Swelling adhesive tape for lithium battery
By using modified magnesium hydroxide-reinforced swelling tape, the problems of swelling pressure control and flame retardancy of lithium batteries under high temperature or overcharge conditions are solved, thereby improving the safety and performance of lithium batteries.
Patent Information
- Application Number
- CN202411265458.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing swelling adhesive tapes for lithium batteries have insufficient expansion performance under high temperature or overcharge conditions, making them prone to delamination, which leads to a decrease in battery safety and performance, and insufficient flame retardancy, posing a risk of spontaneous combustion.
Using natural rubber, synthetic rubber, silicone rubber and vinyl acetate copolymer as base materials, modified magnesium hydroxide is added, and modified by dipropyl aluminum hypophosphite and melamine polyphosphate, a swelling tape with excellent expansion and flame retardant properties is prepared.
It effectively controls the expansion pressure of lithium batteries under high temperature or overcharge conditions, improves battery safety performance, and significantly enhances the flame retardant performance of the swelling tape through synergistic flame retardant effect.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of swelling tapes, in particular to a swelling tape for lithium batteries. Background Art
[0002] With the rapid development of the new energy industry, the safety of new energy batteries has attracted much attention. In the manufacturing of battery cells, especially in the design process of lithium batteries, in order to facilitate the assembly of the battery cell and the shell, a certain gap must be reserved between the two. The existence of the gap causes the battery to shake and collide during long-term use, causing the positive and negative ears of the battery cell to break, thereby affecting the service life of the battery, and causing the battery to have risks such as battery short circuit due to the relative movement of the battery cell and the shell during use. In addition, lithium batteries may cause the internal pressure of the battery to increase in a high temperature environment or overcharged state. If this pressure cannot be effectively controlled, it may cause safety problems such as battery rupture or combustion. In the prior art, swelling tape is usually used to control the expansion of lithium batteries. However, due to the limited expansion performance of the swelling tape on the market, the ability to cope with high temperature or overcharge is insufficient. After being soaked in high temperature and electrolyte, it is easy to open the glue and the swelling rate is low, which affects the performance of the battery. In addition, the heating of lithium batteries is easy to cause spontaneous combustion, which in turn causes certain damage to the personal and property safety of users. Therefore, it is urgent to provide a swelling tape for lithium batteries to solve the shortcomings of the prior art. Summary of the invention
[0003] In view of the deficiencies in the prior art, the object of the present invention is to provide a swelling tape for a lithium battery, which has excellent expansion performance and pressure relief capability, can effectively control the expansion pressure generated by the lithium battery under high temperature or overcharge conditions, thereby improving the safety performance of the battery, and can greatly improve the flame retardant properties of the swelling tape.
[0004] In order to solve the above technical problems, the present invention provides a swelling tape for lithium batteries, which is prepared by the following raw materials in parts by weight: 60-80 parts of base material, 25-40 parts of foaming agent, 8-15 parts of first antioxidant, 8-15 parts of binder, wherein the mass ratio of the base material, foaming agent, first antioxidant and binder is 70:30:10:10; Wherein, the base material is prepared from the following raw materials in parts by weight: 10-15 parts of natural rubber, 20-30 parts of synthetic rubber, 10-15 parts of silicone rubber, and 20-30 parts of vinyl acetate copolymer, wherein the mass ratio of the natural rubber to the synthetic rubber is 1:2, and the mass ratio of the silicone rubber to the vinyl acetate copolymer is 1:2.
[0005] As a preferred solution of the present invention, the synthetic rubber is prepared from the following raw materials in parts by weight: 50-60 parts of EPDM rubber, 5-10 parts of epoxy resin, 5-10 parts of white carbon black, 15-25 parts of modified magnesium hydroxide, 1-2 parts of a second antioxidant, 3-8 parts of an accelerator, 2-5 parts of a vulcanizing agent, and 1-3 parts of a lubricant, wherein the modified magnesium hydroxide is obtained by modifying magnesium hydroxide with dipropyl aluminum hypophosphite and melamine polyphosphate; The preparation method of the modified magnesium hydroxide comprises: adding dipropyl aluminum hypophosphite and melamine polyphosphate into water and mixing them to obtain a modifier, and adding magnesium hydroxide into the modifier to obtain the modified magnesium hydroxide.
[0006] As a preferred embodiment of the present invention, the mass ratio of the magnesium hydroxide, dipropyl aluminum hypophosphite and melamine polyphosphate is 100:(4-6):(2-3).
[0007] As a preferred embodiment of the present invention, the method for preparing the synthetic rubber comprises the following steps: S11, adding a specified amount of EPDM rubber and epoxy resin into an internal mixer for mixing; S12, adding a specified amount of white carbon black, modified magnesium hydroxide, an antioxidant, a accelerator, and a lubricant into an internal mixer and mixing them, and then adding a vulcanizing agent and mixing them to obtain a rubber mixture; S13, extruding the mixed rubber through an extruder to obtain synthetic rubber.
[0008] As a preferred embodiment of the present invention, the foaming agent is any one of azodicarbonamide, azobisisoheptanenitrile and 4,4'-oxybisbenzenesulfonylhydrazide.
[0009] As a preferred embodiment of the present invention, the first antioxidant is any one of antioxidant 1010, antioxidant 168, and antioxidant 1076.
[0010] As a preferred embodiment of the present invention, the binder is any one of styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer and styrene-ethylene-butylene-styrene block copolymer.
[0011] As a preferred solution of the present invention, it is prepared by including the following raw materials in parts by weight: 70 parts of base material, 30 parts of foaming agent, 12 parts of first antioxidant, and 12 parts of binder, wherein the mass ratio of the base material, foaming agent, first antioxidant and binder is 70:30:10:10; Wherein, the base material is prepared from the following raw materials in parts by weight: 13 parts of natural rubber, 25 parts of synthetic rubber, 12 parts of silicone rubber, and 25 parts of vinyl acetate copolymer, wherein the mass ratio of the natural rubber to the synthetic rubber is 1:2, and the mass ratio of the silicone rubber to the vinyl acetate copolymer is 1:2.
[0012] As a preferred embodiment of the present invention, the method for preparing the swelling tape for lithium batteries comprises the following steps: S21, adding a specified amount of natural rubber and synthetic rubber into a first internal mixer and mixing them in proportion to obtain a rubber mixture; S22, adding a specified amount of silicone rubber and vinyl acetate copolymer into a second internal mixer and mixing them in proportion to obtain a copolymer mixture; S23, subjecting the rubber mixture and the copolymer mixture to a hot pressing treatment to obtain an expansion tape material; S24, adding a specified amount of a foaming agent, a first antioxidant, and a binder into a third internal mixer and mixing them in proportion, and then adding the expansion tape material into the third internal mixer for heating and mixing, so that the components are fully melted and mixed, and then extruding through an extruder to obtain a swelling tape material; S25, pouring the heated swelling tape material into a mold, and performing calendering, pressing, and slicing to obtain a swelling tape semi-finished product; S26, cooling and shaping the swollen adhesive tape semi-finished product to obtain a swollen adhesive tape finished product.
[0013] As a preferred embodiment of the present invention, the method for preparing the swellable tape product for lithium battery comprises the following steps: S31, winding the swollen tape product on the surface of the lithium battery; S32, placing the lithium battery wrapped with the finished swelling tape into a battery housing, installing a battery cover, and obtaining a finished lithium battery.
[0014] Compared with the prior art, the present invention has the following beneficial effects: The swelling tape for lithium batteries in the present invention is composed of natural rubber, synthetic rubber, silicone rubber and vinyl acetate copolymer, has excellent expansion performance and pressure relief ability, can effectively control the expansion pressure generated by lithium batteries under high temperature or overcharge conditions, thereby improving the safety performance of the battery. By adding modified magnesium hydroxide to the synthetic rubber, the prepared swelling tape has better flame retardant properties. Dipropyl aluminum hypophosphite and polyphosphate melamine jointly modify the magnesium hydroxide. Dipropyl aluminum hypophosphite decomposes into volatile phosphides and captures free radicals generated by combustion to inhibit combustion. Polyphosphate melamine decomposes in the polymer to generate non-combustible gas and absorbs heat generated by the polymer, thereby generating a synergistic flame retardant effect, greatly improving the flame retardant properties of the swelling tape. DETAILED DESCRIPTION
[0015] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0016] The specific raw materials mentioned in the following examples can all be obtained commercially, and the techniques and equipment used are well known to those skilled in the art.
[0017] The present invention provides a technical solution: A swelling tape for lithium battery, comprising the following raw materials in parts by weight: 60-80 parts of base material, 25-40 parts of foaming agent, 8-15 parts of first antioxidant, 8-15 parts of binder, wherein the mass ratio of the base material, foaming agent, first antioxidant and binder is 70:30:10:10; Wherein, the base material is prepared from the following raw materials in parts by weight: 10-15 parts of natural rubber, 20-30 parts of synthetic rubber, 10-15 parts of silicone rubber, and 20-30 parts of vinyl acetate copolymer, wherein the mass ratio of the natural rubber to the synthetic rubber is 1:2, and the mass ratio of the silicone rubber to the vinyl acetate copolymer is 1:2.
[0018] In this embodiment, the synthetic rubber is prepared from the following raw materials in parts by weight: 50-60 parts of EPDM rubber, 5-10 parts of epoxy resin, 5-10 parts of white carbon black, 15-25 parts of modified magnesium hydroxide, 1-2 parts of a second antioxidant, 3-8 parts of an accelerator, 2-5 parts of a vulcanizing agent, and 1-3 parts of a lubricant, wherein the modified magnesium hydroxide is obtained by modifying magnesium hydroxide with dipropyl aluminum hypophosphite and melamine polyphosphate; The preparation method of the modified magnesium hydroxide comprises: adding dipropyl aluminum hypophosphite and melamine polyphosphate into water and mixing them to obtain a modifier, and adding magnesium hydroxide into the modifier to obtain the modified magnesium hydroxide.
[0019] In this embodiment, the mass ratio of magnesium hydroxide, dipropyl aluminum hypophosphite and melamine polyphosphate is 100:(4-6):(2-3).
[0020] In this embodiment, the method for preparing the synthetic rubber comprises the following steps: S11, adding a specified amount of EPDM rubber and epoxy resin into an internal mixer for mixing; S12, adding a specified amount of white carbon black, modified magnesium hydroxide, an antioxidant, a accelerator, and a lubricant into an internal mixer and mixing them, and then adding a vulcanizing agent and mixing them to obtain a rubber mixture; S13, extruding the mixed rubber through an extruder to obtain synthetic rubber.
[0021] In this embodiment, the foaming agent is any one of azodicarbonamide, azobisisoheptanenitrile, and 4,4'-oxybisbenzenesulfonylhydrazide.
[0022] In this embodiment, the first antioxidant is any one of antioxidant 1010 , antioxidant 168 , and antioxidant 1076 .
[0023] In this embodiment, the binder is any one of styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer, and styrene-ethylene-butylene-styrene block copolymer.
[0024] In this embodiment, the following raw materials are included in parts by weight: 70 parts of base material, 30 parts of foaming agent, 12 parts of first antioxidant, and 12 parts of binder, wherein the mass ratio of the base material, foaming agent, first antioxidant and binder is 70:30:10:10; Wherein, the base material is prepared from the following raw materials in parts by weight: 13 parts of natural rubber, 25 parts of synthetic rubber, 12 parts of silicone rubber, and 25 parts of vinyl acetate copolymer, wherein the mass ratio of the natural rubber to the synthetic rubber is 1:2, and the mass ratio of the silicone rubber to the vinyl acetate copolymer is 1:2.
[0025] In this embodiment, the method for preparing the swelling tape for lithium battery comprises the following steps: S21, adding a specified amount of natural rubber and synthetic rubber into a first internal mixer and mixing them in proportion to obtain a rubber mixture; S22, adding a specified amount of silicone rubber and vinyl acetate copolymer into a second internal mixer and mixing them in proportion to obtain a copolymer mixture; S23, subjecting the rubber mixture and the copolymer mixture to a hot pressing treatment to obtain an expansion tape material; S24, adding a specified amount of a foaming agent, a first antioxidant, and a binder into a third internal mixer and mixing them in proportion, and then adding the expansion tape material into the third internal mixer for heating and mixing, so that the components are fully melted and mixed, and then extruding through an extruder to obtain a swelling tape material; S25, pouring the heated swelling tape material into a mold, and performing calendering, pressing, and slicing to obtain a swelling tape semi-finished product; S26, cooling and shaping the swollen adhesive tape semi-finished product to obtain a swollen adhesive tape finished product.
[0026] In this embodiment, the method for preparing the swellable tape product for lithium battery comprises the following steps: S31, winding the swollen tape product on the surface of the lithium battery; S32, placing the lithium battery wrapped with the finished swelling tape into a battery housing, installing a battery cover, and obtaining a finished lithium battery.
[0027] The swelling tape for lithium batteries in the present invention is composed of natural rubber, synthetic rubber, silicone rubber and vinyl acetate copolymer, has excellent expansion performance and pressure relief ability, can effectively control the expansion pressure generated by lithium batteries under high temperature or overcharge conditions, thereby improving the safety performance of the battery. By adding modified magnesium hydroxide to the synthetic rubber, the prepared swelling tape has better flame retardant properties. Dipropyl aluminum hypophosphite and polyphosphate melamine jointly modify the magnesium hydroxide. Dipropyl aluminum hypophosphite decomposes into volatile phosphides and captures free radicals generated by combustion to inhibit combustion. Polyphosphate melamine decomposes in the polymer to generate non-combustible gas and absorbs heat generated by the polymer, thereby generating a synergistic flame retardant effect, greatly improving the flame retardant properties of the swelling tape. Specific implementation cases
[0028] Example 1 A swelling tape for lithium battery, comprising the following raw materials in parts by weight: 70 parts of base material, 30 parts of foaming agent, 10 parts of first antioxidant, and 10 parts of binder, wherein the mass ratio of the base material, foaming agent, first antioxidant and binder is 70:30:10:10; Wherein, the base material is prepared from the following raw materials in parts by weight: 13 parts of natural rubber, 25 parts of synthetic rubber, 12 parts of silicone rubber, and 25 parts of vinyl acetate copolymer, wherein the mass ratio of the natural rubber to the synthetic rubber is 1:2, and the mass ratio of the silicone rubber to the vinyl acetate copolymer is 1:2.
[0029] In this embodiment, the foaming agent is azodicarbonamide, the first antioxidant is antioxidant 1010, and the binder is styrene-butadiene-styrene block copolymer.
[0030] The synthetic rubber is prepared from the following raw materials in parts by weight: 55 parts of EPDM rubber, 7 parts of epoxy resin, 7 parts of white carbon black, 20 parts of modified magnesium hydroxide, 1.5 parts of a second antioxidant, 5 parts of an accelerator, 4 parts of a vulcanizing agent, and 2 parts of a lubricant, wherein the modified magnesium hydroxide is obtained by modifying magnesium hydroxide with dipropyl aluminum hypophosphite and melamine polyphosphate; The preparation method of the modified magnesium hydroxide comprises: adding dipropyl aluminum hypophosphite and melamine polyphosphate into water and mixing them to obtain a modifier, and adding magnesium hydroxide into the modifier to obtain the modified magnesium hydroxide.
[0031] In this embodiment, the mass ratio of the magnesium hydroxide, dipropyl aluminum hypophosphite and melamine polyphosphate is 100:5:2.5.
[0032] In this embodiment, the method for preparing the synthetic rubber comprises the following steps: S11, adding a specified amount of EPDM rubber and epoxy resin into an internal mixer for mixing; S12, adding a specified amount of white carbon black, modified magnesium hydroxide, an antioxidant, a accelerator, and a lubricant into an internal mixer and mixing them, and then adding a vulcanizing agent and mixing them to obtain a rubber mixture; S13, extruding the mixed rubber through an extruder to obtain synthetic rubber.
[0033] In this embodiment, the method for preparing the swelling tape for lithium battery comprises the following steps: S21, adding a specified amount of natural rubber and synthetic rubber into a first internal mixer and mixing them in proportion to obtain a rubber mixture; S22, adding a specified amount of silicone rubber and vinyl acetate copolymer into a second internal mixer and mixing them in proportion to obtain a copolymer mixture; S23, subjecting the rubber mixture and the copolymer mixture to a hot pressing treatment to obtain an expansion tape material; S24, adding a specified amount of a foaming agent, a first antioxidant, and a binder into a third internal mixer and mixing them in proportion, and then adding the expansion tape material into the third internal mixer for heating and mixing, so that the components are fully melted and mixed, and then extruding through an extruder to obtain a swelling tape material; S25, pouring the heated swelling tape material into a mold, and performing calendering, pressing, and slicing to obtain a swelling tape semi-finished product; S26, cooling and shaping the swollen adhesive tape semi-finished product to obtain a swollen adhesive tape finished product.
[0034] In this embodiment, the method for preparing the swellable tape product for lithium battery comprises the following steps: S31, winding the swollen tape product on the surface of the lithium battery; S32, placing the lithium battery wrapped with the finished swelling tape into the battery housing, installing the battery cover, and obtaining the finished lithium battery. 60-80 parts of base material, 25-40 parts of foaming agent, 8-15 parts of first antioxidant, 8-15 parts of binder, the mass ratio of the base material, foaming agent, first antioxidant and binder is 70:30:10:10 Example 2 A swelling tape for lithium battery, comprising the following raw materials in parts by weight: 77 parts of base material, 33 parts of foaming agent, 11 parts of first antioxidant, and 11 parts of binder, wherein the mass ratio of the base material, the foaming agent, the first antioxidant and the binder is 70:30:10:10; Wherein, the base material is prepared from the following raw materials in parts by weight: 13 parts of natural rubber, 25 parts of synthetic rubber, 12 parts of silicone rubber, and 25 parts of vinyl acetate copolymer, wherein the mass ratio of the natural rubber to the synthetic rubber is 1:2, and the mass ratio of the silicone rubber to the vinyl acetate copolymer is 1:2.
[0035] In this embodiment, the foaming agent is azodicarbonamide, the first antioxidant is antioxidant 1010, and the binder is styrene-butadiene-styrene block copolymer.
[0036] The synthetic rubber is prepared from the following raw materials in parts by weight: 55 parts of EPDM rubber, 7 parts of epoxy resin, 7 parts of white carbon black, 20 parts of modified magnesium hydroxide, 1.5 parts of a second antioxidant, 5 parts of an accelerator, 4 parts of a vulcanizing agent, and 2 parts of a lubricant, wherein the modified magnesium hydroxide is obtained by modifying magnesium hydroxide with dipropyl aluminum hypophosphite and melamine polyphosphate; The preparation method of the modified magnesium hydroxide comprises: adding dipropyl aluminum hypophosphite and melamine polyphosphate into water and mixing them to obtain a modifier, and adding magnesium hydroxide into the modifier to obtain the modified magnesium hydroxide.
[0037] In this embodiment, the mass ratio of the magnesium hydroxide, dipropyl aluminum hypophosphite and melamine polyphosphate is 100:5:2.5.
[0038] In this embodiment, the method for preparing the synthetic rubber comprises the following steps: S11, adding a specified amount of EPDM rubber and epoxy resin into an internal mixer for mixing; S12, adding a specified amount of white carbon black, modified magnesium hydroxide, an antioxidant, a accelerator, and a lubricant into an internal mixer and mixing them, and then adding a vulcanizing agent and mixing them to obtain a rubber mixture; S13, extruding the mixed rubber through an extruder to obtain synthetic rubber.
[0039] In this embodiment, the method for preparing the swelling tape for lithium battery comprises the following steps: S21, adding a specified amount of natural rubber and synthetic rubber into a first internal mixer and mixing them in proportion to obtain a rubber mixture; S22, adding a specified amount of silicone rubber and vinyl acetate copolymer into a second internal mixer and mixing them in proportion to obtain a copolymer mixture; S23, subjecting the rubber mixture and the copolymer mixture to a hot pressing treatment to obtain an expansion tape material; S24, adding a specified amount of a foaming agent, a first antioxidant, and a binder into a third internal mixer and mixing them in proportion, and then adding the expansion tape material into the third internal mixer for heating and mixing, so that the components are fully melted and mixed, and then extruding through an extruder to obtain a swelling tape material; S25, pouring the heated swelling tape material into a mold, and performing calendering, pressing, and slicing to obtain a swelling tape semi-finished product; S26, cooling and shaping the swollen adhesive tape semi-finished product to obtain a swollen adhesive tape finished product.
[0040] In this embodiment, the method for preparing the swellable tape product for lithium battery comprises the following steps: S31, winding the swollen tape product on the surface of the lithium battery; S32, placing the lithium battery wrapped with the finished swelling tape into a battery housing, installing a battery cover, and obtaining a finished lithium battery. Comparative Example 1
[0041] The difference between Comparative Example 1 and Example 1 is that the synthetic rubber described in Comparative Example 1 is different from that in Example 1, and the other parts are the same; In this comparative example, the synthetic rubber does not contain modified magnesium hydroxide. Comparative Example 2
[0042] The difference between Comparative Example 2 and Example 1 is that the synthetic rubber described in Comparative Example 2 is different from that in Example 1, and the others are the same; In this comparative example, the magnesium hydroxide in the synthetic rubber is unmodified. Comparative Example 3
[0043] The difference between Comparative Example 3 and Example 1 is that the modified magnesium hydroxide in the synthetic rubber described in Comparative Example 3 is different from that in Example 1, and the others are the same; In this comparative example, the modified magnesium hydroxide was only modified by dipropyl aluminum hypophosphite, and the mass ratio of magnesium hydroxide to dipropyl aluminum hypophosphite was 100:5. Comparative Example 4
[0044] The difference between Comparative Example 4 and Example 1 is that the modified magnesium hydroxide in the synthetic rubber described in Comparative Example 4 is different from that in Example 1, and the others are the same; In this comparative example, the modified magnesium hydroxide was only modified by melamine polyphosphate, and the mass ratio of magnesium hydroxide to melamine polyphosphate was 100:2.5. Comparative Example 5
[0045] The swelling tape produced by Suzhou Bozhijun New Materials Co., Ltd. is used.
[0046] The swelling tapes prepared in the above-mentioned Examples 1-2 and Comparative Examples 1-5 were tested for total thickness according to GB / T7125-2014, tensile strength according to GB / T30776, and flame retardancy according to UL94-2006. Swelling rate test: the tapes were cut into 50 mm*50 mm sizes as test samples, and the test samples were immersed in electrolyte at 45°C / 60°C / 85°C for 4 hours, and then the test samples were taken out and flattened to test their thickness. Swelling rate = thickness after immersion / thickness before immersion*100%. The test results are shown in Table 1: Table 1 Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Total thickness / μm 87 86 87 89 88 85 87 45°C swelling rate / % 175 172 173 171 169 172 122 60°C swelling rate / % 193 172 188 189 185 182 134 85°C swelling rate / % 212 195 205 208 203 207 150 Tensile strength / MPa 137 134 135 133 136 132 114 Flame retardant V-0 V-0 V-1 V-1 V-1 V-1 V-1 It can be seen from the data in Table 1 that the swelling tape for lithium batteries prepared by the present invention has high swelling rate, tensile strength and flame retardancy. The swelling rate of the swelling tape reaches more than 200% at 85°C, and the flame retardancy reaches V-0, with good performance. It can be seen from the data of Comparative Examples 1-5 and Examples 1 and 2 that adding modified magnesium hydroxide obtained by modifying dipropyl aluminum hypophosphite and melamine polyphosphate to synthetic rubber can greatly improve the flame retardancy.
[0047] All technical features in this embodiment can be freely combined according to actual needs.
[0048] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present technical solution is within the protection scope of the present invention.
Claims
1. A swelling tape for lithium batteries, characterized in that: The method is prepared by comprising the following raw materials in parts by weight: 60-80 parts of base material, 25-40 parts of foaming agent, 8-15 parts of first antioxidant, 8-15 parts of binder, wherein the mass ratio of the base material, foaming agent, first antioxidant and binder is 70:30:10:10; Wherein, the base material is prepared from the following raw materials in parts by weight: 10-15 parts of natural rubber, 20-30 parts of synthetic rubber, 10-15 parts of silicone rubber, and 20-30 parts of vinyl acetate copolymer, wherein the mass ratio of the natural rubber to the synthetic rubber is 1:2, and the mass ratio of the silicone rubber to the vinyl acetate copolymer is 1:
2.
2. A swelling tape for lithium batteries according to claim 1, characterized in that: The synthetic rubber is prepared from the following raw materials in parts by weight: 50-60 parts of EPDM rubber, 5-10 parts of epoxy resin, 5-10 parts of white carbon black, 15-25 parts of modified magnesium hydroxide, 1-2 parts of a second antioxidant, 3-8 parts of an accelerator, 2-5 parts of a vulcanizing agent, and 1-3 parts of a lubricant, wherein the modified magnesium hydroxide is obtained by modifying magnesium hydroxide with dipropyl aluminum hypophosphite and melamine polyphosphate; The preparation method of the modified magnesium hydroxide comprises: adding dipropyl aluminum hypophosphite and melamine polyphosphate into water and mixing them to obtain a modifier, and adding magnesium hydroxide into the modifier to obtain the modified magnesium hydroxide.
3. A swelling tape for lithium batteries according to claim 2, characterized in that: The mass ratio of the magnesium hydroxide, dipropyl aluminum hypophosphite and melamine polyphosphate is 100:(4-6):(2-3).
4. A swelling tape for lithium batteries according to claim 3, characterized in that: The preparation method of the synthetic rubber comprises the following steps: S11, adding a specified amount of EPDM rubber and epoxy resin into an internal mixer for mixing; S12, adding a specified amount of white carbon black, modified magnesium hydroxide, an antioxidant, a accelerator, and a lubricant into an internal mixer and mixing them, and then adding a vulcanizing agent and mixing them to obtain a rubber mixture; S13, extruding the mixed rubber through an extruder to obtain synthetic rubber.
5. The swelling tape for lithium battery according to claim 1, characterized in that: The foaming agent is any one of azodicarbonamide, azobisisoheptanenitrile and 4,4'-oxybisbenzenesulfonylhydrazide.
6. A swelling tape for lithium battery according to claim 1, characterized in that: The first antioxidant is any one of antioxidant 1010 , antioxidant 168 , and antioxidant 1076 .
7. The swelling tape for lithium battery according to claim 1, characterized in that: The binder is any one of styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer and styrene-ethylene-butylene-styrene block copolymer.
8. The swelling tape for lithium battery according to claim 1, characterized in that: The method is prepared by comprising the following raw materials in parts by weight: 70 parts of base material, 30 parts of foaming agent, 12 parts of first antioxidant, and 12 parts of binder, wherein the mass ratio of the base material, foaming agent, first antioxidant and binder is 70:30:10:10; Wherein, the base material is prepared from the following raw materials in parts by weight: 13 parts of natural rubber, 25 parts of synthetic rubber, 12 parts of silicone rubber, and 25 parts of vinyl acetate copolymer, wherein the mass ratio of the natural rubber to the synthetic rubber is 1:2, and the mass ratio of the silicone rubber to the vinyl acetate copolymer is 1:
2.
9. A swelling tape for lithium batteries according to claims 1-8, characterized in that: The preparation method of the swelling tape for lithium battery comprises the following steps: S21, adding a specified amount of natural rubber and synthetic rubber into a first internal mixer and mixing them in proportion to obtain a rubber mixture; S22, adding a specified amount of silicone rubber and vinyl acetate copolymer into a second internal mixer and mixing them in proportion to obtain a copolymer mixture; S23, subjecting the rubber mixture and the copolymer mixture to a hot pressing treatment to obtain an expansion tape material; S24, adding a specified amount of a foaming agent, a first antioxidant, and a binder into a third internal mixer and mixing them in proportion, and then adding the expansion tape material into the third internal mixer for heating and mixing, so that the components are fully melted and mixed, and then extruding through an extruder to obtain a swelling tape material; S25, pouring the heated swelling tape material into a mold, and performing calendering, pressing, and slicing to obtain a swelling tape semi-finished product; S26, cooling and shaping the swollen adhesive tape semi-finished product to obtain a swollen adhesive tape finished product.
10. A swelling tape for lithium batteries according to claim 9, characterized in that: The method for preparing the swellable adhesive tape finished product for lithium battery comprises the following steps: S31, winding the swollen tape product on the surface of the lithium battery; S32, placing the lithium battery wrapped with the finished swelling tape into a battery housing, installing a battery cover, and obtaining a finished lithium battery.