Polyurethane adhesive, hollow-core shaving board containing polyurethane adhesive and preparation method of hollow-core shaving board
Through the modification and pulse extrusion process of polyurethane adhesive, the problems of insufficient formaldehyde release and performance in hollow particle board are solved, high environmental protection grade and excellent mechanical properties are achieved, and the safety and stability of hollow particle board are ensured.
Patent Information
- Application Number
- CN202411055240.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The adhesives of existing hollow particleboards contain free formaldehyde, which leads to the release of formaldehyde, affecting the environmental protection level and home comfort, and the static curve strength and dimensional change rate are insufficient, making it difficult to meet environmental protection and performance requirements.
Using polyurethane adhesive, the isocyanate index is controlled within the range of 50-150 through specific combination and modification of polyols and isocyanates. Combined with pulse extrusion technology, hollow particle board without aldehyde is prepared to improve static curve strength and reduce the dimensional change rate. .
The high environmental protection level of hollow particle board without aldehyde addition is achieved, with a static curve strength of ≥2.2MPa, a squeezing size change rate ≤5.9%, a mortality-free addition, and a non-stick board during the production process, improving product quality and environmental performance.
Smart Images

Figure BDA0004976190860000131 
Figure BDA0004976190860000141
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of artificial board materials, and particularly relates to a polyurethane adhesive, a hollow particle board containing the same, and a preparation method of the hollow particle board. Background Art
[0002] Hollow particleboard, also known as bridge hole mechanical board, is made of wood and non-wood plant shavings as raw materials. After drying and gluing, it is added to an extruder equipped with a metal pipe and heated and continuously extruded to form a hollow board. It has the characteristics of good thermal insulation performance, good sound insulation effect, and light weight. Hollow particleboard is mainly used as a filler for wooden doors. At present, it is mainly produced using urea-formaldehyde glue, and most of them are E1 grade.
[0003] However, urea-formaldehyde glue contains free formaldehyde, and the product after curing is unstable and will gradually separate and release formaldehyde, which is a Class I carcinogen. Therefore, with the improvement of people's environmental awareness and the improvement of home safety requirements, hollow particleboard produced with urea-formaldehyde glue will gradually be eliminated, and it is necessary to develop hollow particleboard without formaldehyde.
[0004] For example, CN105946087A reports a flame-retardant particle board and a preparation method thereof, wherein the adhesive used is a modified urea-formaldehyde resin adhesive. Although the urea-formaldehyde resin is modified, aldehyde is still added, which increases the formaldehyde emission of the hollow particle board, and the environmental protection level of the product is low.
[0005] For example, CN1115401762A reports a manufacturing process for an ENF-grade flame-retardant hollow particleboard, which is produced using lignin adhesives. However, all lignin adhesives currently on the market contain free formaldehyde, but the free formaldehyde content is lower than that of traditional urea-formaldehyde adhesives, but they cannot be called formaldehyde-free adhesives in essence. Moreover, the boards produced by lignin adhesives will have obvious odors after being soaked in water. Although it is not common in life to soak doors in water, in the hot and humid environment of the south in summer, boards produced by lignin adhesives may also emit unpleasant odors, which does not meet people's requirements for the comfort of the home environment.
[0006] Therefore, developing an adhesive without formaldehyde addition that can improve the static bending strength of hollow particleboard and reduce the dimensional change rate of hollow particleboard is an urgent problem to be solved in this field. Summary of the invention
[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a polyurethane adhesive, a hollow particle board containing the same, and a method for preparing the hollow particle board; the polyurethane adhesive is used to prepare the hollow particle board, has no formaldehyde added, does not increase the formaldehyde emission of the hollow particle board, and has a high environmental protection level; and can improve the static bending strength of the hollow particle board and reduce the dimensional change rate and thickness deviation of the hollow particle board.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a polyurethane adhesive, wherein the raw materials for preparing the polyurethane adhesive include polyols and polyisocyanates; in the raw materials, the isocyanate index (R) is 50 to 150; the polyols include a combination of low-functionality polyols and high-functionality polyols; the functionality of the low-functionality polyols is 2; the functionality of the high-functionality polyols is greater than 2; and the mass ratio of the low-functionality polyols to the high-functionality polyols is 1:0.2 to 0.4.
[0010] Isocyanate can be directly used as an adhesive for hollow particleboard, and its bonding principle is mainly that isocyanate reacts with water in the raw material to form polyurea to form bonding. However, polyurea is hard and brittle, and easily causes problems such as deformation of the board. Therefore, the present invention uses polymer polyol to modify isocyanate to form a polyurethane adhesive, and controls the modification ratio within a specific range, that is, controls R to be 50-150, and selects polyols with specific composition and ratio as the adhesive for hollow particleboard, which can improve the static bending strength of the hollow particleboard and reduce the dimensional change rate and thickness deviation of the hollow particleboard; and the adhesive is a formaldehyde-free adhesive, which will not increase the formaldehyde emission of the hollow particleboard, thereby improving the environmental protection level of the hollow particleboard.
[0011] In the present invention, the isocyanate index is 50 to 150, for example, 50, 52, 55, 58, 60, 62, 65, 68, 70, 72, 75, 78, 80, 82, 85, 88, 90, 92, 95, 98, 100, 102, 105, 108, 110, 112, 115, 118, 120, 122, 125, 128, 130, 132, 135, 138, 140, 142, 145, 148, 150, etc.
[0012] In the present invention, when the isocyanate index is low, the dimensional change rate of the hollow particle board during extrusion is high; when the isocyanate index is high, the dimensional change rate of the hollow particle board during extrusion is high and the static bending strength is low.
[0013] Preferably, the mass ratio of the low-functionality polyol to the high-functionality polyol is 1:0.2-0.4, wherein the specific value of 0.2-0.4 can be, for example, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, etc.
[0014] In the present invention, low-functionality polyol and high-functionality polyol are compounded, and the mass ratio of the low-functionality polyol and the high-functionality polyol is controlled within the above-defined range, so that the obtained hollow particle board has higher static bending strength and lower dimensional change rate.
[0015] In the present invention, the functionality of the high-functionality polyol is greater than 2, for example, it may be 3, 4, 5, 6, etc.
[0016] Preferably, the polyol comprises polyether polyol and / or polyester polyol.
[0017] Preferably, the number average molecular weight of the polyol is 500-4000, for example, 500, 600, 800, 1000, 1200, 1400, 1600, 1800, 2000, 2200, 2400, 2600, 2800, 3000, 3200, 3400, 3600, 3800, 4000, etc.; the hydroxyl value is 35-450 mg KOH / g, for example, 35 mg KOH / g, 40 mg KOH / g, 45 mg KOH / g, 50 mg KOH / g, 60 mg KOH / g, 80 mg KOH / g, 100 mg KOH / g, 120 mg KOH / g, 140 mg KOH / g, 160 mg KOH / g, 180 mg KOH / g, 200 mg KOH / g, 220 mg KOH / g, 240 mg KOH / g, 260mg KOH / g, 280mg KOH / g, 300mg KOH / g, 320mg KOH / g, 340mg KOH / g, 360mg KOH / g, 380mg KOH / g, 400mg KOH / g, 420mg KOH / g, 440mg KOH / g, 450mg KOH / g, etc.
[0018] Preferably, the polyol comprises at least one of a combination of a low-functionality polyether polyol and a high-functionality polyether polyol, and a combination of a low-functionality polyester polyol and a high-functionality polyether polyol.
[0019] Preferably, when the polyol is selected from a combination of a low-functionality polyether polyol and a high-functionality polyether polyol, the low-functionality polyol includes polyether polyol A and / or polyether polyol B; the number average molecular weight of polyether polyol A is less than the number average molecular weight of polyether polyol B, and the hydroxyl value of polyether polyol A is greater than the hydroxyl value of polyether polyol B.
[0020] Preferably, the number average molecular weight of the polyether polyol A is 500-1500, for example, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, etc.; the hydroxyl value is 75-225 mg KOH / g, for example, 75 mg KOH / g, 80 mg KOH / g, 90 mg KOH / g, 100 mg KOH / g, 110 mg KOH / g, 120 mg KOH / g, 130 mg KOH / g, 140 mg KOH / g, 150 mg KOH / g, 160 mg KOH / g, 170 mg KOH / g, 180 mg KOH / g, 190 mg KOH / g, 200 mg KOH / g, 205 mg KOH / g, 210 mg KOH / g, 215 mg KOH / g, 220 mg The number average molecular weight of the polyether polyol B is 1500-2500, for example, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, etc.; the hydroxyl value is 45-75 mg KOH / g, for example, 45 mg KOH / g, 50 mg KOH / g, 55 mg KOH / g, 60 mg KOH / g, 65 mg KOH / g, 70 mg KOH / g, 75 mg KOH / g, etc.
[0021] Preferably, when the polyol is selected from a combination of a low-functionality polyether polyol and a high-functionality polyether polyol, the high-functionality polyether polyol includes polyether polyol C and / or polyether polyol D; the number average molecular weight of polyether polyol C is less than the number average molecular weight of polyether polyol D, and the hydroxyl value of polyether polyol C is greater than the hydroxyl value of polyether polyol D.
[0022] Preferably, the number average molecular weight of the polyether polyol C is 500-2500, for example, 500, 600, 700, 800, 900, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1800, 2000, 2200, 2400, 2500, etc.; the hydroxyl value is 65-450 mg KOH / g, for example, 65 mg KOH / g, 70 mg KOH / g, 80 mg KOH / g, 90 mg KOH / g, 100 mg KOH / g, 120 mg KOH / g, 140 mg KOH / g, 160 mg KOH / g, 180 mg KOH / g, 200 mg KOH / g, 220 mg KOH / g, 240 mg KOH / g, 260 mg KOH / g, 280 mg The number average molecular weight of the polyether polyol D is 2500-4000, for example, 2500, 2600, 2800, 3000, 3200, 3400, 3600, 3800, 4000, etc.; the hydroxyl value is 39-90 mg KOH / g, for example, 40 mg KOH / g, 50 mg KOH / g, 60 mg KOH / g, 70 mg KOH / g, 80 mg KOH / g, 90 mg KOH / g, etc.
[0023] Preferably, when the polyol is selected from a combination of a low-functionality polyether polyol and a high-functionality polyether polyol, the polyol comprises a combination of polyether polyol A and polyether polyol C, and / or a combination of polyether polyol B and polyether polyol D.
[0024] Preferably, when the polyol is selected from a combination of a low-functionality polyester polyol and a high-functionality polyether polyol, the number average molecular weight of the low-functionality polyester polyol is 1500-2500, and the hydroxyl value is 45-75 mg KOH / g; the number average molecular weight of the high-functionality polyether polyol is 500-2500, and the hydroxyl value is 65-450 mg KOH / g.
[0025] Preferably, the high-functionality polyol comprises a trifunctional polyol and / or a tetrafunctional polyol.
[0026] Preferably, the polyisocyanate comprises an aromatic polyisocyanate and / or an aliphatic polyisocyanate.
[0027] Preferably, the polyisocyanate includes at least one of isophorone diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate or polymethylene polyphenyl polyisocyanate, and more preferably at least one of toluene diisocyanate, diphenylmethane diisocyanate or polymethylene polyphenyl polyisocyanate.
[0028] In a second aspect, the present invention provides a method for preparing the polyurethane adhesive according to the first aspect, the preparation method comprising:
[0029] The polyol and polyisocyanate are reacted to obtain the polyurethane adhesive.
[0030] Preferably, the reaction temperature is 60-95°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, etc.; the reaction time is 2-6h, for example, 2h, 3h, 4h, 5h, 6h, etc.
[0031] In a third aspect, the present invention provides a hollow particle board, wherein the material of the hollow particle board includes wood particles and an adhesive; the adhesive includes the polyurethane adhesive according to the first aspect.
[0032] In the present invention, the material of the shavings includes wood material and / or non-wood material; illustratively, the material of the shavings can be poplar, pine, eucalyptus, fir, birch, hard miscellaneous wood, wheat straw, rice straw, cotton and linen stalks, corn stalks, sorghum stalks, reeds, bamboo, etc.; the thickness of the shavings is 0.15-5mm, the width is 0.4-15mm, and the length is 0.5-50mm; before use, the shavings must be dried to make their moisture content uniform; the moisture content of the shavings is 5-15%.
[0033] Preferably, the mass of the adhesive is 1.5-4% of the mass of the wood chips, for example, it can be 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.4%, 3.6%, 3.8%, 4%, etc.
[0034] Preferably, the material of the hollow particle board also includes a waterproofing agent.
[0035] In the present invention, the waterproofing agent includes paraffin and / or emulsified paraffin.
[0036] Preferably, the mass of the waterproofing agent is 0.2-0.4% of the mass of the wood chips, for example, it can be 0.2%, 0.22%, 0.24%, 0.26%, 0.28%, 0.3%, 0.32%, 0.34%, 0.36%, 0.38%, 0.4%, etc.
[0037] In a fourth aspect, the present invention provides a method for preparing the hollow particle board according to the third aspect, the preparation method comprising:
[0038] The hollow particle board is prepared by applying adhesive on the surface of the particles and adopting a pulse extrusion method.
[0039] Since polyurethane adhesives have good bonding properties to materials such as wood and metal, the problem of sticking boards is prone to occur during the production of hollow particle boards using polyurethane adhesives, which in turn affects the equipment operation efficiency and the surface quality of the boards. In the present invention, a pulse extrusion method is used to produce hollow particle boards, and no release agent is needed, so that the problem of sticking boards will not occur during the production process, thereby improving production efficiency and product quality. A specific polyurethane adhesive is used in combination with a pulse extrusion process, so that the hollow particle board obtained has high static bending strength, low dimensional change rate and thickness deviation, and there will be no problem of sticking boards during the production process, and the formaldehyde content of the particle board will not be increased, and the environmental protection level is high.
[0040] Preferably, the pressing plate temperature of the pulse extrusion is 120-220°C, for example, it can be 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, etc.
[0041] Preferably, the gap between the pressure plates of the pulse extrusion is 15 to 60 mm, for example, it can be 15 mm, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm, 50 mm, 55 mm, 60 mm, etc.
[0042] Preferably, the frequency of the pulse extrusion is 2 to 120 times / min, for example, 2 times / min, 4 times / min, 6 times / min, 8 times / min, 10 times / min, 15 times / min, 20 times / min, 25 times / min, 30 times / min, 35 times / min, 40 times / min, 45 times / min, 50 times / min, 55 times / min, 60 times / min, 65 times / min, 70 times / min, 75 times / min, 80 times / min, 85 times / min, 90 times / min, 95 times / min, 100 times / min, 105 times / min, 110 times / min, 115 times / min, 120 times / min, etc.; single The extrusion stroke is 2 to 200 mm, for example, it can be 2 mm, 4 mm, 6 mm, 8 mm, 10 mm, 15 mm, 20 mm, 25 mm, 30 mm, 35 mm, 40 mm, 45 mm, 50 mm, 55 mm, 60 mm, 65 mm, 70 mm, 75 mm, 80 mm, 85 mm, 90 mm, 95 mm, 100 mm, 105 mm, 110 mm, 115 mm, 120 mm, 125 mm, 130 mm, 135 mm, 140 mm, 145 mm, 150 mm, 155 mm, 160 mm, 165 mm, 170 mm, 175 mm, 180 mm, 185 mm, 190 mm, 195 mm, 200 mm, etc.
[0043] In the present invention, by controlling the extrusion frequency and the extrusion stroke, effective heat transfer is ensured, and the board will not stick, thereby maintaining a high surface quality of the board; at the same time, the static bending strength of the hollow particle board can be improved, and the dimensional change rate and thickness deviation of the hollow particle board can be reduced.
[0044] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] The polyurethane adhesive provided by the present invention adopts polymer polyol to modify isocyanate to form polyurethane adhesive, controls the isocyanate index within a specific range, and selects polyol with specific composition and proportion as the adhesive of hollow particle board, which can improve the static bending strength of hollow particle board and reduce the dimensional change rate and thickness deviation of hollow particle board; and the adhesive is a formaldehyde-free adhesive, which will not increase the formaldehyde emission of hollow particle board, thereby improving the environmental protection level of hollow particle board; the static bending strength of the hollow particle board is ≥2.2MPa, the extrusion dimensional change rate is ≤5.9%, and no formaldehyde is added. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0048] Unless otherwise specified, the materials used in the present invention are as follows:
[0049] Polyisocyanate
[0050] Polymethylene polyphenyl polyisocyanate (PMDI): CW20, -NCO content 30-32 wt%, Wanhua Chemical Group Co., Ltd.
[0051] Low functionality ether polyols
[0052] Difunctional polyether polyol C2010D, number average molecular weight 1000, hydroxyl value 112±3.5mg KOH / g, Wanhua Chemical Group Co., Ltd.;
[0053] Difunctional polyether polyol C2020, number average molecular weight 2000, hydroxyl value 56±1.5mg KOH / g, Wanhua Chemical Group Co., Ltd.
[0054] Low functionality polyester polyol
[0055] Difunctional polyester polyol FA2817P, number average molecular weight 2000, hydroxyl value 53-59 mg KOH / g, HuaDa Chemical Group.
[0056] High functionality polyether polyols
[0057] Trifunctional polyether polyol R2305, number average molecular weight 500, hydroxyl value 335±10mg KOH / g, Wanhua Chemical Group Co., Ltd.;
[0058] Tetrafunctional polyether polyol R8241, number average molecular weight 550, hydroxyl value 410±20mg KOH / g, Wanhua Chemical Group Co., Ltd.;
[0059] Trifunctional polyether polyol F3140, number average molecular weight about 4000, hydroxyl value 39.5-43.5 mg KOH / g, Wanhua Chemical Group Co., Ltd.
[0060] Waterproofing agent: No. 58 refined paraffin, Yangzi Petrochemical.
[0061] Eucalyptus shavings: moisture content 10%, thickness 1-2mm, width 3-5mm, length 3-15mm, Wanhua Ecological Board Industry.
[0062] In the present invention, the isocyanate index (R) is the molar ratio of isocyanate groups to hydroxyl groups in the preparation raw materials.
[0063] Example 1
[0064] The present embodiment provides a polyurethane adhesive, the preparation raw materials including 5.2kg of polyol and 100kg of PMDI; the polyol includes difunctional polyether polyol C2010D and trifunctional polyether polyol R2305 in a mass ratio of 1:0.3; the isocyanate index R is 50; the preparation method of the polyurethane adhesive includes: reacting the polyol and PMDI at 75°C for 4h to obtain the polyurethane adhesive.
[0065] Example 2
[0066] The present embodiment provides a polyurethane adhesive, the preparation raw materials including 5.6kg of polyol and 100kg of PMDI; the polyol includes difunctional polyether polyol C2020 and trifunctional polyether polyol F3140 in a mass ratio of 1:0.4; the isocyanate index R is 147; the preparation method of the polyurethane adhesive includes: reacting the polyol and PMDI at 65°C for 5h to obtain the polyurethane adhesive.
[0067] Example 3
[0068] The present embodiment provides a polyurethane adhesive, the preparation raw materials including 4.8kg of polyol and 100kg of PMDI; the polyol includes difunctional polyether polyol C2010D and tetrafunctional polyether polyol R8241 in a mass ratio of 1:0.2; the isocyanate index R is 55; the preparation method of the polyurethane adhesive includes: reacting the polyol and PMDI at 65°C for 5h to obtain the polyurethane adhesive.
[0069] Example 4
[0070] The present embodiment provides a polyurethane adhesive, the preparation raw materials including 5.6 kg of polyol and 100 kg of PMDI; the polyol includes difunctional polyester polyol FA2817P and trifunctional polyether polyol R2305 in a mass ratio of 1:0.4; the isocyanate index R is 56; the preparation method of the polyurethane adhesive includes: reacting the polyol and PMDI at 60° C. for 6 hours to obtain the polyurethane adhesive.
[0071] Example 5
[0072] This embodiment provides a polyurethane adhesive, which differs from Example 1 only in that the trifunctional polyether polyol R2305 is replaced by an equal mass of trifunctional polyether polyol F3140, and the content of PMDI is adjusted so that the R value remains unchanged. Other raw materials, amounts and preparation methods are the same as those in Example 1.
[0073] Example 6
[0074] This embodiment provides a polyurethane adhesive, which differs from Example 4 only in that the trifunctional polyether polyol R2305 is replaced by an equal mass of trifunctional polyether polyol F3140, and the content of PMDI is adjusted so that the R value remains unchanged. Other raw materials, amounts and preparation methods are the same as those in Example 4.
[0075] Comparative Example 1
[0076] This comparative example provides a polyurethane adhesive, which differs from Example 1 only in that the total molar amount of hydroxyl groups in the polyol remains unchanged, there is no trifunctional polyether polyol R2305, and other raw materials, amounts and preparation methods are the same as those in Example 1.
[0077] Comparative Example 2
[0078] This comparative example provides a polyurethane adhesive, which differs from Example 1 only in that the total molar amount of hydroxyl groups in the polyol remains unchanged, there is no difunctional polyether polyol C2010D, and other raw materials, amounts and preparation methods are the same as those in Example 1.
[0079] Comparative Example 3
[0080] This comparative example provides a polyurethane adhesive, which differs from Example 1 only in that the total molar amount of hydroxyl groups in the polyol is ensured to remain unchanged, the mass ratio of the difunctional polyether polyol C2010D to the trifunctional polyether polyol R2305 is 1:0.1, and other raw materials, amounts and preparation methods are the same as those in Example 1.
[0081] Comparative Example 4
[0082] This comparative example provides a polyurethane adhesive, which differs from Example 1 only in that the total molar amount of hydroxyl groups in the polyol is ensured to remain unchanged, the mass ratio of the difunctional polyether polyol C2010D to the trifunctional polyether polyol R2305 is 1:0.5, and other raw materials, amounts and preparation methods are the same as those in Example 1.
[0083] Comparative Example 5
[0084] This comparative example provides a polyurethane adhesive, which differs from Example 1 only in that the amount of PMDI is adjusted so that R is 38, and other raw materials, amounts and preparation methods are the same as those in Example 1.
[0085] Comparative Example 6
[0086] This comparative example provides a polyurethane adhesive, which differs from Example 1 only in that the amount of PMDI is adjusted so that R is 160, and other raw materials, amounts and preparation methods are the same as those in Example 1.
[0087] Comparative Example 7
[0088] This comparative example provides an adhesive, which is a melamine-modified urea-formaldehyde resin purchased from Sheng Wanjia.
[0089] Application Example 1
[0090] This application example provides a hollow particle board and a preparation method thereof, wherein the preparation method of the hollow particle board comprises:
[0091] 3kg of polyurethane adhesive (Example 1) and 0.2kg of waterproofing agent are evenly applied to the surface of 100kg of wood chips; the wood chips after adhesive application are extruded by pulse extrusion, wherein the pressing plate temperature is controlled at 180°C, the pressing plate gap is 35mm, the pulse extrusion frequency is 60 times / minute, and the single extrusion stroke is 8mm, to obtain the hollow particle board.
[0092] Application Example 2
[0093] This application example provides a hollow particle board and a preparation method thereof, wherein the preparation method of the hollow particle board comprises:
[0094] 3.5 kg of polyurethane adhesive (Example 2) and 0.3 kg of waterproofing agent are evenly applied to the surface of 100 kg of wood chips; the wood chips after adhesive application are extruded by pulse extrusion, wherein the pressing plate temperature is controlled at 120° C., the pressing plate gap is 35 mm, the pulse extrusion frequency is 120 times / minute, and the single extrusion stroke is 2 mm, to obtain the hollow particle board.
[0095] Application Example 3
[0096] This application example provides a hollow particle board and a preparation method thereof, wherein the preparation method of the hollow particle board comprises:
[0097] 2kg of polyurethane adhesive (Example 3) and 0.3kg of waterproofing agent are evenly applied to the surface of 100kg of wood chips; the wood chips after adhesive application are extruded by pulse extrusion, wherein the pressing plate temperature is controlled at 120°C, the pressing plate gap is 35mm, the pulse extrusion frequency is 2 times / minute, and the single extrusion stroke is 200mm, to obtain the hollow particle board.
[0098] Application Example 4
[0099] This application example provides a hollow particle board and a preparation method thereof, wherein the preparation method of the hollow particle board comprises:
[0100] 1.5 kg of polyurethane adhesive (Example 4) and 0.4 kg of waterproofing agent are evenly applied to the surface of 100 kg of wood chips; the wood chips after adhesive application are extruded by a pulse extrusion method, wherein the pressing plate temperature is controlled at 160° C., the pressing plate gap is 35 mm, the pulse extrusion frequency is 30 times / minute, and the single extrusion stroke is 20 mm, to obtain the hollow particle board.
[0101] Application Examples 5-6, Comparative Application Examples 1-7
[0102] Application Examples 5 to 6 and Comparative Application Examples 1 to 7 respectively provide a hollow particle board and a preparation method thereof, and the only difference between them and Application Example 1 is that the polyurethane adhesive is the adhesive provided in Example 5, Example 6, and Comparative Examples 1 to 7, respectively, and the other components, amounts, and preparation processes are the same as those in Application Example 1.
[0103] Comparative Application Example 8
[0104] This comparative application example provides a hollow particle board and a preparation method thereof, which differs from Application Example 1 only in that, in the preparation method, the pulse extrusion frequency is 1 time / minute, the single extrusion stroke is 480 mm, and the other components, amounts and preparation processes are the same as those in Application Example 1.
[0105] Performance Testing
[0106] The performance and formaldehyde emission of the hollow particleboard obtained were tested, and whether the board was sticky during hot pressing. Specifically, the performance of the obtained particleboard was measured according to "GBT 34717-2017 Extruded Particleboard"; the obtained particleboard was tested for formaldehyde emission using the climate chamber method according to "GBT 17657-2022 Test Methods for Physical and Chemical Properties of Artificial Boards and Veneer Artificial Boards". The specific test data and test results are shown in Table 1; Among them, the formaldehyde emission of the test wood particle raw material (i.e., eucalyptus wood particle) was 0.01 mg / m 3 .
[0107] Table 1
[0108]
[0109]
[0110] As can be seen from Table 1, the hollow particle board prepared by using the specific polyurethane adhesive of the present invention has a static bending strength of 2.2-2.6 MPa, a dimensional change rate in the extrusion direction of 5.5-5.9%, a small thickness dimensional deviation, and the formaldehyde emission is the same as that of the original particle material. No formaldehyde is added, and the board does not stick during hot pressing.
[0111] By comparing Application Example 1 with Comparative Application Examples 1 to 4, it can be seen that isocyanate must be modified with difunctional and higher-functionality polyols, and the ratio of difunctional and higher-functionality polyols must be within a specific range, so that the resulting sheet can have higher static bending strength and smaller extrusion dimensional change rate.
[0112] From the comparison between Application Example 1 and Comparative Application Examples 5 and 6, it can be seen that when the R value is lower than 50 or greater than 150, the dimensional stability or mechanical properties of the sheet material are significantly reduced.
[0113] From the comparison between Application Example 1 and Comparative Application Example 8, it can be seen that the pulse extrusion frequency must not be lower than 2 times / minute, otherwise the board is prone to sticking, resulting in large deviation in board thickness and a significant decrease in static bending strength.
[0114] From the comparison between Application Example 1 and Comparative Example 7, it can be seen that the hollow particle board prepared by using polyurethane adhesive has significant advantages over urea-formaldehyde resin in mechanical properties and dimensional stability.
[0115] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A polyurethane adhesive, characterized in that: The raw materials for preparing the polyurethane adhesive include polyol and polyisocyanate; In the preparation raw materials, the isocyanate index is 50 to 150; The polyol comprises a combination of a low functionality polyol and a high functionality polyol; The functionality of the low-functionality polyol is 2; the functionality of the high-functionality polyol is >2; The mass ratio of the low-functionality polyol to the high-functionality polyol is 1:0.2-0.
4.
2. The polyurethane adhesive according to claim 1, characterized in that: The polyols include polyether polyols and / or polyester polyols; Preferably, the number average molecular weight of the polyol is 500 to 4000, and the hydroxyl value is 35 to 450 mg KOH / g; Preferably, the polyol comprises at least one of a combination of a low-functionality polyether polyol and a high-functionality polyether polyol, and a combination of a low-functionality polyester polyol and a high-functionality polyether polyol.
3. The polyurethane adhesive according to claim 2, characterized in that: The polyol is selected from a combination of a low-functionality polyether polyol and a high-functionality polyether polyol, and the low-functionality polyether polyol includes polyether polyol A and / or polyether polyol B; The number average molecular weight of the polyether polyol A is less than the number average molecular weight of the polyether polyol B, and the hydroxyl value of the polymer polyol A is greater than the hydroxyl value of the polymer polyol B; Preferably, the number average molecular weight of the polyether polyol A is 500 to 1500, and the hydroxyl value is 75 to 225 mg KOH / g; the number average molecular weight of the polyether polyol B is 1500 to 2500, and the hydroxyl value is 45 to 75 mg KOH / g; Preferably, the polyol is selected from a combination of a low-functionality polyether polyol and a high-functionality polyether polyol, and the high-functionality polyether polyol includes polyether polyol C and / or polyether polyol D; The number average molecular weight of the polyether polyol C is less than the number average molecular weight of the polyether polyol D, and the hydroxyl value of the polyether polyol C is greater than the hydroxyl value of the polyether polyol D; Preferably, the number average molecular weight of the polyether polyol C is 500 to 2500, and the hydroxyl value is 65 to 450 mg KOH / g; the number average molecular weight of the polyether polyol D is 2500 to 4000, and the hydroxyl value is 39 to 90 mg KOH / g; Preferably, the polyol is selected from a combination of a low-functionality polyether polyol and a high-functionality polyether polyol, and the polyol includes a combination of polyether polyol A and polyether polyol C, and / or a combination of polyether polyol B and polyether polyol D.
4. The polyurethane adhesive according to claim 2, characterized in that: The polyol is selected from a combination of low-functionality polyester polyol and high-functionality polyether polyol, wherein the number average molecular weight of the low-functionality polyester polyol is 1500-2500 and the hydroxyl value is 45-75 mg KOH / g; the number average molecular weight of the high-functionality polyether polyol is 500-2500 and the hydroxyl value is 65-450 mg KOH / g.
5. The polyurethane adhesive according to any one of claims 1 to 4, characterized in that: The high-functionality polyol includes a trifunctional polyol and / or a tetrafunctional polyol; Preferably, the polyisocyanate comprises an aromatic polyisocyanate and / or an aliphatic polyisocyanate; Preferably, the polyisocyanate includes at least one of isophorone diisocyanate, dicyclohexylmethane diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate or polymethylene polyphenyl polyisocyanate, and more preferably at least one of toluene diisocyanate, diphenylmethane diisocyanate or polymethylene polyphenyl polyisocyanate.
6. A method for preparing the polyurethane adhesive according to any one of claims 1 to 5, characterized in that: The preparation method comprises: Reacting polyol and polyisocyanate to obtain the polyurethane adhesive; Preferably, the reaction temperature is 60-95° C. and the reaction time is 2-6 hours.
7. A hollow particle board, characterized in that: The materials of the hollow particle board include wood particles and adhesive; the adhesive includes the polyurethane adhesive according to any one of claims 1 to 5.
8. The hollow particle board according to claim 7, characterized in that: The mass of the adhesive is 1.5-4% of the mass of the wood chips; Preferably, the material of the hollow particle board further includes a waterproofing agent; Preferably, the mass of the waterproofing agent is 0.2-0.4% of the mass of the wood chips.
9. A method for preparing a hollow particle board according to claim 7 or 8, characterized in that: The preparation method comprises: The hollow particle board is prepared by applying adhesive on the surface of the wood particles and adopting a pulse extrusion method.
10. The preparation method according to claim 9, characterized in that: The pressing plate temperature of the pulse extrusion is 120-220°C; Preferably, the gap between the pressing plates of the pulse extrusion is 15 to 60 mm; Preferably, the frequency of the pulse extrusion is 2 to 120 times / min, and the single extrusion stroke is 2 to 200 mm.
Citation Information
Patent Citations
Inorganic composite fire retardant polyurethane rigid foam material and preparation method thereof
CN106478920A
Compound foaming adhesive for light shaving board
CN111234763A
Solvent-free single-component moisture-curable polyurethane adhesive suitable for wood and preparation method thereof
CN111704883A
An adhesive and its preparation and application
CN112391142A
Single-component polyurethane adhesive for wood and preparation method thereof
CN114133907A