Formaldehyde-free peeled full-poplar shaving board production process

By compiling and modifying the particleboard core layer of poplar wood shavings, combined with PMDI adhesive, a three-dimensional connection network structure is formed, which solves the problem of single particleboard performance and water absorption and moisture, and achieves high-quality and environmentally friendly Low density and high strength characteristics of particle board.

CN118927369AActive Publication Date: 2024-11-12HENGSHUI BA MAI LONG WOOD CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411177215.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing particle board has single performance, poor mechanical properties, low static curve strength, difficult to achieve low density and high strength, easy to absorb water and moisture, and insufficient moisture resistance.

Method used

By comparing the particleboard core layer of poplar wood shavings in different sizes, especially the addition of 0.4-0.6mm thin shavings, combined with PMDI adhesive, and modifying the waterproofing agent and deodorant to form a three-dimensional communication network Structure, improve static curvature strength and moisture-proof performance.

Benefits of technology

Under the process conditions where the aldehyde-free addition is maintained, the density of particleboards is reduced, the static curvature strength and moisture-proof performance are improved, and the market needs for high-quality and environmentally friendly particleboards are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011031090000121
    Figure BDA0005011031090000121
Patent Text Reader

Abstract

The invention provides a production process of a formaldehyde-free peeled full-poplar shaving board. The poplar wood shavings of the surface-core layer material of the shaving board are compounded in different sizes, especially the thin shavings of 0.4-0.6 mm are added, the shape of the shavings is improved, conditions are created for reducing the density of the shaving board, reducing deformation, improving the static bending intensity and improving the edge compactness, the PMDI adhesive is combined, and the waterproof agent and the deodorant are modified, so that the water-proof effect of the shaving board is improved, and the service life of the shaving board is prolonged. Production is carried out under the technological condition that no formaldehyde is added, the static bending intensity of the shaving board is improved, meanwhile, the density is as low as 600 kg / m < 3 >, the water absorption thickness swelling rate is reduced, the humidity resistance is improved, and therefore the formaldehyde-free peeled full-poplar low-density and high-strength shaving board is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of artificial boards, and in particular relates to a production process of formaldehyde-free peeled poplar wood particleboard. Background Art

[0002] Particleboard is a kind of man-made board made by cutting wood and other raw materials into pieces of certain specifications, drying, mixing with adhesives, additives, etc., and pressing at a certain temperature. The raw materials of particleboard are widely available, and the amount of glue used in the production process is small. The product has the characteristics of greater strength and higher stability, and has a very broad development space in my country. The adhesives of particleboard are mostly urea-formaldehyde resin glue and phenol-formaldehyde resin glue. The curing temperature of aldehyde adhesives is low, and they have good gluing effects on particleboards made of various plant materials such as wheat straw and rice husks. The hot pressing temperature is not high, so it is widely used in production, but it has the disadvantage of releasing free formaldehyde to pollute the environment and endanger the health of users; particleboard has poor mechanical properties, low static bending strength, and significantly reduced bending resistance after pressure, so reinforcements are needed to assist in improving its bearing capacity; in addition, since the main material of particleboard is wood, it is easy to absorb water and moisture, which causes the compacted part inside the particleboard to expand and spread, causing the entire board to be damaged. In summary, the existing particle board has single performance, and cannot achieve low density, high moisture resistance, and no deformation in furniture door surfaces, wall cabinet integration, and decoration scenes. Its performance in strength, odorlessness, moisture resistance, and load-bearing capacity is not as good as market expectations.

[0003] Therefore, how to use innovative processes and material selection to improve the static bending strength of particleboard during use, expand the application scenarios, reduce the water absorption thickness expansion rate, and improve moisture-proof performance while maintaining the formaldehyde-free particleboard products, has become a direction that needs to be focused on. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a formaldehyde-free peeled poplar particleboard production process, aiming to solve the problems of the existing particleboard having single performance, poor mechanical properties, low static bending strength, difficulty in achieving the technical effect of low density and high strength, and easy absorption of water and moisture and insufficient moisture-proof ability.

[0005] The present invention improves the particle shape by compounding poplar wood particles of the particleboard surface core layer material in different sizes, especially adding 0.4-0.6mm thin particles, creating conditions for reducing the density of the particleboard, reducing deformation, improving the static bending strength and improving the edge density. The invention combines PMDI adhesive, and modifies the waterproof agent and deodorant. The production is carried out under the process condition of maintaining the process of no formaldehyde addition, thereby improving the static bending strength of the particleboard and reducing the density to 600kg / m 3, and reduce the water absorption thickness expansion rate, improve moisture resistance, so as to obtain formaldehyde-free peeling all-poplar low-density and high-strength particleboard.

[0006] The technical solution of the present invention is as follows:

[0007] A production process for formaldehyde-free peeled poplar particleboard comprises the following preparation steps:

[0008] Step S1: preparing a surface material and a core material, wherein the surface material comprises a first surface material and a second surface material, wherein the first surface material is 20 parts of poplar wood shavings, the second surface material is 20 parts of poplar wood shavings, and the core material is 24 parts of poplar wood shavings I and 36 parts of poplar wood shavings II;

[0009] Step S2: sizing the surface layer material and the core layer material described in step S1, uniformly mixing the surface layer material, PMDI, acidified paraffin and deodorant in a first mixer to obtain a sizing surface layer material, and uniformly mixing the core layer material, PMDI, amide paraffin and deodorant in a second mixer to obtain a sizing core layer material;

[0010] Step S3: paving the glued surface layer material described in step S2 to form a first slab surface layer, paving on the first glued surface layer material to form a slab core layer, and paving on the side of the slab core layer away from the first slab surface layer to form a second slab surface layer, to obtain a slab;

[0011] Step S4: pre-pressing the slab using a pre-pressing machine, and continuously flat-pressing the pre-pressed slab using a continuous flat-pressing machine to obtain a formaldehyde-free peeled poplar particleboard.

[0012] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the objectives and beneficial effects of the present invention can be better achieved and realized.

[0013] As a preferred technical solution of the present invention, the poplar wood shavings I and poplar wood shavings II are obtained by mechanical processing of poplar wood shavings, the poplar wood shavings I are 0.4 mm thick and 45 mm long; the poplar wood shavings II are 0.6 mm thick and 45 mm long.

[0014] Poplar wood shavings I are relatively larger in volume and can serve as the main support of the particleboard. Poplar wood shavings II are smaller in size and easier to compress, so they can fill the gaps in the main support, making the pores inside the sample smaller and the particles more tightly bonded. With the help of thin particles, the density of the particleboard can be effectively reduced while the static bending strength and edge density can be improved, and the thickness expansion rate of the particleboard can be reduced.

[0015] As a preferred technical solution of the present invention, the preparation method of the acidified paraffin is as follows: 100 parts of emulsified paraffin are added to a reaction kettle with a stirrer and heated to 150°C; then 20 parts of maleic anhydride are added and stirred evenly under nitrogen protection; then 10 parts of dibenzoyl peroxide are added, the temperature is controlled at 180°C, the reaction is carried out for 1 hour, and the acidified paraffin is obtained after purification.

[0016] As a preferred technical solution of the present invention, the preparation method of the amidated paraffin is as follows: 100 parts of emulsified paraffin and 200 parts of toluene are added to a reactor with a stirrer, heated to 90°C, and stirred for 0.5h; 5 parts of ethylenediamine are added to 10 parts of benzenesulfonic acid solution (mass fraction concentration is 20%), and stirred evenly to obtain an amidating reagent; 20 parts of the amidating reagent are added to the reactor, stirred for reaction at a temperature of 100°C for 3h, and after the reaction is completed, the amidated paraffin is obtained by condensation and separation.

[0017] The maleic anhydride group of the acidified paraffin in the surface layer can react with the isocyanate group of PMDI, and the PMDI in the core layer reacts with the amide paraffin to form urea compounds. At the same time, the maleic anhydride group of the modified paraffin in the surface layer reacts with the amino group of the modified paraffin in the core layer to form a cyclization reaction. The modified paraffin acts as a bridge to form a three-dimensional interconnected network structure that penetrates the surface layer and the core layer, significantly improving the physical properties of the particleboard, such as the static bending strength. At the same time, paraffin is a hydrophobic substance, and the network structure formed by the modified paraffin can also block moisture and prevent moisture from entering the pores of the wood particles, thereby improving the moisture-proof performance of the particleboard.

[0018] As a preferred technical solution of the present invention, the deodorant is a nano-metal deodorant; the preparation method of the nano-metal deodorant is: add 80 parts of deionized water into a reactor, adjust the temperature to 70°C, add 15 parts of polyethylene glycol, and stir for 0.5h; cool to 40°C, add 5 parts of α-cyclodextrin dissolving agent, stir evenly, add 3 parts of ricinoleic acid zinc ester, and stir at a speed of 4000r / min for 1h; control the temperature to 50°C, add 10 parts of nano zinc oxide, stir at a speed of 4000r / min for 0.5h, cool to 25°C, add 3 parts of dodecyl dimethyl benzyl ammonium bromide, stir evenly to obtain the nano-metal deodorant.

[0019] Nano zinc oxide in the deodorant has good thermal conductivity. Its high thermal conductivity enables it to transfer heat effectively. The good thermal conductivity allows the surface material and the core material to be heated evenly, which is more conducive to the reaction of isocyanate and improves the strength of the particleboard through the full reaction of PMDI adhesive.

[0020] Preferably, the amount of PMDI added in the sizing in step S2 is 25 kg / m 3 , the amount of acidified paraffin added is 6kg / m 3The addition amount of amide paraffin is 7kg / m 3 , the amount of deodorant added is 1kg / m 3 .

[0021] Preferably, in step S3, the moisture content of the first slab surface layer and the second slab surface layer is 17%, and the moisture content of the slab core layer is 4%.

[0022] Preferably, in step S3, the thickness of the first slab surface layer and the second slab surface layer is 2-3 mm, and the thickness of the slab core layer is 4-8 mm.

[0023] Preferably, in step S4, when the continuous flat press continuously flattens the pre-pressed slab, the pre-pressed slab passes through the first zone, the second zone, the third zone and the fourth zone in sequence at a uniform speed; the maximum pressure in the first zone is controlled to be 500N / cm 2 , the temperature is 240℃; the maximum pressure in the second zone is 400N / cm 2 , temperature is 230℃; the maximum pressure in the third zone is 200N / cm 2 , the temperature is 220℃; the maximum pressure in the fourth zone is 200N / cm 2 , the temperature is 200℃; the operating pressure of the hydraulic system controlling the continuous press is 300bar.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention uses PMDI adhesive and peeled poplar wood shavings for continuous flat pressing to produce a three-layer structure. Through innovative processes and material selection, with the help of the addition of 0.4-0.6 mm thin shavings, the shavings morphology is improved, the pores inside the sample are made smaller, the bonding between the shavings is tighter, and the density of the particleboard is effectively reduced while the static bending strength and edge density are improved. The production is carried out under the process conditions of maintaining no formaldehyde addition, and the formaldehyde-free peeled poplar low-density and high-strength particleboard is obtained, which meets the market's growing demand for high-quality, environmentally friendly particleboards.

[0026] (2) The present invention improves the internal bonding strength, increases the static bending strength, and reduces the water absorption thickness expansion rate of the particleboard by compounding wood particles of different sizes; forms a three-dimensional interconnected network structure that penetrates the surface layer and the core layer by using modified paraffin wax as a bridge, significantly improving the static bending strength and other physical properties of the particleboard; in addition, the modified paraffin wax is used as a bridge to form a three-dimensional interconnected network structure that penetrates the surface layer and the core layer, significantly improving the static bending strength and other physical properties of the particleboard; effectively transfers heat by containing nano-metal deodorizers to facilitate the reaction of isocyanate, and improves the strength of the particleboard through the full reaction of the PMDI adhesive. DETAILED DESCRIPTION

[0027] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0028] The sources of some components in the embodiments and comparative examples are as follows:

[0029] Wood shavings: Poplar wood shavings were purchased from Wanhua Jingzhou Company; Poplar wood shavings I were obtained by mechanical processing of poplar wood shavings (thickness 0.4 mm, length 45 mm); Poplar wood shavings II were obtained by mechanical processing of poplar wood shavings (thickness 0.6 mm, length 45 mm).

[0030] Adhesive: PMDI adhesive was purchased from Wanhua Chemical Group Co., Ltd.; urea-formaldehyde resin adhesive was purchased from Zibo Huasen Adhesive Co., Ltd.

[0031] Paraffin: Emulsified paraffin, purchased from Hansheng Group (solid content 42%).

[0032] Preparation of acidified paraffin: 100 parts of emulsified paraffin (purchased from Hansheng Group) are added to a reactor with a stirrer and heated to 150°C; then 20 parts of maleic anhydride (CAS No. 108-31-6) are added and stirred evenly under nitrogen protection; then 10 parts of dibenzoyl peroxide (CAS No. 94-36-0) are added, the temperature is controlled at 180°C, the reaction is carried out for 1 hour, and the acidified paraffin is obtained after purification.

[0033] Preparation of amidated paraffin: 100 parts of emulsified paraffin (purchased from Hansheng Group) and 200 parts of toluene (CAS No. 108-88-3) are added to a reactor with a stirrer, heated to 90°C, and stirred for 0.5h; 5 parts of ethylenediamine (CAS No. 107-15-3) are added to 10 parts of 20% mass fraction benzenesulfonic acid solution (benzenesulfonic acid CAS No. 3453-84-7), and stirred evenly to obtain an amidating reagent; 20 parts of the amidating reagent are added to the reactor, stirred and reacted at a temperature of 100°C for 3h, and after the reaction is completed, the amidated paraffin is obtained by condensation and separation.

[0034] Preparation of nano metal deodorant: 80 parts of deionized water are added to a reactor, the temperature is adjusted to 70°C, 15 parts of polyethylene glycol (CAS No. 25322-68-3) are added, and stirred for 0.5h; the temperature is lowered to 40°C, 5 parts of α-cyclodextrin (CAS No. 51211-51-9) solvent are added, and after stirring evenly, 3 parts of ricinoleic acid zinc ester (CAS No. 13040-19-2) are added, and stirred at a speed of 4000r / min for 1h; the temperature is controlled to 50°C, 10 parts of nano zinc oxide (CAS No. 1314-13-2) are added, and stirred at a speed of 4000r / min for 0.5h, the temperature is lowered to 25°C, 3 parts of dodecyl dimethyl benzyl ammonium bromide (CAS No. 7281-04-1) are added, and after stirring evenly, a nano metal deodorant is obtained.

[0035] Example 1

[0036] This embodiment provides a process for producing formaldehyde-free peeled poplar particleboard, comprising the following steps:

[0037] Step S1: preparing a surface material and a core material, wherein the surface material comprises a first surface material and a second surface material, wherein the first surface material is 20 parts of poplar wood shavings, the second surface material is 20 parts of poplar wood shavings, and the core material is 24 parts of poplar wood shavings I and 36 parts of poplar wood shavings II;

[0038] Step S2: Gluing the surface layer material and the core layer material described in step S1, uniformly mixing the surface layer material, PMDI adhesive, acidified paraffin, and nano-metal deodorant in a first mixer to obtain a sizing surface layer material, and uniformly mixing the core layer material, PMDI adhesive, amide paraffin, and nano-metal deodorant in a second mixer to obtain a sizing core layer material; the amount of PMDI added in the sizing is 25kg / m 3 , the amount of acidified paraffin added is 6kg / m 3 The addition amount of amide paraffin is 7kg / m 3 , the amount of deodorant added is 1kg / m 3 ;

[0039] Step S3: Paving the glued surface layer material described in step S2 to form a first slab surface layer, paving on the first glued surface layer material to form a slab core layer, and paving on the side of the slab core layer away from the first slab surface layer to form a second slab surface layer, to obtain a slab; controlling the moisture content of the first slab surface layer and the second slab surface layer to be 17%, and the moisture content of the slab core layer to be 4%; the thickness of the first slab surface layer and the second slab surface layer to be 3 mm, and the thickness of the slab core layer to be 8 mm;

[0040] Step S4: Use a pre-pressing machine to pre-press the slab, and use a continuous flat press to continuously flat-press the pre-pressed slab, so that the pre-pressed slab passes through the first zone, the second zone, the third zone and the fourth zone in sequence at a uniform speed; control the maximum pressure of the first zone to be 500N / cm 2 , the temperature is 240℃; the maximum pressure in the second zone is 400N / cm 2 , temperature is 230℃; the maximum pressure in the third zone is 200N / cm 2 , the temperature is 220℃; the maximum pressure in the fourth zone is 200N / cm 2 , the temperature is 200℃; the operating pressure of the hydraulic system controlling the continuous flat press is 300bar; after continuous flat pressing, a formaldehyde-free peeled poplar particleboard is obtained.

[0041] Example 2

[0042] This embodiment provides a process for producing formaldehyde-free peeled poplar particleboard, comprising the following steps:

[0043] Step S1: preparing a surface material and a core material, wherein the surface material comprises a first surface material and a second surface material, wherein the first surface material is 20 parts of poplar wood shavings, the second surface material is 20 parts of poplar wood shavings, and the core material is 24 parts of poplar wood shavings I and 36 parts of poplar wood shavings II;

[0044] Step S2: Gluing the surface layer material and the core layer material described in step S1, uniformly mixing the surface layer material, PMDI adhesive, acidified paraffin, and nano-metal deodorant in a first mixer to obtain a sizing surface layer material, and uniformly mixing the core layer material, PMDI adhesive, amide paraffin, and nano-metal deodorant in a second mixer to obtain a sizing core layer material; the amount of PMDI added in the sizing is 25kg / m 3 , the amount of acidified paraffin added is 6kg / m 3 The addition amount of amide paraffin is 7kg / m 3 , the amount of deodorant added is 1kg / m 3 ;

[0045] Step S3: Paving the glued surface layer material described in step S2 to form a first slab surface layer, paving on the first glued surface layer material to form a slab core layer, and paving on the side of the slab core layer away from the first slab surface layer to form a second slab surface layer, to obtain a slab; controlling the moisture content of the first slab surface layer and the second slab surface layer to be 17%, and the moisture content of the slab core layer to be 4%; the thickness of the first slab surface layer and the second slab surface layer to be 2 mm, and the thickness of the slab core layer to be 4 mm;

[0046] Step S4: Use a pre-pressing machine to pre-press the slab, and use a continuous flat press to continuously flat-press the pre-pressed slab, so that the pre-pressed slab passes through the first zone, the second zone, the third zone and the fourth zone in sequence at a uniform speed; control the maximum pressure of the first zone to be 500N / cm 2 , the temperature is 240℃; the maximum pressure in the second zone is 400N / cm 2 , temperature is 230℃; the maximum pressure in the third zone is 200N / cm 2 , the temperature is 220℃; the maximum pressure in the fourth zone is 200N / cm 2 , the temperature is 200℃; the operating pressure of the hydraulic system controlling the continuous flat press is 300bar; after continuous flat pressing, a formaldehyde-free peeled poplar particleboard is obtained.

[0047] Example 3

[0048] This embodiment provides a process for producing formaldehyde-free peeled poplar particleboard, comprising the following steps:

[0049] Step S1: preparing a surface material and a core material, wherein the surface material comprises a first surface material and a second surface material, wherein the first surface material is 20 parts of poplar wood shavings, the second surface material is 20 parts of poplar wood shavings, and the core material is 24 parts of poplar wood shavings I and 36 parts of poplar wood shavings II;

[0050] Step S2: Gluing the surface layer material and the core layer material described in step S1, uniformly mixing the surface layer material, PMDI adhesive, acidified paraffin, and nano-metal deodorant in a first mixer to obtain a sizing surface layer material, and uniformly mixing the core layer material, PMDI adhesive, amide paraffin, and nano-metal deodorant in a second mixer to obtain a sizing core layer material; the amount of PMDI added in the sizing is 25kg / m 3 , the amount of acidified paraffin added is 6kg / m 3 The addition amount of amide paraffin is 7kg / m 3 , the amount of deodorant added is 1kg / m 3 ;

[0051] Step S3: Paving the glued surface layer material described in step S2 to form a first slab surface layer, paving on the first glued surface layer material to form a slab core layer, and paving on the side of the slab core layer away from the first slab surface layer to form a second slab surface layer, to obtain a slab; controlling the moisture content of the first slab surface layer and the second slab surface layer to be 17%, and the moisture content of the slab core layer to be 4%; the thickness of the first slab surface layer and the second slab surface layer to be 3 mm, and the thickness of the slab core layer to be 7 mm;

[0052] Step S4: Use a pre-pressing machine to pre-press the slab, and use a continuous flat press to continuously flat-press the pre-pressed slab, so that the pre-pressed slab passes through the first zone, the second zone, the third zone and the fourth zone in sequence at a uniform speed; control the maximum pressure of the first zone to be 500N / cm 2 , the temperature is 240℃; the maximum pressure in the second zone is 400N / cm 2 , temperature is 230℃; the maximum pressure in the third zone is 200N / cm 2 , the temperature is 220℃; the maximum pressure in the fourth zone is 200N / cm 2 , the temperature is 200℃; the operating pressure of the hydraulic system controlling the continuous flat press is 300bar; after continuous flat pressing, a formaldehyde-free peeled poplar particleboard is obtained.

[0053] Example 4

[0054] This embodiment provides a production process for formaldehyde-free peeled poplar particleboard. The only difference from Example 1 is that in this embodiment, 24 parts of poplar wood shavings I and 36 parts of poplar wood shavings II in the core layer are replaced with 60 parts of poplar wood shavings, and the rest is the same as Example 1.

[0055] Example 5

[0056] This embodiment provides a production process for formaldehyde-free peeled poplar particleboard. The only difference from Embodiment 1 is that the acidified paraffin in the surface layer is replaced by emulsified paraffin, and the amide paraffin in the core layer is replaced by emulsified paraffin. The rest is the same as Embodiment 1.

[0057] Example 6

[0058] This embodiment provides a process for producing formaldehyde-free peeled poplar particleboard. The only difference from Embodiment 1 is that the nano-metal deodorant is replaced with a zinc ricinoleate solution (mass fraction concentration 4%) deodorant, and the rest is the same as Embodiment 1.

[0059] Comparative Example 1

[0060] This comparative example provides a particleboard production process, comprising the following steps:

[0061] Step S1: preparing a surface material and a core material, wherein the surface material comprises a first surface material and a second surface material, wherein the first surface material is 20 parts of poplar wood shavings, the second surface material is 20 parts of poplar wood shavings, and the core material is 60 parts of poplar wood shavings;

[0062] Step S2: Gluing the surface layer material and the core layer material described in step S1, uniformly mixing the surface layer material, urea-formaldehyde resin adhesive, emulsified paraffin, and ricinoleic acid zinc ester solution (mass fraction concentration 4%) and deodorant in a first mixer to obtain a sizing surface layer material, and uniformly mixing the core layer material, urea-formaldehyde resin adhesive, emulsified paraffin, and ricinoleic acid zinc ester solution (mass fraction concentration 4%) and deodorant in a second mixer to obtain a sizing core layer material; the addition amount of urea-formaldehyde resin adhesive in the sizing is 25kg / m 3 , the amount of emulsified paraffin added is 6kg / m 3 , the amount of deodorant added is 1kg / m 3 ;

[0063] Step S3: Paving the glued surface layer material described in step S2 to form a first slab surface layer, paving on the first glued surface layer material to form a slab core layer, and paving on the side of the slab core layer away from the first slab surface layer to form a second slab surface layer, to obtain a slab; controlling the moisture content of the first slab surface layer and the second slab surface layer to be 17%, and the moisture content of the slab core layer to be 4%; the thickness of the first slab surface layer and the second slab surface layer to be 3 mm, and the thickness of the slab core layer to be 8 mm;

[0064] Step S4: Use a pre-pressing machine to pre-press the slab, and use a continuous flat press to continuously flat-press the pre-pressed slab, so that the pre-pressed slab passes through the first zone, the second zone, the third zone and the fourth zone in sequence at a uniform speed; control the maximum pressure of the first zone to be 500N / cm 2 , the temperature is 240℃; the maximum pressure in the second zone is 400N / cm 2 , temperature is 230℃; the maximum pressure in the third zone is 200N / cm 2 , the temperature is 220℃; the maximum pressure in the fourth zone is 200N / cm 2 , the temperature is 200℃; the operating pressure of the hydraulic system controlling the continuous flat press is 300bar; after continuous flat pressing, a formaldehyde-free peeled poplar particleboard is obtained.

[0065] Comparative Example 2

[0066] This comparative example provides a particleboard production process, which is different from comparative example 1 only in that the surface layer of this comparative example uses acidified paraffin instead of emulsified paraffin.

[0067] Comparative Example 3

[0068] This comparative example provides a particleboard production process, which is different from comparative example 1 only in that the core layer of this comparative example uses amide paraffin instead of emulsified paraffin.

[0069] The performance of the particleboard provided in the above embodiments and comparative examples was tested, and the testing method was as follows:

[0070] Formaldehyde emission: Tested in accordance with the requirements of GB 18580-2017 Limits of formaldehyde emission from artificial boards and their products for interior decoration and renovation materials.

[0071] Static bending strength: Tested in accordance with the requirements of GB / T 4897-2015 Particleboard.

[0072] Water absorption thickness expansion rate: Tested in accordance with the requirements of GB / T 4897-2015 Particleboard.

[0073] Density: Test according to the requirements of GB / T 17657-2013 Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels.

[0074] The above performance test data is shown in Table 1.

[0075] Table 1 Performance test results

[0076]

[0077] From the above content, it can be seen that the present invention obtains formaldehyde-free peeled poplar particleboard (Example 1 to Example 3) by compounding different sizes of poplar wood particles, which are the core layer materials of the particleboard, combining PMDI adhesive, and modifying the waterproofing agent and the deodorant. No formaldehyde release is detected, the static bending strength is 20.1-20.3MPa, the water absorption thickness expansion rate is 2.2-2.4%, and the density is 600kg / m 3 .

[0078] Compared with Example 1, if the core layer does not use 24 parts of poplar wood shavings I and 36 parts of poplar wood shavings II, the static bending strength decreases, the water absorption thickness expansion rate increases, and the density increases (Example 4); compared with Example 1, if the surface layer does not use acidified paraffin and the core layer does not use amide paraffin, the static bending strength decreases and the water absorption thickness expansion rate increases (Example 5); compared with Example 1, if the nano-metal deodorant is not used, the static bending strength decreases (Example 6).

[0079] Comparative Example 1 does not adopt the technical innovation of the present invention, and the formaldehyde emission of the particleboard is 0.128 mg / m 3 , static bending strength is 15.1MPa, water absorption thickness expansion rate is 5.2%, density is 650kg / m 3 ; Compared with Comparative Example 1, if the surface layer uses acidified paraffin, the static bending strength is improved (Comparative Example 2); Compared with Comparative Example 1, if the core layer uses amide paraffin, the static bending strength is improved (Comparative Example 3).

[0080] In summary, the present invention improves the particle shape by compounding the poplar wood particles of the particleboard surface core layer material in different sizes, especially adding 0.4-0.6 mm thin particles, creating conditions for reducing the density of the particleboard, reducing deformation, improving the static bending strength and improving the edge density, combining with PMDI adhesive, and modifying the waterproof agent and deodorant, and producing under the process condition of maintaining no formaldehyde addition, thereby improving the static bending strength of the particleboard and reducing the density to 600 kg / m 3 , and reduce the water absorption thickness expansion rate, improve moisture resistance, so as to obtain formaldehyde-free peeling all-poplar low-density and high-strength particleboard.

[0081] The applicant declares that the present invention illustrates the detailed process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A production process for formaldehyde-free peeled poplar particleboard, characterized in that: The method comprises the following preparation steps: Step S1: preparing a surface material and a core material, wherein the surface material comprises a first surface material and a second surface material, wherein the first surface material is 20 parts of poplar wood shavings, the second surface material is 20 parts of poplar wood shavings, and the core material is 24 parts of poplar wood shavings I and 36 parts of poplar wood shavings II; Step S2: sizing the surface layer material and the core layer material described in step S1, uniformly mixing the surface layer material, PMDI, acidified paraffin and deodorant in a first mixer to obtain a sizing surface layer material, and uniformly mixing the core layer material, PMDI, amide paraffin and deodorant in a second mixer to obtain a sizing core layer material; Step S3: paving the glued surface layer material described in step S2 to form a first slab surface layer, paving on the first glued surface layer material to form a slab core layer, and paving on the side of the slab core layer away from the first slab surface layer to form a second slab surface layer, to obtain a slab; Step S4: pre-pressing the slab using a pre-pressing machine, and continuously flat-pressing the pre-pressed slab using a continuous flat-pressing machine to obtain a formaldehyde-free peeled poplar particleboard.

2. The process for producing formaldehyde-free peeled poplar particleboard according to claim 1, characterized in that: The poplar wood shavings I and poplar wood shavings II are obtained by mechanical processing of poplar wood shavings. The poplar wood shavings I have a thickness of 0.4 mm and a length of 45 mm; the poplar wood shavings II have a thickness of 0.6 mm and a length of 45 mm.

3. The process for producing formaldehyde-free peeled poplar particleboard according to claim 1, characterized in that: The preparation method of the acidified paraffin is as follows: 100 parts of emulsified paraffin are added into a reaction kettle with a stirrer, and heated to 150° C.; then 20 parts of maleic anhydride are added, and stirred evenly under nitrogen protection; then 10 parts of dibenzoyl peroxide are added, the temperature is controlled at 180° C., the reaction is performed for 1 hour, and the acidified paraffin is obtained after purification.

4. The process for producing formaldehyde-free peeled poplar particleboard according to claim 1, characterized in that: The preparation method of the amidated paraffin is as follows: 100 parts of emulsified paraffin and 200 parts of toluene are added into a reaction kettle with a stirrer, heated to 90°C, and stirred for 0.5h; 5 parts of ethylenediamine are added into 10 parts of benzenesulfonic acid solution, and stirred evenly to obtain an amidating agent; 20 parts of the amidating agent are added into the reaction kettle, stirred and reacted at a temperature of 100°C for 3h, and after the reaction is completed, the amidated paraffin is obtained by condensation and separation.

5. The process for producing formaldehyde-free peeled poplar particleboard according to claim 1, characterized in that: The deodorant is a deodorant containing nano metals.

6. The process for producing formaldehyde-free peeled poplar particleboard according to claim 5, characterized in that: The preparation method of the nano metal deodorant is as follows: 80 parts of deionized water are added into a reactor, the temperature is adjusted to 70°C, 15 parts of polyethylene glycol are added, and the mixture is stirred for 0.5h; the temperature is lowered to 40°C, 5 parts of α-cyclodextrin dissolving agent are added, the mixture is stirred evenly, 3 parts of ricinoleic acid zinc ester are added, and the mixture is stirred at a speed of 4000r / min for 1h; the temperature is controlled to 50°C, 10 parts of nano zinc oxide are added, the mixture is stirred at a speed of 4000r / min for 0.5h, the temperature is lowered to 25°C, 3 parts of dodecyl dimethyl benzyl ammonium bromide are added, and the mixture is stirred evenly to obtain the nano metal deodorant.

7. The process for producing formaldehyde-free peeled poplar particleboard according to claim 1, characterized in that: The amount of PMDI added in the sizing in step S2 is 25 kg / m 3 , the amount of acidified paraffin added is 6kg / m 3 The addition amount of amide paraffin is 7kg / m 3 , the amount of deodorant added is 1kg / m 3 .

8. The process for producing formaldehyde-free peeled poplar particleboard according to claim 1, characterized in that: In step S3, the moisture content of the first slab surface layer and the second slab surface layer is 17%, and the moisture content of the slab core layer is 4%.

9. The process for producing formaldehyde-free peeled poplar particleboard according to claim 1, characterized in that: In step S3, the thickness of the first slab surface layer and the second slab surface layer is 2-3 mm, and the thickness of the slab core layer is 4-8 mm.

10. The process for producing formaldehyde-free peeled poplar particleboard according to claim 1, characterized in that: When the continuous flat press in step S4 continuously flattens the pre-pressed slab, the pre-pressed slab passes through the first zone, the second zone, the third zone and the fourth zone at a uniform speed in sequence; the maximum pressure in the first zone is controlled to be 500 N / cm 2 , the temperature is 240℃; the maximum pressure in the second zone is 400N / cm 2 , the temperature is 230℃; The maximum pressure in the third zone is 200N / cm 2 , the temperature is 220℃; the maximum pressure in the fourth zone is 200N / cm 2 , The temperature is 200°C; the operating pressure of the hydraulic system controlling the continuous flat press is 300 bar.

Citation Information

Patent Citations

  • Method for making a polyurea-polyurethane composite structure substantially free of volatile organic compounds

    CA2399984A1

  • Fire-retardant polyolefin based wood plastic composite material and preparation method thereof

    CN102321374A

  • Production method for particle board used for formaldehyde-free environment-friendly floorboard substrate

    CN106272862A

  • Method for producing wood composites containing thixotropic binder compositions

    JP2002533249A