Phosphorus hydrotalcite flame-retardant adhesive and preparation method thereof

By combining phosphorus hydrotalcite with melamine resin in wood adhesives, combining nitrogen-phosphorus-based and condensed phase flame retardant mechanism, the problem of poor flame retardant performance and glue performance in the prior art is solved, and high efficiency is achieved Flame retardant and stable glue, suitable for industrial production.

CN118931441APending Publication Date: 2024-11-12NANJING FORESTRY UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411266105.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

While the existing flame retardant adhesives for wood improve flame retardant performance, the adhesive performance is not high and the preparation process is complicated, making it not suitable for industrial production.

Method used

Phosphorus hydrotalcite is used as flame retardant, and by combining with melamine resin, combining nitrogen-phosphorus and condensed phase flame retardant mechanism, a phosphorus-based hydrotalcite flame retardant adhesive with high-efficiency flame retardant and stable glue performance is prepared, which simplifies the The preparation process was carried out.

Benefits of technology

With low addition amount, the limit oxygen index increases to more than 60%, the glue strength reaches the requirements of Class I plywood, which has industrial production potential and market promotion value.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a phosphorus hydrotalcite flame-retardant adhesive and a preparation method thereof, and the flame-retardant adhesive is prepared by taking phosphorus hydrotalcite, formaldehyde, urea, melamine and the like as raw materials through a simple reaction method. The flame-retardant adhesive disclosed by the invention has efficient flame retardance, excellent bonding performance and good stability, and meets the requirements of halogen-free, non-toxic and green flame-retardant adhesives.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to the technical field of adhesives, in particular to a flame retardant adhesive for wood materials. Background Art

[0002] Wood has environmentally friendly properties such as biodegradability and renewability, and has advantages such as high specific strength, electrical insulation, and rich natural multi-porous structure. It plays an important role in the fields of construction, home decoration, packaging, etc. However, the global high-quality natural wood resources are increasingly scarce. In order to improve the utilization rate of wood materials, adhesives are compounded with low-quality wood materials such as small-diameter wood, branch wood, wood chips, and shavings to prepare artificial boards with excellent performance. However, most adhesives are relatively flammable, and combustion produces toxic gases and smoke, which poses a serious threat to people's lives and property safety. Therefore, they need to be flame-retardant.

[0003] 1. For example, 201110111600.1 discloses a method for producing a flame retardant adhesive, wherein one or more of ammonium polyphosphate, melamine orthophosphate and melamine pyrophosphate are compounded with a carbonizing agent, a dehydrating agent, an auxiliary agent and a water-soluble amino resin to prepare a flame retardant adhesive for wood. Although the plywood prepared by the method has good flame retardancy and smoke suppression performance, due to the variety of auxiliary agents and the addition of a large amount of inorganic fillers and organic alcohols to the water-based adhesive, the adhesive has low bonding performance and poor stability.

[0004] 2. For example, the disclosed invention patent CN202210029548.3 uses microencapsulated red phosphorus, microencapsulated ammonium polyphosphate and aluminum hydroxide as flame retardants and mixes them with urea-formaldehyde resin to prepare a flame-retardant adhesive to prepare a flame-retardant plywood with an oxygen index as high as 35.2%. However, the preparation process of the microencapsulated flame retardant is complicated and involves vacuum drying equipment, which is not suitable for industrial production.

[0005] Hydrotalcite is a promising inorganic metal flame retardant due to its non-toxic, non-volatile, highly stable and designable properties. Hydrotalcite is a typical layered material with metal hydroxide as the main layer, in which anions and some water molecules are embedded. During combustion, the metal oxides produced by the decomposition of hydrotalcite can form a stable carbon layer on the surface of the wood, which blocks heat invasion and isolates oxygen; the evaporation of water molecules dilutes the concentration of external combustible gases and reduces the temperature of the combustion environment. In addition, hydrotalcite has the ability to exchange anions, and the selection of anions with flame retardant ability can improve the flame retardant properties of hydrotalcite.

[0006] To this end, the present invention uses phosphorus-containing compounds and hydrotalcite to prepare a phosphorus-based hydrotalcite flame-retardant adhesive, and the hydrotalcite is modified by intercalation of phosphorus-containing functional groups to enhance the flame retardancy of the hydrotalcite, so that the flame retardant has both gas-phase and solid-phase dual flame retardant effects. When the hydrotalcite is compounded with a melamine resin adhesive, not only its high bonding strength is maintained, but also the adhesive has high flame retardancy with a low addition amount of the flame retardant. At the same time, the preparation process is simple and has the potential to achieve industrial production. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention provides a method for preparing a phosphorus-based hydrotalcite flame-retardant adhesive to solve the problems mentioned in the above background technology.

[0008] To achieve the above object, the present invention provides the following technical solutions: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of 3 to 6 parts of a phosphorus-based hydrotalcite flame retardant, 49 to 51 parts of formaldehyde, 27 to 28 parts of urea, and 14 to 18 parts of melamine;

[0009] The phosphorus-based hydrotalcite flame retardant is composed of the following raw materials in parts by weight: 1 to 3 parts of hydrotalcite, 1 to 3 parts of phosphorus-containing compounds and 4 to 6 parts of amino compounds.

[0010] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49-51 parts of formaldehyde and 13-14 parts of urea are uniformly mixed, the temperature is kept constant at 80-90°C, and the reaction is carried out at a constant temperature for 60-80 minutes S2, after the reaction, add 3 to 6 parts of phosphorus-based hydrotalcite flame retardant, keep the pH value at 4.6 to 4.8 for 20 to 30 minutes, and then adjust the pH value to 9.1 to 9.5. S3, after the reaction of S2 is completed, 14 to 18 parts of melamine are added to the mixture, the temperature is kept constant at 80 to 90°C for 120 to 140 minutes, the remaining urea is added, the reaction is continued for 20 to 30 minutes, and the mixture is cooled and discharged.

[0011] The preparation method of the phosphorus-based zinc-aluminum hydroxide flame retardant: The zinc-aluminum hydrotalcite powder is calcined at 500-600° C. to obtain a bimetallic oxide; the bimetallic oxide, the phosphorus-containing compound and the amino compound are uniformly mixed in water, and the pH value is adjusted to be acidic, the temperature is kept constant at 30-120° C., the reaction is continuously stirred for 2-10 hours, and the reaction is dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0012] In the method for preparing a phosphorus-based hydrotalcite flame retardant, the phosphorus-containing compound is selected from one or more of phytic acid, hydroxyethylidene diphosphonic acid, and potassium hexadecanol phosphate.

[0013] In the method for preparing a phosphorus-based hydrotalcite flame retardant, the amino compound is one or more of urea, melamine, triethylamine, ethylenediamine, dicyandiamide, and benzoguanamine.

[0014] Compared with the prior art, the present invention has the following beneficial effects: (1) Highly effective flame retardant: The phosphorus-based hydrotalcite flame retardant resin adhesive of the present invention combines the flame retardant mechanism of nitrogen and phosphorus in free radical annihilation and the condensed phase flame retardant mechanism of hydrotalcite, effectively improving the flame retardant efficiency. When the flame retardant is added in an amount of only 1-2%, the limiting oxygen index (LOI) can be increased to more than 60%. (2) High bonding strength: The adhesive prepared with this flame retardant has stable performance and a long storage period. The bonding strength of the prepared plywood can reach the requirements of Class I plywood in "Plywood" GB / T 9846-2015, and has good market promotion value. DETAILED DESCRIPTION

[0015] The technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The present invention will be further described below in conjunction with the embodiments. The following embodiments are only used to more clearly illustrate the technical scheme of the present invention, and cannot be used to limit the scope of protection of the present invention.

[0016] Comparative Example 1: A resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 49 parts of formaldehyde, 28 parts of urea, and 14 parts of melamine;

[0017] The preparation method of the resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, keep the pH value at 4.6 for 20 min, and then adjust the pH value to 9. S3, after the reaction of S2 is completed, 14 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0018] The performance test of Comparative Example 1 shows that the limiting oxygen index of the adhesive is 25.1%.

[0019] Comparative Example 2: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 3 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 14 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 1 part of hydrotalcite, 3 parts of phytic acid and 6 parts of urea.

[0020] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain zinc aluminum oxide. The zinc aluminum oxide, phytic acid and urea were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0021] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde, 14 parts of urea, and 3 parts of phosphorus-based hydrotalcite flame retardant are uniformly mixed, the temperature is kept constant at 90° C., and the reaction is carried out at a constant temperature for 60 minutes. S2, after the reaction, the pH value was maintained at 4.6 for 20 min, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 14 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0022] The performance test of comparative example 2 shows that the limiting oxygen index of the adhesive is 42.4%.

[0023] Comparative Example 3: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 3 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 14 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 1 part of hydrotalcite, 3 parts of phytic acid and 6 parts of urea.

[0024] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain zinc aluminum oxide. The zinc aluminum oxide, phytic acid and urea were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0025] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90°C, and the reaction is carried out at the constant temperature for 60 minutes. S2, after the reaction, the pH value was maintained at 4.6 for 20 min, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 14 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, 3 parts of phosphorus-based hydrotalcite flame retardant are added, the mixture is mixed evenly, cooled, and discharged.

[0026] The performance test of comparative example 3 shows that the limiting oxygen index of the adhesive is 32.4%.

[0027] Embodiment 1: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 3 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 14 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 1 part of hydrotalcite, 3 parts of phytic acid and 6 parts of urea.

[0028] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain zinc aluminum oxide. The zinc aluminum oxide, phytic acid and urea were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0029] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 3 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 14 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0030] The performance test of Example 1 shows that the limiting oxygen index of the adhesive is 60.1%.

[0031] Embodiment 2: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 3 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 14 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 3 parts of hydrotalcite, 1 part of phytic acid and 4 parts of urea.

[0032] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain zinc aluminum oxide. The zinc aluminum oxide, phytic acid and melamine were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0033] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 3 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 14 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0034] The performance test of Example 2 shows that the limiting oxygen index of the adhesive is 64.5%.

[0035] Embodiment three: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 18 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 1 part of hydrotalcite, 3 parts of phytic acid and 6 parts of urea.

[0036] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, phytic acid and triethylamine were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0037] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 6 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 18 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0038] The performance test of Example 3 shows that the limiting oxygen index of the adhesive is 65.5%.

[0039] Embodiment 4: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 18 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 3 parts of hydrotalcite, 1 part of phytic acid and 4 parts of urea.

[0040] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, phytic acid and ethylenediamine were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0041] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 6 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 18 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0042] The performance test of Example 4 shows that the limiting oxygen index of the adhesive is 64.0%.

[0043] Embodiment five: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 14 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 1 part of hydrotalcite, 3 parts of phytic acid and 6 parts of urea.

[0044] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, phytic acid and dicyandiamide were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0045] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 6 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 14 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0046] The performance test of Example 5 shows that the limiting oxygen index of the adhesive is 64.5%.

[0047] Embodiment six: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 14 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 3 parts of hydrotalcite, 1 part of hydroxyethylidene diphosphonic acid and 4 parts of urea.

[0048] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, phytic acid and benzocyanuric acid were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0049] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 6 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 14 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0050] The performance test of Example 6 shows that the limiting oxygen index of the adhesive is 69.1%.

[0051] Embodiment seven: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 18 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 1 part of hydrotalcite, 3 parts of triphenyl phosphate and 6 parts of urea.

[0052] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, triphenyl phosphate and urea were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0053] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 3 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 18 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0054] The performance test of Example 7 shows that the limiting oxygen index of the adhesive is 70.1%.

[0055] Embodiment eight: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 18 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 3 parts of hydrotalcite, 1 part of diammonium phosphate and 4 parts of urea.

[0056] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, ammonium dihydrogen phosphate and urea were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0057] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 6 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 18 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0058] The performance test of Example 8 shows that the limiting oxygen index of the adhesive is 73.1%.

[0059] Embodiment nine: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 18 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 1 part of hydrotalcite, 3 parts of potassium n-hexadecanol phosphate and 6 parts of urea.

[0060] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, potassium hexadecanol phosphate and urea were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0061] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 18 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 6 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 14 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0062] The performance test of Example 9 shows that the limiting oxygen index of the adhesive is 73.1%.

[0063] Embodiment ten: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 18 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 3 parts of hydrotalcite, 1 part of bis(4-hydroxyphenyl)phenylphosphine oxide and 4 parts of urea.

[0064] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, bis(4-hydroxyphenyl)phenylphosphine oxide and urea were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0065] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 6 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 18 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0066] The performance test of Example 10 shows that the limiting oxygen index of the adhesive is 79.1%.

[0067] Embodiment eleven: A phosphorus-based hydrotalcite flame-retardant resin adhesive, characterized in that it is composed of the following raw materials in parts by weight: 6 parts of phosphorus-based hydrotalcite flame retardant, 49 parts of formaldehyde, 28 parts of urea, and 18 parts of melamine; The phosphorus-based hydrotalcite flame retardant is characterized in that it is composed of the following raw materials in parts by weight: 3 parts of hydrotalcite, 1 part of dimethyl methylphosphonate and 4 parts of urea.

[0068] The method for preparing the phosphorus-based hydrotalcite flame retardant is characterized by: The hydrotalcite powder was calcined at 500°C to obtain a bimetallic oxide. The bimetallic oxide, dimethyl methylphosphonate and urea were uniformly mixed in water, the pH value was adjusted to 2, the temperature was kept constant at 60°C, the reaction was stirred for 6 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

[0069] The preparation method of the phosphorus-based hydrotalcite flame-retardant resin adhesive comprises the following steps: S1, 49 parts of formaldehyde and 14 parts of urea are uniformly mixed, the temperature is kept constant at 90℃, and the reaction is carried out at a constant temperature for 60 minutes S2, after the reaction, 6 parts of phosphorus-based hydrotalcite flame retardant were added, the pH value was kept at 4.6 for 20 minutes, and then the pH value was adjusted to 9. S3, after the reaction of S2 is completed, 18 parts of melamine are added to the mixture, the temperature is kept constant at 80°C for 120 minutes, the remaining urea is added, the reaction is continued for 20 minutes, and the mixture is cooled and discharged.

[0070] The performance test of Example 11 shows that the limiting oxygen index of the adhesive is 77.1%. Examples of applications of the above flame retardant adhesives In order to test the bonding strength of the phosphorus-based hydrotalcite flame-retardant adhesive, plywood was prepared for the adhesives of Comparative Examples 1 to 3 and Examples 1 to 11, and the bonding strength test was carried out. A poplar veneer with a thickness of 1.5 mm was selected, and the amount of glue applied was 250 g / cm 2 , double-sided gluing, three-layer veneer vertical assembly, hot pressing temperature of 150℃, hot pressing time of 1.25min / mm, after hot pressing, plywood prepared with different flame retardant adhesives was obtained. The bonding strength is shown in Table 1. Table 1 Sample No. Bonding strength (MPa) Comparative Example 1 0.93 Comparative Example 2 0.50 Comparative Example 3 0.71 Example 1 0.89 Example 2 0.88 Example 3 0.94 Example 4 0.91 Example 5 0.85 Example 6 0.80 Example 7 0.89 Example 8 0.88 Example 9 0.91 Example 10 0.89 Embodiment 11 0.93

[0071] It can be seen from Comparative Examples 1 to 3, Examples 1 to 11 and Table 1 that the phosphorus-based hydrotalcite flame-retardant adhesive produced by the method of the present invention has good flame retardancy, and the addition of phosphorus-based hydrotalcite at different stages of adhesive preparation will have a significant impact on the flame retardancy and bonding strength of the adhesive. The limiting oxygen index of the phosphorus-based hydrotalcite adhesive can reach 60.1 to 79.1%, and the bonding strength of the plywood prepared with the flame-retardant adhesive can reach the requirements of Class I plywood in "Plywood" GB / T 9846-2015, and has good market promotion value.

[0072] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the invention, the scope of which is determined by the appended claims and their equivalents.

Claims

1. A phosphorus-based hydrotalcite flame retardant adhesive, characterized in that The invention is composed of the following raw materials in parts by weight: 3 to 10 parts of phosphorus hydrotalcite flame retardant, 30 to 60 parts of formaldehyde, 25 to 60 parts of urea and 10 to 20 parts of melamine.

2. The method for preparing the phosphorus-based hydrotalcite flame retardant adhesive as claimed in claim 1, characterized in that The following steps are involved: S1, uniformly mixing 30-60 parts of formaldehyde and 15-30 parts of urea, reacting at 50-100° C. for 60-80 minutes; S2, after the reaction, add 3 to 10 parts of phosphorus-based hydrotalcite flame retardant, react under acidic conditions until completion, and adjust the pH value of the system to alkaline; S3, after the reaction in step 2 is completed, 10 to 20 parts of melamine are added to the mixture, the temperature is kept constant at 70 to 100° C. for 100 to 180 minutes, the remaining urea is added, the reaction is continued for 30 to 90 minutes, cooling is performed, and the material is discharged.

3. The phosphorus-based hydrotalcite flame retardant according to claim 1, characterized in that The invention is composed of the following raw materials in parts by weight: 1 to 3 parts of hydrotalcite, 1 to 3 parts of phosphorus-containing compounds and 4 to 6 parts of amino compounds.

4. The method for preparing a phosphorus-based hydrotalcite flame retardant according to claim 1, characterized in that: The hydrotalcite powder is calcined at 500-600° C. to obtain a bimetallic oxide; the bimetallic oxide, a phosphorus-containing compound and an amino compound are uniformly mixed in water, and the pH value is adjusted to be acidic, reacted at 30-120° C. for 2-10 hours, and dried to obtain a phosphorus-based hydrotalcite flame retardant.

5. The method for preparing a phosphorus-based hydrotalcite flame retardant according to claim 4, characterized in that: The phosphorus-containing compound is one or more of phytic acid, hydroxyethylidene diphosphonic acid, potassium salt of hexadecanol phosphate, triphenyl phosphate, ammonium dihydrogen phosphate, bis(4-hydroxyphenyl)phenyl phosphine oxide, and dimethyl methylphosphonate.

6. The method for preparing a phosphorus-based hydrotalcite flame retardant according to claim 4, characterized in that: The amino compound is one or more of urea, melamine, triethylamine, ethylenediamine, dicyandiamide and benzoguanamine.

Citation Information

Patent Citations

  • Flame-retardant adhesive and preparation method thereof

    CN109628050A

  • Modified hydrotalcite as well as preparation method and application thereof

    CN113025079A

  • Flame-retardant urea-formaldehyde resin adhesive and preparation method thereof

    CN113831871A

  • Modified-layered-silicate-basedaldehyde-free flame-retardant adhesive and application thereof