Polyurethane adhesive enhanced by utilizing molecular pulley effect as well as preparation method and application of polyurethane adhesive
By introducing polyrothane into polyurethane adhesive, the molecular pulley effect is used to improve the compatibility between parathra and polyurethane, the problem of insufficient bonding strength and toughness of polyurethane adhesive is solved, and high-performance environmental protection is achieved Continuous polyurethane adhesive, suitable for bonding of wood artificial boards.
Patent Information
- Application Number
- CN202411255029.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-09
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material synthesis and wood-based panels, and in particular to a polyurethane adhesive enhanced by molecular pulley effect, and a preparation method and application thereof. Background Art
[0002] Polyurethane adhesives are made by reacting polyester or polyether polyols with isocyanates. They have the advantages of excellent flexibility, low temperature resistance, wear resistance, good curing speed, etc. They have high adhesion to various substrates such as metal, wood, and plastic, and are widely used in furniture, packaging, construction, cargo, transportation and other industries. However, the polyols currently used to prepare polyurethane adhesives usually come from non-renewable petroleum resources, which have disadvantages such as high pollution and high cost. As the country vigorously advocates green production, some renewable biomass raw materials have been explored and become substitutes for petroleum-based polyols. Vegetable oil is a typical renewable resource. Its easy availability and derivability make it the most utilized renewable resource in industry and academia.
[0003] Castor oil is a ricinoleic acid triglyceride that is abundant, inexpensive, and non-toxic. Unlike other vegetable oils, it has an average hydroxyl function of 2.7 and is superior to other vegetable oils in the preparation of cross-linked macromolecules. Polyurethane adhesives prepared using castor oil as a polyol have the advantages of high biodegradability and low ecotoxicity. In addition, the long-chain non-polar fatty acid segments of castor oil can improve the water resistance and moisture resistance of polyurethane adhesives. However, castor oil-based polyurethane adhesives have low bonding strength, which significantly limits their application range. Therefore, there is a need to further improve their performance.
[0004] At present, introducing natural clay as filler into polyurethane adhesives has become one of the effective strategies to improve the mechanical strength of polyurethane. Palygorskite is a water-rich magnesium aluminum silicate clay with a unique nanorod crystal structure. It has attracted extensive attention from researchers due to its good mechanical strength and elasticity. However, palygorskite is prone to agglomeration in the polymer matrix and has weak compatibility with polyurethane adhesives, which greatly weakens the effect of palygorskite on the performance enhancement of polyurethane. Although palygorskite has been modified by various strategies, such as mechanical modification, thiol grafting modification, and hydrothermal modification, there is still a lack of effective stress transfer at the interface between the modified palygorskite and the polyurethane adhesive, resulting in low bonding strength and poor toughness of the polyurethane adhesive. Therefore, how to use innovative methods to achieve effective interface transfer and dissipation is a technical problem that needs to be solved to achieve the performance enhancement of polyurethane adhesives. Summary of the invention
[0005] Technical problem to be solved: In view of the problems in the prior art that the internal rotation of the polymer chain is blocked and the chain slip is difficult due to the aggregation of polyurethane fillers, and the bonding strength of castor oil polyurethane adhesive is low, the present invention provides a polyurethane adhesive enhanced by molecular pulley effect and its preparation method and application, which can realize the preparation of environmentally friendly polyurethane adhesive with effective stress transfer, high strength and good water resistance. The castor oil polyurethane adhesive prepared by the present invention has good bonding performance and toughness. At the same time, the reinforcing modifier palygorskite and the castor oil raw material of polyurethane polyol are natural renewable materials, which are environmentally friendly and sustainable, and the raw material cost is low. The synthesized polyurethane adhesive has industrial application prospects.
[0006] Technical solution: A polyurethane adhesive enhanced by molecular pulley effect, wherein the raw materials are proportioned as follows by mass: 24-26 parts of isocyanate, 12-14 parts of castor oil, 0.2 parts of catalyst, and 1-4 parts of palygorskite-terminated polyrotaxane.
[0007] Preferably, the preparation method of the palygorskite-terminated polyrotaxane is as follows: functionalized pretreated palygorskite and pseudopolyrotaxane are stirred and reacted in anhydrous acetone, and the palygorskite-terminated polyrotaxane is obtained after filtering, washing and vacuum drying, and the mass ratio of the functionalized pretreated palygorskite to the pseudopolyrotaxane is (0.05-0.11):1.
[0008] Preferably, the preparation method of the functionalized pretreated palygorskite is as follows: the purified palygorskite is reacted with a silane coupling agent γ-aminopropyltrimethoxysilane to obtain amino palygorskite, and then the modified palygorskite is obtained by N-hydroxysuccinimide, wherein the mass ratio of palygorskite, γ-aminopropyltrimethoxysilane and N-hydroxysuccinimide is 1:0.2-0.4:0.5-1.
[0009] Preferably, the purified palygorskite is a palygorskite activated by hydrochloric acid with a pH of 6-7.
[0010] Preferably, the preparation method of the pseudopolyrotaxane is as follows: ultrasonically treat an aqueous solution of aminopropyl-terminated polydimethylsiloxane and cyclodextrin, then stir at room temperature, filter the reaction solution, and vacuum dry to obtain a pseudopolyrotaxane, wherein the weight ratio of aminopropyl-terminated polydimethylsiloxane to cyclodextrin is 1:(5.5-7).
[0011] Preferably, the catalyst is dibutyltin dilaurate or triethylamine.
[0012] Based on the above-mentioned method for preparing a polyurethane adhesive enhanced by molecular pulley effect, the steps are as follows:
[0013] (1) Add castor oil and isocyanate into a reaction kettle, stir evenly, react at 35°C-60°C for 20-40 minutes to obtain an isocyanate-terminated prepolymer, and vacuum degasify for later use (vacuum degassing is used to remove bubbles or gas in the system, which helps to improve the stability of the reaction system);
[0014] (2) Then, palygorskite-terminated polyrotaxane and a catalyst are added for cross-linking modification to obtain a polyurethane adhesive enhanced by the molecular pulley effect.
[0015] Based on the above application of the polyurethane adhesive enhanced by molecular pulley effect in the preparation of wood-based panels.
[0016] Preferably, the polyurethane adhesive is used for bonding poplar veneers, and the bonding is performed by hot pressing, with a hot pressing temperature of 120-135° C., a hot pressing pressure of 1.0-1.5 MPa, and a hot pressing time of 5-8 minutes.
[0017] Preferably, the polyurethane adhesive is used for gluing particleboard, with an application amount of 5-6 wt%, pressure, temperature and time: 1.6-3.0 MPa, 135-150°C, and 4-5 minutes.
[0018] The present invention introduces polyrotaxane into the polyurethane adhesive. The polyrotaxane can disperse the stress and dissipate energy in the system through the molecular slip motion of the main molecular ring during the stretching process. The compatibility between palygorskite and polyurethane is significantly improved through the synergistic effect of the interpenetrating network of multiple hydrogen bonds and the interface sliding structure, and the cohesion and water-resistant bonding strength of the adhesive are significantly improved.
[0019] Beneficial effects: (1) The present invention utilizes the molecular slip effect of the main molecular ring of polyrotaxane during the stretching process to overcome the problem of the existing polyurethane filler aggregation leading to the obstruction of the internal rotation of the polymer chain and the difficulty of chain slip. When the polyurethane adhesive is subjected to external force, the guest molecular chains of the polyrotaxane can effectively form crystals, hindering the expansion of cracks and significantly improving the toughness, cohesion and bonding strength of the adhesive layer.
[0020] (2) The castor oil-based polyurethane adhesive prepared by the present invention is environmentally friendly and sustainable, has low raw material cost, and is easy to apply on a practical scale. DETAILED DESCRIPTION
[0021] The present invention is described by specific embodiments, which can make it easy for those skilled in the art to understand other advantages and effects of the present invention. In addition, the present invention can also be put into practical application according to different specific implementation methods, and the details in this specification can also be appropriately adjusted according to different viewpoints and applications to ensure that it does not deviate from the original intention of the present invention. It should be noted that the following embodiments and their features can be combined with each other without causing contradictions.
[0022] In the examples of this specification, all raw materials are from common commercially available products unless otherwise specified.
[0023] The preparation method of the palygorskite-terminated polyrotaxane used in the following embodiments includes:
[0024] (1) Add 50 mL of 37% hydrochloric acid to 15 g of 9 wt% palygorskite aqueous solution and stir overnight, then centrifuge and wash until the pH is 6-7 to obtain acid-treated palygorskite. Add 0.2-0.4 g of γ-aminopropyltriethoxysilane to 10 mL of toluene solution and stir until completely dissolved, then add 1 g of acid-treated palygorskite, stir in a water bath at 80 °C for 3 hours, then filter, wash and dry.
[0025] (2) 3.5 parts of palygorskite prepared in step (1) were dissolved in 0.9 parts of succinic anhydride solution and stirred at 60°C for 2 hours under a nitrogen atmosphere. Then 1.8 parts of N-hydroxysuccinimide and 5 mL of dichloromethane were added as solvent and stirred at 40°C for 24 hours. The pretreated palygorskite was obtained by filtration, rotary evaporation and washing.
[0026] (3) Add 2 parts of aminopropyl-terminated polydimethylsiloxane to 25 parts of γ-cyclodextrin aqueous solution (including 11-14 parts of γ-cyclodextrin), and ultrasonicate the mixture in a water bath for 1 hour, and then stir at 35°C overnight. Then filter the above reaction solution and vacuum dry to obtain pseudo-polyrotaxane. Dissolve the palygorskite in step (2) in 10 mL of anhydrous acetone, stir with pseudo-polyrotaxane at 50°C for 6 hours, and then filter, centrifuge, wash and dry to obtain palygorskite-terminated polyrotaxane.
[0027] Example 1
[0028] This embodiment provides a method for preparing a high-performance castor oil polyurethane adhesive.
[0029] (1) 12 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate were stirred and mixed, reacted at 60°C for 40 minutes, and vacuum degassed three times for later use.
[0030] (2) Dissolve 1 part of palygorskite-terminated polyrotaxane in 1.5 parts of anhydrous acetone, add the mixture into step (1), and then add 0.2 parts of dibutyltin dilaurate as a catalyst. Stir evenly at room temperature to obtain a high-performance palygorskite-terminated polyrotaxane-enhanced castor oil-based polyurethane adhesive.
[0031] Example 2
[0032] (1) 12 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate were stirred and mixed, reacted at 60°C for 40 minutes, and vacuum degassed three times for later use.
[0033] (2) Dissolve 2 parts of palygorskite-terminated polyrotaxane in 1.5 parts of anhydrous acetone, add the mixture into step (1), and then add 0.2 parts of dibutyltin dilaurate as a catalyst. Stir evenly at room temperature to obtain a high-performance palygorskite-terminated polyrotaxane-enhanced castor oil-based polyurethane adhesive.
[0034] Example 3
[0035] (1) 12 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate were stirred and mixed, reacted at 60°C for 40 minutes, and vacuum degassed three times for later use.
[0036] (2) Dissolve 3 parts of palygorskite-terminated polyrotaxane in 1.5 parts of anhydrous acetone, add the mixture in step (1), and then add 0.2 parts of dibutyltin dilaurate as a catalyst. Stir evenly at room temperature to obtain a high-performance palygorskite-terminated polyrotaxane-enhanced castor oil-based polyurethane adhesive.
[0037] Example 4
[0038] (1) 12 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate were stirred and mixed, reacted at 60°C for 40 minutes, and vacuum degassed three times for later use.
[0039] (2) Dissolve 4 parts of palygorskite-terminated polyrotaxane in 1.5 parts of anhydrous acetone, add the mixture in step (1), and then add 0.2 parts of dibutyltin dilaurate as a catalyst. Stir evenly at room temperature to obtain a high-performance palygorskite-terminated polyrotaxane-enhanced castor oil-based polyurethane adhesive.
[0040] Example 5
[0041] (1) 14 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate were stirred and mixed, reacted at 60°C for 40 minutes, and vacuum degassed three times for later use.
[0042] (2) Dissolve 3 parts of palygorskite-terminated polyrotaxane in 1.5 parts of anhydrous acetone, add the mixture in step (1), and then add 0.2 parts of dibutyltin dilaurate as a catalyst. Stir evenly at room temperature to obtain a high-performance palygorskite-terminated polyrotaxane-enhanced castor oil-based polyurethane adhesive.
[0043] Example 6
[0044] (1) 12 parts of dehydrated castor oil and 26 parts of diphenylmethane diisocyanate were stirred and mixed, reacted at 60°C for 40 minutes, and vacuum degassed three times for later use.
[0045] (2) Dissolve 3 parts of palygorskite-terminated polyrotaxane in 1.5 parts of anhydrous acetone, add the mixture in step (1), and then add 0.2 parts of dibutyltin dilaurate as a catalyst. Stir evenly at room temperature to obtain a high-performance palygorskite-terminated polyrotaxane-enhanced castor oil-based polyurethane adhesive.
[0046] Comparative Example 1
[0047] 12 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate were mixed, 0.2 parts of dibutyltin dilaurate were added as a catalyst, and the mixture was reacted at 60° C. for 40 minutes to obtain a castor oil polyurethane adhesive.
[0048] Comparative Example 2
[0049] 12 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate were mixed, 3 parts of palygorskite and 0.2 parts of dibutyltin dilaurate were added as a catalyst, and the mixture was reacted at 60° C. for 40 minutes to obtain a palygorskite-reinforced castor oil-based polyurethane adhesive.
[0050] Comparative Example 3
[0051] 12 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate were mixed, 0.2 parts of dibutyltin dilaurate was added as a catalyst, and the mixture was reacted at 60°C for 40 minutes. 3 parts of palygorskite-terminated polyrotaxane were dissolved in 1.5 parts of anhydrous acetone, added to the above reactants, and stirred evenly at room temperature to obtain a modified castor oil polyurethane adhesive.
[0052] Comparative Example 4
[0053] 1 part of acid-treated palygorskite was reacted with 0.5 parts of chitosan in 50 mL of deionized water for 6 hours (80°C), and then vacuum dried at 60°C overnight to obtain chitosan-modified palygorskite. 3 parts of chitosan-modified palygorskite were added to a mixture of 12 parts of dehydrated castor oil and 24 parts of diphenylmethane diisocyanate, 0.2 parts of dibutyltin dilaurate was added as a catalyst, and the mixture was reacted at 60°C for 40 minutes to obtain a modified castor oil polyurethane adhesive.
[0054] Test example
[0055] The castor oil polyurethane adhesive prepared in the examples and comparative examples was used for bonding poplar veneers (coating amount 180 g / m 2 , hot pressing at 120°C and 1.2 MPa for 5 minutes). The bonding strength test was carried out according to the method of national standard GB / T17657-2013, with a tensile speed of 20 mm / min. The bonding strength results of the castor oil polyurethane adhesives prepared in Examples 1-6 and Comparative Examples 1-4 to wood are shown in Table 1 below.
[0056] Table 1
[0057]
[0058] As can be seen from the above table, compared with Comparative Examples 1 and 2, the dry / wet bonding strength of the embodiments is significantly improved. Mainly due to the performance limitations of castor oil itself, the unmodified castor oil polyurethane leads to insufficient cohesive strength of the adhesive, which is insufficient to provide sufficient bonding force and has low bonding strength. The introduction of palygorskite can improve the bonding performance to a certain extent, but palygorskite is prone to agglomeration and has weak compatibility with polyurethane adhesives, which greatly weakens the reinforcing effect of palygorskite. In the embodiment, palygorskite is modified to prepare palygorskite-terminated polyrotaxane, which has good plasticizing and reinforcing effects, and can improve the viscosity of the polyurethane adhesive, making it easier to apply and form a uniform adhesive layer, which is conducive to significantly improving the bonding strength. In the case of the same amount of dehydrated castor oil and isocyanate, the dry / wet bonding strength of Example 3 is the highest. Adding the same amount of palygorskite-terminated polyrotaxane, adding castor oil (Example 5) or isocyanate (Example 6) will cause the bonding strength to increase or decrease. Since the added castor oil may cause the crosslinking density in the adhesive to decrease, the looseness of the molecular structure of the adhesive is increased, thereby reducing the bonding strength. Increasing the isocyanate content within an appropriate range helps to form a tighter network structure and enhance the bonding strength of the adhesive. Compared with Example 3, changing the order of adding the catalyst (Comparative Example 3) will reduce the bonding strength of the adhesive, mainly because the catalyst added first in Comparative Example 3 causes the isocyanate and castor oil to react rapidly at a certain ratio, affecting the crosslinking reaction of the subsequent palygorskite-terminated polyrotaxane in the polyurethane adhesive. Compared with Comparative Example 4, under the same amount of modifier added, the bonding strength of Example 3 is significantly better, mainly because the introduction of polyrotaxane allows effective stress transfer at the interface between palygorskite and the polyurethane adhesive, thereby enhancing the bonding strength of the polyurethane adhesive.
[0059] The castor oil polyurethane adhesive films prepared in the examples and comparative examples were subjected to tensile tests at a tensile speed of 50 mm / min to evaluate the toughness of the adhesive. The toughness results of the castor oil polyurethane adhesives prepared in Examples 1-6 and Comparative Examples 1-4 after curing are shown in Table 2 below.
[0060] Table 2
[0061]
[0062] As shown in Table 2, the toughness of the adhesive in the embodiment is significantly higher than that in the comparative example, indicating that the toughness of the polyurethane adhesive with the addition of palygorskite-terminated polyrotaxane is significantly enhanced. This is mainly because the palygorskite-terminated polyrotaxane has a molecular pulley effect. When the adhesive is impacted by an external force, the internal polymer chain can effectively realize stress transfer through rotation and chain slippage, reduce stress concentration, and promote a significant enhancement of the toughness of the polyurethane adhesive.
[0063] The castor oil polyurethane adhesive prepared in the examples and comparative examples was applied to the preparation of particleboard (sizing amount 6%, pressure, temperature, time: 1.6 MPa, 135°C, 5 minutes), and the internal bonding strength of the particleboard was tested (vertical tensile speed was 2 mm / min). The internal bonding strength of the castor oil polyurethane adhesive prepared in Examples 1-6 and Comparative Examples 1-4 on the particleboard is shown in Table 3.
[0064] Table 3
[0065]
[0066] The results in Table 3 show that compared with the comparative example, the internal bonding strength of the particleboard bonded with the palygorskite-terminated polyrotaxane-modified castor oil polyurethane adhesive is significantly higher. When the amount of dehydrated castor oil and isocyanate is the same, the internal bonding strength of Examples 2 and 3 is relatively high, and the addition of more palygorskite-terminated polyrotaxanes causes the internal bonding strength of the adhesive to decrease instead (Example 4). This is mainly because excessive addition of palygorskite-terminated polyrotaxanes may cause the adhesion performance of the adhesive to weaken, thereby affecting the bonding strength between the adhesive and the particleboard. Therefore, it is important to balance the selection of an appropriate amount of palygorskite-terminated polyrotaxanes to maintain the performance of the adhesive and effectively improve the internal bonding strength of the particleboard. When the same amount of palygorskite-terminated polyrotaxanes is added, the increase in the isocyanate content leads to a slight increase in the internal bonding strength of the particleboard (Example 6), because the high reactivity of the isocyanate group will promote the bonding of the polyurethane adhesive to the wood particles to a certain extent.
[0067] Although the general concept, specific embodiments and experiments of the present invention are described in detail above, it is obvious to a person skilled in the art that some modifications or improvements are made on the basis of the present invention. Therefore, these modifications or improvements made without changing the original intention of the present invention are considered to be within the scope of protection of the present invention.
Claims
1. A polyurethane adhesive enhanced by molecular pulley effect, characterized in that: The raw materials are proportioned as follows by weight: 24-26 parts of isocyanate, 12-14 parts of castor oil, 0.2 parts of catalyst, and 1-4 parts of palygorskite-terminated polyrotaxane.
2. The polyurethane adhesive enhanced by molecular pulley effect according to claim 1, characterized in that: The preparation method of the palygorskite-terminated polyrotaxane is as follows: functionalized pretreated palygorskite and pseudopolyrotaxane are stirred and reacted in anhydrous acetone, and the palygorskite-terminated polyrotaxane is obtained after filtering, washing and vacuum drying, wherein the mass ratio of the functionalized pretreated palygorskite to the pseudopolyrotaxane is (0.05-0.11):
1.
3. The polyurethane adhesive enhanced by molecular pulley effect according to claim 2, characterized in that: The preparation method of the functionalized pretreated palygorskite is as follows: the purified palygorskite is reacted with a silane coupling agent γ-aminopropyltrimethoxysilane to obtain amino palygorskite, and then the modified palygorskite is obtained by N-hydroxysuccinimide, wherein the mass ratio of palygorskite, γ-aminopropyltrimethoxysilane and N-hydroxysuccinimide is 1:0.2-0.4:0.5-1.
4. The polyurethane adhesive enhanced by molecular pulley effect according to claim 3, characterized in that: The purified palygorskite is a palygorskite activated with hydrochloric acid and having a pH value of 6-7.
5. The polyurethane adhesive enhanced by molecular pulley effect according to claim 2, characterized in that: The preparation method of the pseudopolyrotaxane is as follows: ultrasonically treat an aqueous solution of aminopropyl-terminated polydimethylsiloxane and cyclodextrin, then stir at room temperature, filter the solution after the reaction, and vacuum dry to obtain a pseudopolyrotaxane, wherein the weight ratio of aminopropyl-terminated polydimethylsiloxane to cyclodextrin is 1:(5.5-7).
6. The polyurethane adhesive enhanced by molecular pulley effect according to claim 1, characterized in that: The catalyst is dibutyltin dilaurate or triethylamine.
7. A method for preparing a polyurethane adhesive enhanced by molecular pulley effect according to claim 1, characterized in that: Here are the steps: (1) Add castor oil and isocyanate into a reaction kettle, stir evenly, react at 35°C-60°C for 20-40 min to obtain an isocyanate-terminated prepolymer, and vacuum degas for later use; (2) Then, palygorskite-terminated polyrotaxane and a catalyst are added for cross-linking modification to obtain a polyurethane adhesive enhanced by the molecular pulley effect.
8. Use of the polyurethane adhesive enhanced by molecular pulley effect according to claim 1 in the preparation of wood-based panels.
9. The use according to claim 8, characterized in that: The polyurethane adhesive is used for bonding poplar veneers, and the bonding adopts a hot pressing process, the hot pressing temperature is 120-135° C., the hot pressing pressure is 1.0-1.5 MPa, and the hot pressing time is 5-8 minutes.
10. The use according to claim 8, characterized in that: The polyurethane adhesive is used for gluing particleboard, with an application amount of 5-6 wt%, pressure, temperature and time: 1.6-3.0 MPa, 135-150°C, and 4-5 minutes.
Citation Information
Patent Citations
Pressure-sensitive adhesive composition and pressure-sensitive adhesive sheet making use of the same
CN101405361A
Preparation method of attapulgite / aqueous polyurethane compound binder
CN101768418A
Viscose, high-performance artificial turf and preparation method thereof
CN101831265A
Adhesive composition and adhesive sheet
CN102245728A
Polyurethane two-component or multi-component systems having a latent thickening tendency
CN106459337A
Cited By
High-flame-retardant cold-resistant dynamic-fatigue-resistant composite cable and preparation method thereof
CN120424464A