Preparation method of natural latex-polyvinyl alcohol adhesive
By preparing a natural latex-polyvinyl alcohol adhesive, the problems of pollution from fossil-based adhesives and poor bonding performance of natural latex have been solved, providing a green and environmentally friendly cardboard box adhesive with strong adhesion to meet the needs of cardboard box bonding.
Patent Information
- Application Number
- CN202411119776.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
Existing fossil-based adhesives cause serious environmental pollution and have poor bonding effects, while natural latexes have poor bonding effects on polar materials, making it difficult to meet the bonding requirements of cardboard boxes.
A natural latex-polyvinyl alcohol adhesive was prepared by mixing natural latex with 50% S dispersion, 40% ZnO dispersion, 10% polyvinyl alcohol solution, stabilizer, dispersant and accelerator in a certain proportion and carrying out a vulcanization reaction, thereby improving adhesion and stability.
The prepared adhesive is environmentally friendly, has strong adhesion, excellent water resistance and stability, and meets the requirements for cardboard box bonding.
Smart Images

Figure CN118931427A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a packaging carton adhesive, and more particularly to a preparation method and application of a natural latex-polyvinyl alcohol adhesive. Background Art
[0002] Cartons are the most widely used packaging products. With the trend of online shopping, packaging cartons have become one of the indispensable items in the logistics process, bearing the important responsibilities of containing, protecting products and aesthetics. The compressive strength of packaging cartons depends not only on the comprehensive ring crush strength of the cardboard, but also on the bonding effect of the corrugated cardboard. The adhesive directly determines the bonding effect of the cardboard. The quality of the bonding effect directly affects the edge pressure of the cardboard. At the same time, the adhesive performance also affects the moisture return and moisture absorption of the cardboard.
[0003] Fossil-based adhesives, mainly polyurethane glue and trialdehyde glue (urea-formaldehyde glue, melamine resin glue, phenolic resin glue), have advantages such as good stability, low cost and fast drying. However, the greenhouse gases and formaldehyde produced by fossil-based adhesives pollute the environment and are harmful to human health. In addition, fossil resources are non-renewable and are facing the situation of resource depletion. Natural polymer materials based on renewable resources have the advantages of being cheap and environmentally friendly. Using them as adhesives has become a hot topic for research and development at home and abroad. Water-based adhesives stand out for their advantages such as being non-flammable, safe to use, and avoiding the harm of organic solvents to the human body.
[0004] Among many raw materials, natural rubber latex has strong self-adhesiveness, fast adhesion, easy molding, good comprehensive properties (such as high elasticity, high strength, wear resistance, tear resistance, corrosion resistance, flexibility, etc.), good film-forming properties, small creep, large cohesion and high temperature resistance, etc. It is a good material for making water-based adhesives. However, natural rubber latex itself is a non-polar molecule, and its bonding effect on polar materials such as cartons is relatively poor. Therefore, it is of great significance to improve natural rubber latex (NRL) to increase its bonding strength and adhesion to cartons. Summary of the invention
[0005] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0006] The purpose of the invention is to provide a natural latex-polyvinyl alcohol adhesive which is green and environmentally friendly, has strong bonding strength, excellent water resistance and stability, and is used for gluing packaging cartons.
[0007] In order to achieve these purposes and other advantages according to the present invention, a method for preparing a natural latex-polyvinyl alcohol adhesive is provided, characterized in that it is prepared from the following raw materials in parts by weight: 88-100 parts of natural latex, 1.5 parts of 50% S dispersion, 0.5 parts of 40% ZnO dispersion, 5-60 parts of 10% polyvinyl alcohol solution, 0.5 parts of stabilizer, 2.0 parts of diffusant, and 0.5 parts of accelerator;
[0008] The preparation method of the natural latex-polyvinyl alcohol adhesive comprises the following steps:
[0009] Step 1, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water in a beaker according to a weight ratio, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and standing for more than 12 hours for later use;
[0010] Step 2, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water according to the weight ratio into a beaker, stirring continuously for 5-8 hours, and leaving for more than 12 hours for later use;
[0011] Step 3, preparing the 10% polyvinyl alcohol solution: adding 10 parts of polyvinyl alcohol and 90 parts of soft water into a beaker according to weight, stirring at 90° C. for 60 minutes until the polyvinyl alcohol is dissolved, and cooling to room temperature for later use;
[0012] Step 4: Add 88-100 parts of the natural rubber latex, 1.5 parts of the 50% S dispersion, 0.5 parts of the 40% ZnO dispersion, 5-60 parts of the 10% polyvinyl alcohol solution, 0.5 parts of the stabilizer, 2.0 parts of the diffusant, and 0.5 parts of the accelerator into a beaker according to a proportion by weight, heat to 40-60° C., carry out a vulcanization reaction at a stirring speed of 300-330 rpm for 20-60 minutes, and cool to room temperature.
[0013] Preferably, the stabilizer is one or both of 10% casein solution and 10% KOH solution.
[0014] Preferably, the preparation method of the 10% casein solution is as follows: weigh out the ingredients according to weight proportions of casein 10 parts, borax 1.5 parts, 28% ammonia water 3.2 parts and soft water 85.3 parts, and heat and stir until the ingredients are completely dissolved.
[0015] Preferably, the 10% KOH solution is prepared as follows: 10 parts of KOH and 90 parts of soft water are added into a beaker by weight and stirred continuously until all the KOH is dissolved.
[0016] Preferably, the diffusing agent is a 10% NF solution, and the preparation method of the 10% NF solution is as follows: 10 parts of NF and 90 parts of soft water are added into a beaker by weight and stirred until the NF is completely dissolved, and then cooled at room temperature for use.
[0017] Preferably, the accelerator is a 50% ZDC dispersion or a 50% ZBEC dispersion, and the preparation method of the 50% ZDC dispersion or the 50% ZBEC dispersion is as follows: grind ZDC or ZBEC powder in a mortar for later use; add 50 parts of ZDC or ZBEC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water in a beaker according to weight parts, stir continuously for 5-8 hours, and stand for more than 12 hours for later use.
[0018] Preferably, the polyvinyl alcohol in step three is any one of polyvinyl alcohol 1788, polyvinyl alcohol 1799, polyvinyl alcohol 2499, polyvinyl alcohol 2099, and polyvinyl alcohol 2488, or a combination of two of them.
[0019] Preferably, the vulcanization reaction time in step 4 is 40 minutes and the vulcanization reaction temperature is 40°C.
[0020] The present invention at least includes the following beneficial effects: the natural latex-polyvinyl alcohol adhesive prepared by the present invention is green and environmentally friendly, has strong bonding strength, excellent water resistance and stability, and can fully meet the requirements of carton bonding.
[0021] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The present invention is a flow chart of a method for preparing a natural latex-polyvinyl alcohol adhesive. DETAILED DESCRIPTION
[0023] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0024] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0025] Example 1
[0026] Step 1, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water in a beaker according to a weight ratio, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and standing for more than 12 hours for later use;
[0027] Step 2, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water according to the weight ratio into a beaker, stirring continuously for 5-8 hours, and leaving for more than 12 hours for later use;
[0028] Step 3, preparing the 10% polyvinyl alcohol solution: adding 10 parts of polyvinyl alcohol and 90 parts of soft water into a beaker according to weight, stirring at 90° C. for 60 minutes until the polyvinyl alcohol is dissolved, and cooling to room temperature for later use;
[0029] Step 4: Add 100 parts of the natural latex, 1.5 parts of the 50% S dispersion, 0.5 parts of the 40% ZnO dispersion, 5 parts of the 10% polyvinyl alcohol solution, 0.5 parts of the stabilizer, 2.0 parts of the diffusant, and 0.5 parts of the accelerator into a beaker according to the proportions, heat to 40°C, carry out vulcanization reaction at a stirring speed of 300-330 rpm for 40 minutes, and cool to room temperature.
[0030] The stabilizer is a 10% casein solution, and the preparation method of the 10% casein solution is as follows: weigh the ingredients according to weight: 10 parts of casein, 1.5 parts of borax, 3.2 parts of 28% ammonia water and 85.3 parts of soft water, and heat and stir until the ingredients are completely dissolved.
[0031] The diffusing agent is a 10% NF solution. The preparation method of the 10% NF solution is as follows: 10 parts of NF and 90 parts of soft water are added into a beaker according to weight, and stirred until the NF is completely dissolved, and then cooled at room temperature for use.
[0032] The accelerator is a 50% ZDC dispersion, and the preparation method of the 50% ZDC dispersion is as follows: ZDC powder is ground in a mortar for later use; 50 parts of ZDC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water are added into a beaker according to weight proportion, stirred continuously for 5-8 hours, and left for more than 12 hours for later use.
[0033] After testing, the prepared natural latex-polyvinyl alcohol environmentally friendly adhesive was found to have a viscosity of 841 mPa·s and a peel strength of 6.53N.
[0034] Example 2
[0035] Step 1, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water in a beaker according to a weight ratio, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and standing for more than 12 hours for later use;
[0036] Step 2, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water according to the weight ratio into a beaker, stirring continuously for 5-8 hours, and leaving for more than 12 hours for later use;
[0037] Step 3, preparing the 10% polyvinyl alcohol solution: adding 10 parts of polyvinyl alcohol and 90 parts of soft water into a beaker according to weight, stirring at 90° C. for 60 minutes until the polyvinyl alcohol is dissolved, and cooling to room temperature for later use;
[0038] Step 4: Add 100 parts of the natural latex, 1.5 parts of the 50% S dispersion, 0.5 parts of the 40% ZnO dispersion, 15 parts of the 10% polyvinyl alcohol solution, 0.5 parts of the stabilizer, 2.0 parts of the diffusant, and 0.5 parts of the accelerator into a beaker according to the proportions by weight, heat to 40° C., carry out vulcanization reaction at a stirring speed of 300-330 rpm for 40 minutes, and cool to room temperature.
[0039] The stabilizer is a 10% casein solution. The preparation method of the 10% casein solution is as follows: weigh the ingredients according to weight: 10 parts of casein, 1.5 parts of borax, 3.2 parts of 28% ammonia water and 85.3 parts of soft water, and heat and stir until the ingredients are completely dissolved.
[0040] The diffusing agent is a 10% NF solution. The preparation method of the 10% NF solution is as follows: 10 parts of NF and 90 parts of soft water are added into a beaker according to weight, and stirred until the NF is completely dissolved, and then cooled at room temperature for later use.
[0041] The accelerator is a 50% ZDC dispersion. The preparation method of the 50% ZDC dispersion is as follows: grind ZDC powder in a mortar for later use; add 50 parts of ZDC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water in a beaker according to weight, stir continuously for 5-8 hours, and stand for more than 12 hours for later use.
[0042] After testing, the prepared natural latex-polyvinyl alcohol environmentally friendly adhesive was found to have a viscosity of 1296 mPa·s and a peel strength of 9.20N.
[0043] Example 3
[0044] Step 1, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water in a beaker according to a weight ratio, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and standing for more than 12 hours for later use;
[0045] Step 2, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water according to the weight ratio into a beaker, stirring continuously for 5-8 hours, and leaving for more than 12 hours for later use;
[0046] Step 3, preparing the 10% polyvinyl alcohol solution: adding 10 parts of polyvinyl alcohol and 90 parts of soft water into a beaker according to weight, stirring at 90° C. for 60 minutes until the polyvinyl alcohol is dissolved, and cooling to room temperature for later use;
[0047] Step 4: add 100 parts of the natural latex, 1.5 parts of the 50% S dispersion, 0.5 parts of the 40% ZnO dispersion, 30 parts of the 10% polyvinyl alcohol solution, 0.5 parts of the stabilizer, 2.0 parts of the diffusant, and 0.5 parts of the accelerator into a beaker according to the proportions, heat to 40°C, carry out vulcanization reaction at a stirring speed of 300-330 rpm for 40 minutes, and cool to room temperature.
[0048] The stabilizer is a 10% casein solution, and the preparation method of the 10% casein solution is as follows: weigh the ingredients according to weight: 10 parts of casein, 1.5 parts of borax, 3.2 parts of 28% ammonia water and 85.3 parts of soft water, and heat and stir until the ingredients are completely dissolved.
[0049] The diffusing agent is a 10% NF solution. The preparation method of the 10% NF solution is as follows: 10 parts of NF and 90 parts of soft water are added into a beaker according to weight, and stirred until the NF is completely dissolved, and then cooled at room temperature for use.
[0050] The accelerator is a 50% ZDC dispersion, and the preparation method of the 50% ZDC dispersion is as follows: ZDC powder is ground in a mortar for later use; 50 parts of ZDC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water are added into a beaker according to weight proportion, stirred continuously for 5-8 hours, and left for more than 12 hours for later use.
[0051] After testing, the prepared natural latex-polyvinyl alcohol environmentally friendly adhesive was found to have a viscosity of 2523 mPa·s and a peel strength of 7.57N.
[0052] Example 4
[0053] Step 1, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water in a beaker according to a weight ratio, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and standing for more than 12 hours for later use;
[0054] Step 2, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water according to the weight ratio into a beaker, stirring continuously for 5-8 hours, and leaving for more than 12 hours for later use;
[0055] Step 3, preparing the 10% polyvinyl alcohol solution: adding 10 parts of polyvinyl alcohol and 90 parts of soft water into a beaker according to weight, stirring at 90° C. for 60 minutes until the polyvinyl alcohol is dissolved, and cooling to room temperature for later use;
[0056] Step 4: Add 100 parts of the natural latex, 1.5 parts of the 50% S dispersion, 0.5 parts of the 40% ZnO dispersion, 60 parts of the 10% polyvinyl alcohol solution, 0.5 parts of the stabilizer, 2.0 parts of the diffusant, and 0.5 parts of the accelerator into a beaker according to the proportions by weight, heat to 40°C, carry out vulcanization reaction at a stirring speed of 300-330 rpm for 40 minutes, and cool to room temperature.
[0057] The stabilizer is a 10% casein solution, and the preparation method of the 10% casein solution is as follows: weigh the ingredients according to weight: 10 parts of casein, 1.5 parts of borax, 3.2 parts of 28% ammonia water and 85.3 parts of soft water, and heat and stir until the ingredients are completely dissolved.
[0058] The diffusing agent is a 10% NF solution. The preparation method of the 10% NF solution is as follows: 10 parts of NF and 90 parts of soft water are added into a beaker according to weight, and stirred until the NF is completely dissolved, and then cooled at room temperature for use.
[0059] The accelerator is a 50% ZDC dispersion, and the preparation method of the 50% ZDC dispersion is as follows: ZDC powder is ground in a mortar for later use; 50 parts of ZDC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water are added into a beaker according to weight proportion, stirred continuously for 5-8 hours, and left for more than 12 hours for later use.
[0060] After testing, the prepared natural latex-polyvinyl alcohol environmentally friendly adhesive was found to have a viscosity of 3274 mPa·s and a peel strength of 8.99N.
[0061] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.
[0062] As described above, the natural latex-polyvinyl alcohol adhesive prepared by the present invention is green and environmentally friendly, has strong bonding strength, excellent water resistance and stability, and can fully meet the requirements of carton bonding.
[0063] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and the embodiments. It can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily realized. Therefore, without departing from the general concept defined by the claims and equivalent scope, the present invention is not limited to the specific details and the illustrations shown and described here.
Claims
1. A method for preparing a natural latex-polyvinyl alcohol adhesive, characterized in that: The invention is prepared from the following raw materials in parts by weight: 88-100 parts of natural rubber latex, 1.5 parts of 50% S dispersion, 0.5 parts of 40% ZnO dispersion, 5-60 parts of 10% polyvinyl alcohol solution, 0.5 parts of stabilizer, 2.0 parts of diffusing agent and 0.5 parts of accelerator; The preparation method of the natural latex-polyvinyl alcohol adhesive comprises the following steps: Step 1, preparing the 50% S dispersion: grinding S powder in a mortar for later use; adding 35 parts of S, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 26 parts of soft water in a beaker according to the weight ratio, stirring continuously at a speed of 300-330 rpm for 5-8 hours, and standing for more than 12 hours for later use; Step 2, preparing the 40% ZnO dispersion: grinding ZnO powder in a mortar for later use; adding 40 parts of ZnO, 25 parts of 10% casein, 2 parts of 10% KOH, 12 parts of 10% NF and 21 parts of soft water according to the weight ratio into a beaker, stirring continuously for 5-8 hours, and standing for more than 12 hours for later use; Step 3, preparing the 10% polyvinyl alcohol solution: adding 10 parts of polyvinyl alcohol and 90 parts of soft water into a beaker according to weight, stirring at 90° C. for 60 minutes until the polyvinyl alcohol is dissolved, and cooling to room temperature for later use; Step 4: Add 88-100 parts of the natural rubber latex, 1.5 parts of the 50% S dispersion, 0.5 parts of the 40% ZnO dispersion, 5-60 parts of the 10% polyvinyl alcohol solution, 0.5 parts of the stabilizer, 2.0 parts of the diffusant, and 0.5 parts of the accelerator into a beaker according to a proportion by weight, heat to 40-60° C., carry out a vulcanization reaction at a stirring speed of 300-330 rpm for 20-60 minutes, and cool to room temperature.
2. The method for preparing the natural latex-polyvinyl alcohol adhesive according to claim 1, characterized in that: The stabilizer is one or both of 10% casein solution and 10% KOH solution.
3. The method for preparing the natural latex-polyvinyl alcohol adhesive according to claim 2, characterized in that: The preparation method of the 10% casein solution is as follows: weigh out the ingredients according to weight, including 10 parts of casein, 1.5 parts of borax, 3.2 parts of 28% ammonia water and 85.3 parts of soft water, and heat and stir until the ingredients are completely dissolved.
4. The method for preparing the natural latex-polyvinyl alcohol adhesive according to claim 2, characterized in that: The preparation method of the 10% KOH solution is as follows: 10 parts of KOH and 90 parts of soft water are added into a beaker according to weight, and stirred continuously until the KOH is completely dissolved.
5. The method for preparing the natural latex-polyvinyl alcohol adhesive according to claim 1, characterized in that: The diffusing agent is a 10% NF solution. The preparation method of the 10% NF solution is as follows: 10 parts of NF and 90 parts of soft water are added into a beaker according to weight, and stirred until the NF is completely dissolved, and then cooled at room temperature for use.
6. The method for preparing the natural latex-polyvinyl alcohol adhesive according to claim 1, characterized in that: The accelerator is a 50% ZDC dispersion or a 50% ZBEC dispersion. The preparation method of the 50% ZDC dispersion or the 50% ZBEC dispersion is as follows: ZDC or ZBEC powder is ground in a mortar for later use; 50 parts of ZDC or ZBEC, 20 parts of 10% casein, 1 part of 10% KOH, 1 part of 10% NF and 28 parts of soft water are added into a beaker according to weight proportion, stirred continuously for 5-8 hours, and left for more than 12 hours for later use.
7. The method for preparing the natural latex-polyvinyl alcohol adhesive according to claim 1, characterized in that: The polyvinyl alcohol in step three is any one of polyvinyl alcohol 1788, polyvinyl alcohol 1799, polyvinyl alcohol 2499, polyvinyl alcohol 2099, and polyvinyl alcohol 2488, or a combination of two of them.
8. The method for preparing the natural latex-polyvinyl alcohol adhesive according to claim 1, characterized in that: The vulcanization reaction time in step 4 is 40 minutes and the vulcanization reaction temperature is 40°C.