Adhesive for aerogel packaging film, adhesive tape and preparation method of adhesive

By combining modified acrylate with hydrogenated rosin resin and aluminum salt curing agent, combined with inorganic filler and vinyl silane coupling agent, the problem of insufficient adhesion of aerogel packaging film is solved, and high viscosity strength and flame retardant are achieved The improvement of performance ensures the packaging effect in the field of new energy vehicles.

CN118931435APending Publication Date: 2024-11-12TAICANG SIDIKE NEW MATERIALS SCI & TECH CO LTD +1

Patent Information

Application Number
CN202411032927.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing acrylic packaging film has low adhesion to the aerogel, which leads to the phenomenon of drumming, bubbling and layering when used in the field of new energy vehicles, affecting the packaging effect and performance.

Method used

By combining modified acrylic acid ester with hydrogenated rosin resin and aluminum salt curing agent, inorganic filler, vinyl silane coupling agent, glacial acetic acid, the initial viscosity and viscosity strength of the adhesive are improved, and appropriate halogen-free resistance are selected Fueling agent to enhance the flame retardant properties of the tape.

Benefits of technology

The bonding strength and flame retardant properties of the aerogel packaging film are significantly improved, and the occurrence of drumming, bubbles and layering phenomena during the packaging process is avoided, ensuring the heat insulation and flame retardant effect of the aerogel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970380620000081
    Figure BDA0004970380620000081
  • Figure BDA0004970380620000091
    Figure BDA0004970380620000091
  • Figure BDA0004970380620000101
    Figure BDA0004970380620000101
Patent Text Reader

Abstract

The invention discloses an adhesive for an aerogel packaging film, an adhesive tape and a preparation method thereof, and the adhesive is prepared from the following raw material components in parts by weight: 100 parts of modified acrylate, 0.1-1 part of a curing agent, 10-30 parts of tackifying resin, 3-8 parts of inorganic filler, 0.2-1 part of a silane coupling agent, 15-30 parts of a halogen-free flame retardant, 2-10 parts of an antioxidant and 5-10 parts of glacial acetic acid, and 30-80 parts of a first organic solvent. The product provided by the invention can meet the packaging requirement of aerogel in a new energy automobile, has relatively good flame retardant property, and can improve the thermal runaway management effect; by improving the bonding strength of the adhesive tape to the aerogel and the opposite bonding strength of the adhesive tape, it can be guaranteed that the phenomena of bubbling and layering do not occur in the using process of the aerogel packaging film, and then the flame-retardant and heat-insulating effects of the aerogel can be better guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of aerogel packaging film materials, and in particular to an adhesive and a tape for aerogel packaging film and a preparation method thereof. Background Art

[0002] Aerogel is a nano-scale porous solid material formed by the sol-gel method, which has excellent properties such as light weight, heat insulation, and fire resistance. In the field of new energy vehicles, the application of aerogel is mainly focused on improving the safety and performance of batteries. Specifically, aerogel products are compounded with substrates such as glass fiber and ceramic fiber, which not only retains the light weight and heat insulation characteristics of aerogel, but also gives aerogel flexibility and toughness, making aerogel products have ultra-long service life, super strong heat insulation performance, ultra-high fire resistance, and super mechanical properties. These characteristics enable aerogel products to be used in the field of new energy vehicle power batteries, further improving the safety of power batteries, but aerogel has low hardness, easy to lose powder, fall off, break, etc., so it needs to be wrapped with a packaging film when used, and a position of about 1 cm needs to be reserved on the edge for the acrylic adhesive surface of the packaging film to be bonded and packaged to ensure the packaging effect.

[0003] Conventional acrylic packaging films currently used in the market have low adhesion between acrylic glue and aerogel, so bulging is prone to occur between aerogel and packaging film during use after packaging; at the same time, the adhesion between glue and glue is low, and during use, due to the high-temperature expansion of gas, the packaging film around the edges is also prone to bubbling and delamination. In view of the current situation, it is currently necessary to develop an acrylic tape with high initial adhesion, good adhesion to aerogel, and high adhesion strength. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an adhesive and tape for aerogel encapsulation film and a preparation method thereof in view of the deficiencies in the above-mentioned prior art. The present invention provides an adhesive tape and a preparation scheme having high adhesion to aerogel, high adhesion strength and flame retardancy. By modifying acrylate and matching with preferred hydrogenated rosin resin and aluminum salt curing agent, the acrylic tape can have high initial adhesion wettability and good adhesion to aerogel; by adding inorganic fillers and vinyl silane coupling agents and glacial acetic acid, the adhesion strength of the adhesive can be significantly improved.

[0005] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: in the first aspect of the present invention, an adhesive for aerogel encapsulation film is provided, comprising the following raw material components in parts by weight: 100 parts of modified acrylate, 0.1-1 parts of curing agent, 10-30 parts of tackifying resin, 3-8 parts of inorganic filler, 0.2-1 parts of silane coupling agent, 15-30 parts of halogen-free flame retardant, 2-10 parts of antioxidant, 5-10 parts of glacial acetic acid, and 30-80 parts of a first organic solvent.

[0006] Preferably, the modified acrylate is obtained by polymerizing the following raw materials in parts by weight:

[0007] 70-90 parts of soft monomer, 5-20 parts of hard monomer, 2-8 parts of functional monomer, 140-180 parts of second organic solvent, and 0.2-0.5 parts of initiator.

[0008] Preferably, the soft monomer is selected from one or more of isooctyl acrylate, ethyl acrylate, n-butyl acrylate, lauryl acrylate and octadecyl acrylate;

[0009] The hard monomer is selected from one or more of styrene, methyl acrylate, methyl methacrylate, ethyl methacrylate and isobornyl methacrylate;

[0010] The functional monomer is selected from any one of hydroxyethyl acrylate, acrylic acid, methacrylic acid, and hydroxypropyl acrylate, or a combination of at least two thereof.

[0011] Preferably, the functional monomer is a mixture of acrylic acid and hydroxypropyl methacrylate, and the mass ratio of acrylic acid to hydroxypropyl methacrylate is 3:1.

[0012] Preferably, the modified acrylate is prepared by the following method:

[0013] S1. In an inert gas atmosphere, the soft monomer, the hard monomer, the functional monomer and part of the second organic solvent are stirred evenly, and an initiator accounting for 1 / 4 of the total mass is first added, and the mixture is reacted at 66° C.-69° C. for 1 h-2 h to obtain a first reaction solution;

[0014] S2, adding an initiator accounting for 1 / 4 of the total mass to the first reaction solution described in S1, stirring and reacting at 73° C.-78° C. for 1 h-3 h to obtain a second reaction solution;

[0015] S3. Add the remaining initiator to the second reaction liquid described in S2, stir and react at 80° C.-83° C. for 3 h-6 h, and then add the remaining second solvent to obtain modified acrylate.

[0016] Preferably, the curing agent is one or more of an isocyanate curing agent and an aluminum salt curing agent;

[0017] The tackifying resin is one or more of rosin resin, rosin resin derivative, and terpene resin;

[0018] The inorganic filler is one or more of aluminum oxide, aluminum hydroxide and silicon dioxide.

[0019] Preferably, the silane coupling agent is one or more of vinyl trichlorosilane, vinyl trimethylsilane, and vinyl triisopropyl propoxy silane;

[0020] The halogen-free flame retardant composition is one or more of phosphorus-based and nitrogen-based flame retardants and carbon-forming agents;

[0021] The antioxidant is a mixture of hindered phenols and phosphite antioxidants;

[0022] The first solvent and the second solvent are one or more of ethyl acetate, butyl acetate and toluene.

[0023] Preferably, the halogen-free flame retardant is a mixture of flame retardant RF-605D and flame retardant RF-280;

[0024] The tackifying resin is at least one of Arakawa's KE-311 and KE-359 resins;

[0025] The curing agent is a mixture of hexamethylene diisocyanate and aluminum triacetylacetonate.

[0026] A second aspect of the present invention provides a method for preparing the adhesive for aerogel packaging film as described above, comprising the following steps:

[0027] 1) adding a halogen-free flame retardant and an inorganic filler composition to a portion of a first organic solvent and stirring to pre-disperse, then mixing with a modified acrylate, a tackifying resin, a silane coupling agent, an antioxidant, glacial acetic acid and the remaining portion of the first organic solvent, stirring evenly and filtering to obtain a filtrate;

[0028] 2) Adding a curing agent to the filtrate obtained in step 1) and stirring evenly to obtain the adhesive for the aerogel encapsulation film.

[0029] According to a third aspect of the present invention, there is provided a gel encapsulation film adhesive tape, which is prepared by the following method: uniformly coating the aerogel encapsulation film adhesive as described above on the corona surface of the substrate, drying, attaching a release film to the adhesive layer, aging, and standing to obtain the gel encapsulation film adhesive tape.

[0030] The beneficial effects of the present invention are:

[0031] The present invention provides an adhesive for an aerogel packaging film and an aerogel packaging film based on the adhesive. The product provided by the present invention can meet the packaging requirements of aerogels in new energy vehicles, has good flame retardant properties, and can improve the effect of thermal runaway management; by improving the bonding strength of the adhesive tape to the aerogel and the adhesive strength of the adhesive tape, it can be ensured that the aerogel packaging film will not have bubbling and stratification during use, thereby better ensuring the flame retardant and heat insulation effects of the aerogel.

[0032] In the adhesive of the present invention, acrylic acid with strong wetting ability is selected and matched with an aluminum salt curing agent, and its oxygen atoms can form coordination bonds with metal ions to achieve the effect of chemical chelation, thereby improving the wettability of the glue and the bonding effect of the aerogel, ensuring that it is not easy to bulge or bubble during use;

[0033] The present invention introduces a vinyl silane coupling agent and carboxyl glacial acetic acid into the adhesive, and matches the inorganic filler with a specific particle size. The vinyl silane coupling agent contains an unsaturated double bond and three hydrolyzable methoxy groups, wherein the alkoxy groups are hydrolyzed to generate active silanol groups, which are condensed with the inorganic filler to form a chemical bond. The vinyl groups are easily reacted with functional groups OH, COOH, double bonds, etc. in the organic polymer, so that the silane and the organic polymer are connected, and the silane and the organic polymer can be bidirectionally chemically reacted with the inorganic filler and the organic polymer to improve the bonding force, thereby improving the bonding strength of the adhesive. The glacial acetic acid contains carboxylic acid groups and methyl functional groups, and can chemically react with acrylic acid to generate reaction force, thereby forming a strong bonding effect. The metal inorganic filler with a specific particle size can increase the effective bonding area of ​​the adhesive surface during bonding. The combined effect of the above makes the acrylic glue have better bonding performance, and it is not easy to cause bulging and delamination during packaging and use.

[0034] In the traditional scheme, the addition of flame retardants will have a certain impact on the cohesive strength, viscosity and wettability of the tape. Some flame retardants have poor compatibility with acrylic adhesives, and after aging, flame retardant migration and precipitation will occur, resulting in a significant decrease in the performance of the tape. In the adhesive of the present invention, by screening the combination of different flame retardants, a flame retardant with good compatibility with acrylic adhesives and without affecting the high wettability of the tape to aerogels was found. While meeting the performance requirements, its flame retardancy reached VTM-0. DETAILED DESCRIPTION

[0035] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0036] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0037] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0038] The invention provides an adhesive for an aerogel encapsulation film, comprising the following raw material components in parts by weight: 100 parts of modified acrylate, 0.1-1 parts of a curing agent, 10-30 parts of a tackifying resin, 3-8 parts of an inorganic filler, 0.2-1 parts of a silane coupling agent, 15-30 parts of a halogen-free flame retardant, 2-10 parts of an antioxidant, 5-10 parts of glacial acetic acid, and 30-80 parts of a first organic solvent.

[0039] In a preferred embodiment, the modified acrylate is obtained by polymerizing the following raw materials in parts by weight:

[0040] 70-90 parts of soft monomer, 5-20 parts of hard monomer, 2-8 parts of functional monomer, 140-180 parts of second organic solvent, and 0.2-0.5 parts of initiator.

[0041] In a preferred embodiment, the soft monomer of the soft monomer is selected from one or more of isooctyl acrylate, ethyl acrylate, n-butyl acrylate, lauryl acrylate and octadecyl acrylate;

[0042] In a preferred embodiment, the hard monomer is selected from one or more of styrene, methyl acrylate, methyl methacrylate, ethyl methacrylate and isobornyl methacrylate;

[0043] In a preferred embodiment, the functional monomer is selected from any one of hydroxyethyl acrylate, acrylic acid, methacrylic acid, and hydroxypropyl acrylate, or a combination of at least two thereof. More preferably, the functional monomer is a mixture of acrylic acid and hydroxypropyl methacrylate. Furthermore, the mass ratio of acrylic acid to hydroxypropyl methacrylate is 3:1.

[0044] In a preferred embodiment, the initiator is azobisisobutyronitrile and / or dibenzoyl peroxide.

[0045] In a preferred embodiment, the modified acrylate is prepared by the following method:

[0046] S1. In an inert gas atmosphere, the soft monomer, the hard monomer, the functional monomer and part of the second organic solvent are stirred evenly, and an initiator accounting for 1 / 4 of the total mass is first added, and the mixture is reacted at 66° C.-69° C. for 1 h-2 h to obtain a first reaction solution;

[0047] S2, adding an initiator accounting for 1 / 4 of the total mass to the first reaction liquid of S1, stirring and reacting at 73°C-78°C for 1h-3h to obtain a second reaction liquid;

[0048] S3. Add the remaining initiator to the second reaction liquid of S2, stir and react at 80° C.-83° C. for 3 h-6 h, and then add the remaining second solvent to obtain modified acrylate.

[0049] In a preferred embodiment, the curing agent is one or more of an isocyanate curing agent and an aluminum salt curing agent. Further preferably, the curing agent is a mixture of hexamethylene diisocyanate and aluminum triacetylacetonate.

[0050] In a preferred embodiment, the tackifying resin is one or more of rosin resin, rosin resin derivative, and terpene resin. More preferably, the tackifying resin is at least one of Arakawa's KE-311 and KE-359 resins.

[0051] In a preferred embodiment, the inorganic filler is one or more of aluminum oxide, aluminum hydroxide, and silicon dioxide, and has a particle size of 2-4 μm.

[0052] In a preferred embodiment, the silane coupling agent is one or more of vinyl trichlorosilane, vinyl trimethylsilane, and vinyl triisopropyl propoxy silane.

[0053] In a preferred embodiment, the halogen-free flame retardant composition is one or more of phosphorus-based flame retardants, nitrogen-based flame retardants, and carbon-forming agents. Further preferably, the halogen-free flame retardant is a mixture of flame retardant RF-605D and flame retardant RF-280.

[0054] In a preferred embodiment, the antioxidant is a mixture of hindered phenols and phosphite antioxidants; more preferably, it is a mixture of BASF 1010 and BASF 168 antioxidants, and the mass ratio is 1:1.

[0055] In a preferred embodiment, the first solvent and the second solvent are one or more of ethyl acetate, butyl acetate, and toluene.

[0056] The present invention also provides a method for preparing the above adhesive for aerogel packaging film, comprising the following steps:

[0057] 1) adding a halogen-free flame retardant and an inorganic filler composition to a portion of a first organic solvent and stirring to pre-disperse, then mixing with a modified acrylate, a tackifying resin, a silane coupling agent, an antioxidant, glacial acetic acid and the remaining portion of the first organic solvent, stirring evenly and filtering to obtain a filtrate;

[0058] 2) Adding a curing agent to the filtrate obtained in step 1) and stirring evenly to obtain an adhesive for aerogel encapsulation film.

[0059] The present invention also provides a gel packaging film adhesive tape, which is prepared by the following method: uniformly coating the above aerogel packaging film adhesive on the corona surface of the substrate, drying, attaching a release film to the adhesive layer, aging, and standing to obtain the gel packaging film adhesive tape.

[0060] In a preferred embodiment, the thickness of the glue layer is 25-50 μm.

[0061] In a preferred embodiment, the substrate layer is a PET polyester film, and the thickness of the substrate layer is 20-70 μm.

[0062] In a preferred embodiment, the release force of the release film is 5-15 gf / in, the residual bonding rate is ≥90%, and the thickness of the release film is 25-75 μm.

[0063] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.

[0064] The sources of the main raw materials involved in the following examples and comparative examples are as follows:

[0065] Lauryl acrylate, methyl acrylate, acrylic acid, hydroxypropyl methacrylate, and isobornyl methacrylate were purchased from Shanghai Hechuang Chemical Co., Ltd.;

[0066] Azobisisobutyronitrile was purchased from Sinopharm Reagents, analytical grade;

[0067] Aluminum triacetylacetonate was purchased from Hubei Xingyan New Material Technology Co., Ltd.;

[0068] Hexamethylene diisocyanate was purchased from Mitsui Chemicals (Shandong) Co., Ltd.

[0069] Flame retardant RF-605D, purchased from Zhejiang Ruigao New Materials Co., Ltd.;

[0070] Tackifying resin Arakawa KE-311, BASF antioxidant 1010, antioxidant 168, purchased from Shanghai Kaiyin Chemical Co., Ltd.;

[0071] Silane coupling agent, vinyl triisopropylene propoxy silane, was purchased from Qufu Yishun Chemical Co., Ltd.;

[0072] Silane coupling agent, vinyltrimethylsilane, was purchased from Zhongshan Dixin Chemical Co., Ltd.;

[0073] Glacial acetic acid and ethyl acetate were purchased from Narmei New Materials (Shandong) Group Co., Ltd.;

[0074] Aluminum hydroxide was purchased from Hefei Zhongke Flame Retardant New Materials Co., Ltd.

[0075] The modified acrylates involved in the following examples and comparative examples are all prepared by the following method:

[0076] S1. Under an inert gas atmosphere, 80 parts of soft monomer, 15 parts of hard monomer, 5 parts of functional monomer and 100 parts of the second organic solvent are stirred uniformly by weight, 0.1 parts of initiator are added first, and the mixture is reacted at 68° C. for 2 hours to obtain a first reaction solution;

[0077] S2, adding 0.1 parts of initiator to the first reaction solution of S1, stirring and reacting at 75°C for 2h to obtain a second reaction solution;

[0078] S3. Add 0.2 parts of the initiator and 50 parts of the second organic solvent to the second reaction solution of S2, and stir the mixture at 82° C. for 5 hours to obtain modified acrylate.

[0079] Among them, the soft monomer is lauric acid acrylate, the hard monomer is methyl acrylate and isobornyl methacrylate, the ratio is 2 / 1, the functional monomer is acrylic acid and hydroxypropyl methacrylate, the ratio is 3 / 1, the initiator is azobisisobutyronitrile, and the second organic solvent is ethyl acetate.

[0080] The preparation methods of the adhesive tape for gel encapsulation films in the following examples and comparative examples are the same, and are specifically as follows:

[0081] 1) adding the halogen-free flame retardant and the inorganic filler composition to 40 parts of the total mass of the first organic solvent and stirring for 20 minutes for pre-dispersion, and then mixing with the modified acrylate, tackifying resin, silane coupling agent, antioxidant, glacial acetic acid (purchased from Nalmei New Materials (Shandong) Group Co., Ltd.) and the remaining part of the first organic solvent (ethyl acetate), stirring for 30 minutes and filtering with a 200-mesh filter to obtain the filtrate;

[0082] 2) adding a curing agent to the filtrate obtained in step 1) and stirring evenly to obtain an adhesive for an aerogel encapsulation film;

[0083] 3) The adhesive for aerogel encapsulation film is evenly coated on the corona surface of a PET substrate with a thickness of 25 μm, the dry adhesive thickness is controlled to be 30 μm, and dried at 100°C for 3 min. After drying, a release film with a thickness of 50 μm is attached to the adhesive layer, and the film is aged in an oven at 40°C for 3 days and left to stand at 23°C for 24 hours to obtain an adhesive tape for aerogel encapsulation film.

[0084] Adhesive tape products for gel encapsulation films of Examples 1-7 and Comparative Examples 1-5 were prepared by the above method according to the formulations shown in Table 1. The parts in the following table are all parts by weight.

[0085] Table 1

[0086]

[0087]

[0088] The following performance tests were performed on the products of Examples 1-7 and Comparative Examples 1-5:

[0089] 1. Thickness test

[0090] (1) After sampling at different positions of the tape, place it in a standard environment for 24 hours;

[0091] (2) Place the tape between the measuring heads of the thickness gauge, with the adhesive side facing up. Gently lower the measuring heads of the thickness gauge and wait for the reading to stabilize. Record the value to an accuracy of 0.001 mm.

[0092] (3) Measure 20 points on each tape, record the values, and calculate the average value.

[0093] 2. Test the adhesion of steel plate

[0094] (1) After sampling at different positions of the tape, place it in a standard environment for 24 hours;

[0095] (2) Cut the tape into 25.4mm*300mm pieces, 3 pieces in total;

[0096] (3) Peel off the release layer of the tape, stick the adhesive surface to the steel plate with a rubber roller, press it with a 2kg pressure roller at a speed of 600mm / min, back and forth twice, and let it stand for 20 minutes under standard environment. No bubbles are allowed between the adhesive surface and the steel plate;

[0097] (4) After the static state is completed, use a tensile testing machine to clamp the lower end of the steel plate and the free end of the tape respectively, peel them at 180° and a speed of 300 mm / min, and record the software readings.

[0098] 3. Adhesion and peeling force test

[0099] (1) After sampling at different positions of the tape, place it in a standard environment for 24 hours;

[0100] (2) Cut the tape into 25.4mm*300mm pieces, 3 pieces in total;

[0101] (3) Peel off the release layer of the tape, use a rubber roller to bond the adhesive surfaces together, and use a 2kg pressure roller to press at a speed of 600 mm / min, back and forth twice, and let it stand for 20 minutes under standard conditions. No bubbles are allowed between the adhesive layers;

[0102] (4) After the static rest, use a tensile testing machine to clamp the two ends of the tape respectively, perform T peeling at 90° and a speed of 300 mm / min, and record the software readings.

[0103] 4. UL 94VTM-0, VTM-1, VTM-2 vertical combustion test

[0104] (1) Application scope: Thin film materials or samples with distortion in V-0, V-1, V-2 vertical combustion tests

[0105] (2) Flame height: 20mm

[0106] (3) Sample requirements: 200±5mm×50±1mm, with a marking line along the length of 125mm, wrapped around a round rod with a diameter of 12.7mm, and the upper end is glued with double-sided tape, two groups of 10 pieces each

[0107] (4) Sample environment conditioning: One group of samples shall be treated at (23±2)℃, (50±5)%RH for 48 hours, and the other group of samples shall be treated at (70±1)℃ for 168 hours. The grade that both groups of samples can reach at the same time shall be the final grade of the samples.

[0108] (5) Test method: adjust the flame height to 20 mm, apply the flame for 3 seconds for the first time, anneal and record the flaming burning time t1, apply the flame for 3 seconds for the second time, anneal and record the flaming burning time t2 and the flameless burning time t3, and record whether the burning exceeds the 125 mm mark and whether there is any dripping that ignites the absorbent cotton below.

[0109] 5. Simulation experiment

[0110] (1) After sampling at different positions of the tape, place it in a standard environment for 24 hours;

[0111] (2) Cut a 0.15 mm thick aerogel pad into a 10 cm*10 cm sample, stack two aerogel pads, and stick them on the aerogel pads with packaging tape, leaving about 1 cm of space around them for bonding;

[0112] (3) Place the bonded finished product in an environmental aging test at 65°C and 95% RH;

[0113] (4) Observe whether there is any stratification on the surface and surrounding of the sample.

[0114] The test results are shown in Table 2 below:

[0115] Table 2

[0116]

[0117]

[0118] According to the test results in Table 2, it can be seen that the peel strength of the embodiment with the addition of vinyl silane coupling agent, glacial acetic acid and inorganic filler of a specific particle size can reach more than 3500 g, and after the encapsulated aerogel is placed at 65 / 95 for aging for 7 days, no bubbling or delamination occurs.

[0119] Compared with the above embodiments, comparative example 1 removes the vinyl silane coupling agent, and the inorganic substance and the organic compound cannot be effectively connected during bonding, resulting in a significant decrease in the bonding peeling force; comparative example 2 removes the glacial acetic acid, which cannot react chemically with acrylate, resulting in a significant decrease in its bonding peeling force; comparative example 3 removes the inorganic filler of a specific particle size, reduces the effect of the silane coupling agent, and at the same time, due to the reduction in contact area, the bonding peeling force is also significantly reduced; comparative examples 4 and 5 use inorganic fillers of other particle sizes, and their particle sizes are too small to have no filling effect, and cannot form effective bonding on the adhesive surface. Too large a particle size will reduce the bonding area, resulting in poor product appearance and performance, so their bonding performance is also low when tested.

[0120] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. An adhesive for aerogel packaging film, It is characterized in that The invention comprises the following raw material components in parts by weight: 100 parts of modified acrylate, 0.1-1 parts of curing agent, 10-30 parts of tackifying resin, 3-8 parts of inorganic filler, 0.2-1 parts of silane coupling agent, 15-30 parts of halogen-free flame retardant, 2-10 parts of antioxidant, 5-10 parts of glacial acetic acid and 30-80 parts of first organic solvent.

2. The adhesive for aerogel encapsulation film according to claim 1, It is characterized in that The modified acrylate is obtained by polymerizing the following raw materials in proportion by weight: 70-90 parts of soft monomer, 5-20 parts of hard monomer, 2-8 parts of functional monomer, 140-180 parts of second organic solvent, and 0.2-0.5 parts of initiator.

3. The adhesive for aerogel encapsulation film according to claim 2, It is characterized in that The soft monomer is selected from one or more of isooctyl acrylate, ethyl acrylate, n-butyl acrylate, lauryl acrylate and octadecyl acrylate; The hard monomer is selected from one or more of styrene, methyl acrylate, methyl methacrylate, ethyl methacrylate and isobornyl methacrylate; The functional monomer is selected from any one of hydroxyethyl acrylate, acrylic acid, methacrylic acid, and hydroxypropyl acrylate, or a combination of at least two thereof.

4. The adhesive for aerogel encapsulation film according to claim 3, It is characterized in that The functional monomer is a mixture of acrylic acid and hydroxypropyl methacrylate, and the mass ratio of acrylic acid to hydroxypropyl methacrylate is 3:

1.

5. The adhesive for aerogel encapsulation film according to claim 2, It is characterized in that The modified acrylate is prepared by the following method: S1. In an inert gas atmosphere, the soft monomer, the hard monomer, the functional monomer and part of the second organic solvent are stirred evenly, and an initiator accounting for 1 / 4 of the total mass is first added, and the mixture is reacted at 66° C.-69° C. for 1 h-2 h to obtain a first reaction solution; S2, adding an initiator accounting for 1 / 4 of the total mass to the first reaction solution described in S1, stirring and reacting at 73° C.-78° C. for 1 h-3 h to obtain a second reaction solution; S3. Add the remaining initiator to the second reaction liquid described in S2, stir and react at 80° C.-83° C. for 3 h-6 h, and then add the remaining second solvent to obtain modified acrylate.

6. The adhesive for aerogel encapsulation film according to claim 1, It is characterized in that The curing agent is one or more of an isocyanate curing agent and an aluminum salt curing agent; The tackifying resin is one or more of rosin resin, rosin resin derivative, and terpene resin; The inorganic filler is one or more of aluminum oxide, aluminum hydroxide and silicon dioxide.

7. The adhesive for aerogel encapsulation film according to claim 2, It is characterized in that The silane coupling agent is one or more of vinyl trichlorosilane, vinyl trimethylsilane, and vinyl triisopropyl propoxy silane; The halogen-free flame retardant composition is one or more of phosphorus-based and nitrogen-based flame retardants and carbon-forming agents; The antioxidant is a mixture of hindered phenols and phosphite antioxidants; The first solvent and the second solvent are one or more of ethyl acetate, butyl acetate and toluene.

8. The adhesive for aerogel encapsulation film according to claim 1, It is characterized in that The flame retardant is a mixture of halogen-free flame retardant RF-605D and flame retardant RF-280; The tackifying resin is at least one of Arakawa's KE-311 and KE-359 resins; The curing agent is a mixture of hexamethylene diisocyanate and aluminum triacetylacetonate.

9. A method for preparing an adhesive for aerogel encapsulation film according to any one of claims 1 to 8, It is characterized in that The following steps are involved: 1) adding a halogen-free flame retardant and an inorganic filler composition to a portion of a first organic solvent and stirring to pre-disperse, then mixing with a modified acrylate, a tackifying resin, a silane coupling agent, an antioxidant, glacial acetic acid and the remaining portion of the first organic solvent, stirring evenly and filtering to obtain a filtrate; 2) Adding a curing agent to the filtrate obtained in step 1) and stirring evenly to obtain the adhesive for the aerogel encapsulation film.

10. An adhesive tape for gel packaging film, It is characterized in that The aerogel packaging film tape is prepared by the following method: uniformly coating the adhesive for aerogel packaging film as claimed in any one of claims 1 to 8 on the corona surface of the substrate, drying, attaching a release film to the adhesive layer, aging, and standing to obtain the adhesive tape for aerogel packaging film.

Citation Information

Patent Citations

  • Single-component acrylic adhesive as well as preparation method and application thereof

    CN114163950A

  • Modified acrylate adhesive, preparation method thereof and flame-retardant mica tape

    CN117736674A

  • Glue and adhesive tape

    CN118165676A

Cited By

  • Aerogel encapsulation thermoset film and method of making

    CN122978862A