried out at 60°C. After complete drying, a conductive polymer modified graphene powder composite material is obtained.

[0039] 2) Preparation of Component A:

[0040] The component ratio is characterized in that the silicone resin, epoxy resin and co-solvent are stirred at a rotation speed of 500-700 rpm for 10-20 minutes to obtain a uniform silicone resin / epoxy resin mixed solution; then a dispersant, carbon nanotubes / fibers, conductive polymer modified graphene composites and defoaming agents are added and stirred at a rotation speed of 500-700 rpm for 10-20 minutes, then zinc powder / aluminum powder, nano zinc oxide, nano titanium oxide, nano silicon oxide, silicon carbide, niobium carbide, niobium carbide and the like are added and stirred at a rotation speed of 1000-1200 rpm for 10-20 minutes, and finally an anti-flash rust additive is added and stirred at a rotation speed of 1000-1200 rpm for 10-20 minutes to obtain slurry A.

[0041] 3) Preparation of component B:

[0042] The curing agent and the co-solvent are stirred at a rotation speed of 500-700 rpm for 10-20 min to obtain slurry B.

[0043] 4) Mix components A and B to prepare a new type of heavy-duty anti-corrosion coating

[0044] Add slurry B to slurry A, stir at 1000-1200 rpm for 10-20 min, and then carry out subsequent anti-corrosion coating brushing, spraying and other processes; cure at room temperature to 70°C or under ultraviolet light for 2-5 hours to prepare a new high temperature resistant / wear-resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating.

[0045] The beneficial effects of the present invention are as follows: (1) The present invention utilizes conductive stone polymer modified graphene powder and carbon nanofiber to achieve electrical conductivity and high temperature resistance and corrosion resistance, and because a conductive network skeleton is formed, the amount of zinc powder / aluminum powder used is reduced; nano silicon oxide, nano zinc oxide, nano titanium oxide, silicon carbide, and niobium carbide can achieve wear resistance, high temperature resistance, and corrosion resistance. The novel high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating has the advantages of strong bonding with metal substrates and corrosion resistance.

[0046] (2) The novel high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating of the present invention can be specifically applied to cement clinker production lines, successfully filling the gap in the long-term use of anti-corrosion materials in cement kiln clinker production line equipment in China.

[0047] (3) The novel high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating prepared by the present invention can be coated by conventional coating processes such as brushing or spraying to form an anti-corrosion coating that integrates the bottom and the surface of the metal substrate. It uses silicone resin and epoxy resin composite as the base material graphene, modified carbon nanotubes as the coating functional enhancement agent, polyamide 650 and phenolic amine T-31 as the composite curing agent to form a high corrosion resistance system. Thanks to the conductive network formed by conductive polymer modified graphene, conductive polymer modified ultrafine ferrophosphorus powder and modified carbon nanotubes, the amount of zinc used in the coating can be reduced. The coating thickness formed on the metal surface by the obtained heavy-duty anti-corrosion composite coating is 300-1000μm, and it can resist corrosion damage of 200-350℃ and strong corrosive media such as hydrogen sulfide for a long time, solve the problem of high temperature and strong corrosion in clinker production equipment in the cement industry, and effectively protect the metal substrate of its production equipment.

[0048] The present invention will be described in more detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 It is a schematic diagram of the production process of the present invention. DETAILED DESCRIPTION

[0050] The directions or positional relationships indicated by the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like in the application text are based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a specific direction, be constructed and operate in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0051] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0052] Embodiment 1, as Figure 1 As shown,

[0053] Preparation of a novel high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating

[0054] Component A:

[0055] Silicone epoxy resin: 40wt.%

[0056] Epoxy resin: 10wt.%

[0057] Co-solvent (mixed co-solvent of n-butanol, xylene and dipropylene glycol butyl ether in a mass ratio of 5:2:1): 8.8wt.%

[0058] Conductive polymer modified graphene powder (4:1 composite of few-layer graphene powder and polyaniline): 1.47wt.%

[0059] Carbon nanotubes / fibers: 1.76wt.%

[0060] Nano zinc oxide: 4.11wt.%

[0061] Nano titanium oxide: 4.11wt.%

[0062] Nano silicon oxide: 2.94wt.%

[0063] Silicon carbide: 2.94wt.%

[0064] Niobium carbide: 2.94wt.%

[0065] Zinc powder: 8.82wt.%

[0066] Acrylic alkyd phenol dispersant: 1.59wt.%

[0067] Silicone defoamer: 1.41wt.%

[0068] Aluminum tripolyphosphate anti-flash rust additive: 0.27wt.%

[0069] Component B:

[0070] Co-solvent (mixed co-solvent of n-butanol, xylene and dipropylene glycol butyl ether in a mass ratio of 5:2:1): 5wt.%

[0071] Curing agent (polyamide 650 and phenolic amine T-31 composite curing agent with a mass ratio of 10:3): 5.6wt.%

[0072] (1) Preparation of conductive polymer modified graphene powder

[0073] The few-layer graphene and polyaniline are matched according to a mass ratio, and the two are uniformly mixed by a high-energy ball milling method, which is characterized in that before ball milling, the balls, the tank and the sample to be milled are heated at 60°C, and then the few-layer graphene powder and the conductive polymer powder are pre-mixed at a mass ratio of 4:1, and then the mixture is put into an agate ball milling tank, and agate balls and anhydrous ethanol are added, and the material-liquid ratio and the ball-to-material ratio are controlled to be 1:4 and 5:1 respectively, and ball milling is carried out with a planetary ball mill, and then vacuum drying is carried out at 60°C. After complete drying, a conductive polymer modified graphene powder composite material is obtained.

[0074] (2) Preparation of Component A

[0075] According to the component ratio of claim 1, it is characterized in that the silicone resin, epoxy resin, and co-solvent are stirred at a speed of 500-700 rpm for 10-20 min to obtain a uniform silicone resin / epoxy resin mixed solution; then a dispersant, carbon nanotubes / fibers, a conductive polymer modified graphene composite, and a defoamer are added and stirred at a speed of 500-700 rpm for 10-20 min, and then zinc powder, nano zinc oxide, nano titanium oxide, nano silicon oxide, silicon carbide, niobium carbide, niobium carbide, etc. are added and stirred at a speed of 1000-1200 rpm for 10-20 min, and finally an anti-flash rust additive is added and stirred at a speed of 1000-1200 rpm for 10-20 min to obtain slurry A.

[0076] (3) Preparation of Component B

[0077] According to the component ratio of claim 1, it is characterized in that the curing agent and the co-solvent are stirred at a rotation speed of 500-700 rpm for 10-20 min to obtain slurry B.

[0078] (4) Preparation of new heavy-duty anticorrosive coating by mixing components A and B

[0079] According to claim 1, it is characterized in that slurry B is added to slurry A, stirred at a speed of 1000-1200rpm for 10-20min, and then subsequent anti-corrosion coating brushing, spraying and other processes are carried out; and cured at room temperature to 70°C or under ultraviolet light for 2-5 hours to prepare a new high temperature resistant / wear-resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating.

[0080] This embodiment can be applied by spraying, rolling, brushing, etc. After testing, its specific performance is as follows

[0081] As shown in Table 1:

[0082]

[0083]

[0084]

[0085]

[0086] Embodiment 2, as Figure 1 As shown,

[0087] Preparation of a new type of high temperature resistant / wear resistant graphene-based organosilicon / epoxy resin composite heavy-duty anticorrosion coating Preparation of a new type of high temperature resistant / wear resistant graphene-based organosilicon / epoxy resin composite heavy-duty anticorrosion coating Component A:

[0088] Silicone epoxy resin: 29wt.%

[0089] Epoxy resin: 19wt.%

[0090] Co-solvent (mixed co-solvent of n-butanol, xylene and dipropylene glycol butyl ether in a mass ratio of 5:2:1): 9wt.%

[0091] Conductive polymer modified graphene powder (4:1 composite of few-layer graphene powder and polyaniline): 1wt.% Carbon nanotube / fiber: 1.5wt.%

[0092] Nano zinc oxide: 4wt.%

[0093] Nano titanium oxide: 4wt.%

[0094] Nano silicon oxide: 3wt.%

[0095] Silicon carbide: 3wt.%

[0096] Niobium carbide: 3wt.%

[0097] Zinc powder: aluminum powder (mass ratio 5:1): 10wt.%

[0098] Acrylic alkyd phenol dispersant: 1.6wt.%

[0099] Silicone defoamer: 1.4wt.%

[0100] Aluminum tripolyphosphate anti-flash rust additive: 0.5wt.%

[0101] Component B:

[0102] Co-solvent (mixed co-solvent of n-butanol, xylene and dipropylene glycol butyl ether in a mass ratio of 5:2:1): 5wt.%

[0103] Curing agent (composite curing agent of polyamide 650, phenolic amine T-31 and KH560 with a mass ratio of 10:3:1): 5wt.%

[0104] (1) Preparation of conductive polymer modified graphene powder

[0105] The few-layer graphene and polyaniline are matched according to a mass ratio, and the two are uniformly mixed by a high-energy ball milling method, which is characterized in that before ball milling, the balls, the tank and the sample to be milled are heated at 60°C, and then the few-layer graphene powder and the conductive polymer powder are pre-mixed at a mass ratio of 4:1, and then the mixture is put into an agate ball milling tank, and agate balls and anhydrous ethanol are added, and the material-liquid ratio and the ball-to-material ratio are controlled to be 1:4 and 5:1 respectively, and ball milling is carried out with a planetary ball mill, and then vacuum drying is carried out at 60°C. After complete drying, a conductive polymer modified graphene powder composite material is obtained.

[0106] (2) Preparation of Component A

[0107] According to the component ratio of claim 1, it is characterized in that the silicone resin, epoxy resin, and co-solvent are stirred at a speed of 500-700 rpm for 10-20 min to obtain a uniform silicone resin / epoxy resin mixed solution; then a dispersant, carbon nanotubes / fibers, conductive polymer modified graphene composites, and a defoaming agent are added and stirred at a speed of 500-700 rpm for 10-20 min, and then zinc powder / aluminum powder, nano zinc oxide, nano titanium oxide, nano silicon oxide, silicon carbide, niobium carbide, niobium carbide, etc. are added and stirred at a speed of 1000-1200 rpm for 10-20 min, and finally an anti-flash rust additive is added and stirred at a speed of 1000-1200 rpm for 10-20 min to obtain slurry A.

[0108] (3) Preparation of Component B

[0109] According to the component ratio of claim 1, it is characterized in that the curing agent and the co-solvent are stirred at a rotation speed of 500-700 rpm for 10-20 min to obtain slurry B.

[0110] (4) Preparation of new heavy-duty anticorrosive coating by mixing components A and B

[0111] According to claim 1, it is characterized in that slurry B is added to slurry A, stirred at a speed of 1000-1200rpm for 10-20min, and then subsequent anti-corrosion coating brushing, spraying and other processes are carried out; and cured at room temperature to 70°C or under ultraviolet light for 2-5 hours to prepare a new high temperature resistant / wear-resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating.

[0112] This embodiment can be applied by spraying, rolling, brushing, etc. After testing, its specific performance is as follows

[0113] As shown in Table 1:

[0114]

[0115]

[0116]

[0117]

[0118]

[0119]

[0120]

[0121]

[0122]

[0123]

[0124] (1) The present invention utilizes conductive stone polymer modified graphene powder and carbon nanofiber to achieve electrical conductivity and high temperature resistance and corrosion resistance, and because a conductive network skeleton is formed, the amount of zinc powder / aluminum powder used is reduced; nano silicon oxide, nano zinc oxide, nano titanium oxide, silicon carbide, and niobium carbide can achieve wear resistance, high temperature resistance, and corrosion resistance. The novel high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating has the advantages of strong bonding with metal substrates and corrosion resistance.

[0125] (2) The novel high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating of the present invention can be specifically applied to cement clinker production lines, successfully filling the gap in the long-term use of anti-corrosion materials in cement kiln clinker production line equipment in China.

[0126] (3) The novel high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating prepared by the present invention can be coated by conventional coating processes such as brushing or spraying to form an anti-corrosion coating that integrates the bottom and the surface of the metal substrate. It uses silicone resin and epoxy resin composite as the base material graphene, modified carbon nanotubes as the coating functional enhancement agent, polyamide 650 and phenolic amine T-31 as the composite curing agent to form a high corrosion resistance system. Thanks to the conductive network formed by conductive polymer modified graphene, conductive polymer modified ultrafine ferrophosphorus powder and modified carbon nanotubes, the amount of zinc used in the coating can be reduced. The coating thickness formed on the metal surface by the obtained heavy-duty anti-corrosion composite coating is 300-1000μm, and it can resist corrosion damage of 200-350℃ and strong corrosive media such as hydrogen sulfide for a long time, solve the problem of high temperature and strong corrosion in clinker production equipment in the cement industry, and effectively protect the metal substrate of its production equipment.

[0127] The above embodiments are merely descriptions of preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary engineering and technical personnel in the field shall fall within the protection scope determined by the claims of the present invention.

[0128] The parts not involved in the present invention are the same as the prior art or can be implemented by using the prior art.

Claims

1. A graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating, characterized in that: The coating is composed of two components, A and B. Component A is composed of organic silicon / epoxy resin composite resin, co-solvent, graphene powder, carbon nanotube / fiber, nano silicon oxide, nano aluminum oxide, nano silicon carbide, nano niobium carbide, nano PTFE fine powder, zinc powder, aluminum powder, dispersant, defoamer and anti-flash rust additive, and component B is composed of co-solvent and curing agent. The specific coating formula is as follows by weight: Component A: Silicone resin: 10-45wt.% Epoxy resin: 5-20wt.% Cosolvent: 5-20wt.% Conductive polymer modified graphene powder: 0.1-2wt.% Carbon nanotubes / fibers: 1-10wt.% Nano zinc oxide: 1-10wt.% Nano titanium oxide: 1-10wt.% Nano silicon oxide: 1-10wt.% Silicon carbide: 1-10wt.% Niobium carbide: 1-10wt.% Zinc powder / aluminum powder: 5-25wt.% Dispersant: 0.2-3wt.% Defoamer: 0.2-3wt.% Anti-flash rust additive: 0.2-3wt.% Component B: Cosolvent: 5-15wt.% Curing agent: 3-10wt.% Add component B to component A, and cure at room temperature to 70°C or under ultraviolet light for 2-5 hours to prepare a new type of high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating; The silicone resin is one or more of pure silicone resin, modified silicone resin (methyl silicone containing methoxy groups), silicone polyester resin, silicone alkyd resin, silicone acrylic resin and silicone epoxy resin; The epoxy resin is one or more of bisphenol A epoxy resin, bisphenol S epoxy resin and epoxy novolac resin.

2. The graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating according to claim 1, characterized in that: The co-solvent is one or more of methanol, ethanol, toluene, xylene, n-butanol, 1,4-butanediol, acetone, ethylene glycol butyl ether, ethyl acetate, propylene glycol methyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, and dipropylene glycol butyl ether.

3. The graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating according to claim 1, characterized in that: The conductive polymer modified graphene powder is a composite of one or more conductive polymers selected from polyaniline (PANI), poly(3,4-ethylenedioxythiophene) (PEDOT), polyethylenedioxythiophene-polystyrene sulfonate (PEDOT:PSS) and few-layer graphene powder.

4. The graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating according to claim 1, characterized in that: The carbon nanotube / fiber may be one or both of carbon nanotube and carbon nanofiber, wherein the carbon nanotube is one or both of carboxylated and amino-treated single-walled nanotube or multi-walled carbon nanotube.

5. The graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating according to claim 1, characterized in that: The particle size of the nano zinc oxide is about 100-500nm; the particle size of the nano titanium oxide is about 10-100nm; the particle size of the nano silicon oxide is about 10-100nm; the particle size of the silicon carbide and niobium carbide is 1-10μm; the zinc powder / aluminum powder is one or both of zinc powder and aluminum powder.

6. The graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating according to claim 1, characterized in that: The dispersant is one or more of a polyurethane dispersant, an acrylic dispersant, and an acetylene alcohol dispersant.

7. The graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating according to claim 1, characterized in that: The defoaming agent is one or more of a mineral oil defoaming agent and a silicon defoaming agent (organic silicon, modified silicon polyether, polydimethylsiloxane (PDMS) and a mixture of silicon dioxide).

8. The graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating according to claim 1, characterized in that: The anti-flash rust additive is one or more of cationic salts (sodium nitrite, sodium molybdate, strontium chromate, zinc phosphate, strontium phosphosilicate, aluminum tripolyphosphate, zinc aluminum phosphate + zinc molybdate) or organic polymer amine anti-flash rust additives.

9. The graphene-based organosilicon / epoxy resin composite heavy-duty anticorrosion coating according to claim 1, characterized in that: The curing agent is one or more of polyamide 650, polyamide 651, polyamide 910, phenolic amine T-31, polythiol QE-340M, polythiol GPM-800, ethylenediamine, hexamethylenediamine, diethylenetriamine, tetraethylenepentamine, diethylaminopropylamine, 4,4′-diaminodiphenyl sulfone, m-phenylenediamine, tetraethyl orthosilicate, silane coupling agent KH-560, KH-550.

10. A method for preparing a graphene-based silicone / epoxy resin composite heavy-duty anticorrosive coating, characterized in that: The preparation method of the novel high temperature resistant / wear resistant graphene-based silicone / epoxy resin composite heavy-duty anticorrosion coating is characterized by comprising the following steps: (1) Preparation of conductive polymer modified graphene powder The few-layer graphene and the conductive polymer powder (one or more than two of PANI, PEDOT, PEDOT:PSS) are mixed according to a mass ratio, and the two are uniformly mixed by a high-energy ball milling method, characterized in that before ball milling, the balls, the tank and the sample to be milled are heated at 60°C, and then the few-layer graphene powder and the conductive polymer powder are pre-mixed at a mass ratio of 5-1:1, and then the mixture is put into an agate ball milling tank, agate balls and anhydrous ethanol are added, and the material-liquid ratio and the ball-to-material ratio are controlled to be 1:3-5: and 4-6:1 respectively, and ball milling is performed with a planetary ball mill, and then vacuum drying is performed at 60°C. After complete drying, a conductive polymer modified graphene powder composite material is obtained; (2) Preparation of Component A: The component ratio is characterized in that the silicone resin, epoxy resin and co-solvent are stirred at a speed of 500-700 rpm for 10-20 minutes to obtain a uniform silicone resin / epoxy resin mixed solution; then a dispersant, carbon nanotubes / fibers, conductive polymer modified graphene composites and defoaming agents are added and stirred at a speed of 500-700 rpm for 10-20 minutes, and then zinc powder / aluminum powder, nano zinc oxide, nano titanium oxide, nano silicon oxide, silicon carbide, niobium carbide, niobium carbide and the like are added and stirred at a speed of 1000-1200 rpm for 10-20 minutes, and finally an anti-flash rust additive is added and stirred at a speed of 1000-1200 rpm for 10-20 minutes to obtain slurry A; (3) Preparation of Component B: Stir the curing agent and the co-solvent at a speed of 500-700 rpm for 10-20 min to obtain slurry B; (4) Components A and B are mixed to prepare a new type of heavy-duty anti-corrosion coating: Add slurry B to slurry A, stir at 1000-1200 rpm for 10-20 min, and then carry out subsequent anti-corrosion coating brushing, spraying and other processes; cure at room temperature to 70°C or under ultraviolet light for 2-5 hours to prepare a new high temperature resistant / wear-resistant graphene-based silicone / epoxy resin composite heavy-duty anti-corrosion coating.

Citation Information

Patent Citations

  • High-temperature-resistant, wear-resistant and corrosion-resistant coating and preparation method thereof

    CN108102479A

  • Wear-resistant anti-corrosion coating material and preparation method and application thereof

    CN109486339A

  • Graphene-based high-temperature-resistant anticorrosive paint and preparation method thereof

    CN111057438A

  • Wear-resistant and corrosion-resistant powder coating for tubing coupling and preparation method and application thereof

    CN111500159A

  • Conductive polymer modified graphene-based epoxy low-zinc heavy anti-corrosion coating and preparation method thereof

    CN116694195A

Cited By

  • Epoxy binding material for paving steel bridge deck in marine environment and application of epoxy binding material

    CN122503057A