Sealant as well as preparation method and application thereof
By using a combination of calcium carbonate and oligomer crosslinking agent in the sealant, the crosslinking density and mechanical properties are improved, and the mechanical properties retention problem of silicone sealant in high temperature and high humidity environment is solved, and the photovoltaic modules are improved load-bearing capacity and service life.
Patent Information
- Application Number
- CN202411184921.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
The existing silicone sealant has poor mechanical properties retention rate in high temperature and high humidity environments, which cannot meet the demand for photovoltaic module bearing capacity.
A sealant including base glue, calcium carbonate, white carbon black, crosslinking agent, coupling agent and catalyst is used. The crosslinking agent is a mixture of the first crosslinking agent and the second crosslinking agent to increase the crosslinking density and use modifications. Nano-nano calcium carbonate and oligomer crosslinking agents improve mechanical properties.
The initial tensile strength of the sealant is not less than 2.8MPa, and the tensile strength after DH1000 is not less than 2.20MPa, which significantly improves the bonding ability and service life of the component laminate and the profile.
Smart Images

Figure BDA0005013244760000161 
Figure BDA0005013244760000171
Abstract
Description
Technical Field
[0001] The present application relates to the field of packaging technology, and specifically provides a sealant and a preparation method and application thereof. Background Art
[0002] Solar photovoltaic power generation is a technology that uses the photovoltaic effect of semiconductor interfaces to directly convert light energy into electrical energy. As the sustainable development of human economy and society places higher and higher demands on energy and environmental protection, this power generation method has received more and more attention. The core component of solar photovoltaic power generation is the solar cell. Due to the defects of the solar cell itself such as thinness, brittleness, and easy oxidation, it is easy to cause permanent damage when exposed to natural environments such as air and rain. Therefore, in order to realize the industrial application of solar power generation, it is required to perform protective sealing to form solar photovoltaic modules. Silicone sealant is particularly suitable for protective sealing of solar cell modules due to its superior high and low temperature resistance, weather resistance, good adhesion and sealing properties.
[0003] In recent years, with the development of photovoltaic modules, the size of the modules has become larger and larger, and the requirements for the bearing capacity of the modules have become higher and higher. Therefore, the performance requirements for various materials of the modules have also increased accordingly, especially the photovoltaic glue used for sealing the module frame, which plays the role of a link between the laminate and the frame. Once the load-bearing force of the module is too large, it is easy to cause the sealant colloid to be torn, resulting in the phenomenon of the laminate falling off the frame, and even causing the module to fail and become unusable. In the photovoltaic industry, the bearing capacity of the module is evaluated by load testing (static mechanical load). The larger the module size, the greater the deformation of the module under the load test state, which greatly increases the risk of the laminate falling off the frame. Therefore, a higher strength sealant is needed to compensate for the risk caused by the excessive deformation of the module. In particular, when simulating the service life of the module, the module will be subjected to high temperature and high humidity (DH) environmental testing to evaluate the long-term reliability. Therefore, the requirements for the mechanical properties of the sealant after high temperature and high humidity are also getting higher and higher.
[0004] Existing technologies all start with silicone oil or coupling agents to increase reactive functional groups to increase cross-linking density, thereby improving colloid strength. Although it can reach 2.5MPa initially, there is no limit on the mechanical properties after environmental aging. Therefore, it cannot guarantee that the component load requirements can still be met after high temperature and high humidity (DH) environmental testing.
[0005] Accordingly, this field requires a new technical solution to solve the above technical problems. Summary of the invention
[0006] The present application aims to solve the above technical problem, that is, to solve the problem of poor retention rate of mechanical properties of existing silicone sealants.
[0007] In a first aspect, the present application provides a sealant, comprising a base glue, calcium carbonate, white carbon black, a cross-linking agent, a coupling agent and a catalyst, wherein the cross-linking agent is a mixture of a first cross-linking agent and a second cross-linking agent, the first cross-linking agent comprises at least one of methyl tributylacetoximine silane, vinyl tributylacetoximine silane and tetrabutyl tributylacetoximine silane, and the second cross-linking agent is a butanone tributylacetoximine silane oligomer.
[0008] In the preferred technical scheme of the above-mentioned sealant, the sealant includes the following components by mass: 30-60 parts of base glue, 30-60 parts of calcium carbonate, 0.5-3 parts of white carbon black, 2-5 parts of cross-linking agent, 0.3-3 parts of coupling agent, and 0.05-0.2 parts of catalyst.
[0009] In the preferred technical solution of the above sealant, the mass ratio of the first cross-linking agent to the second cross-linking agent is 1:(0.3-1).
[0010] In the preferred technical solution of the above sealant, the calcium carbonate is modified nano calcium carbonate, wherein the specific surface area of the modified nano calcium carbonate is 27 to 32 m 2 / g, the pH value of the modified nano calcium carbonate is 7.5-8.5; and / or, the white carbon black includes fumed white carbon black, and the specific surface area of the fumed white carbon black is 150-250m 2 / g.
[0011] In the preferred technical scheme of the above-mentioned sealant, the base glue is a compound mixture of high-viscosity terminal hydroxyl polydimethylsiloxane and low-viscosity terminal hydroxyl polydimethylsiloxane, wherein the viscosity of the high-viscosity terminal hydroxyl polydimethylsiloxane is 10000-80000 mPa·s, and the viscosity of the low-viscosity terminal hydroxyl polydimethylsiloxane is 1000-5000 mPa·s.
[0012] In the preferred technical solution of the above sealant, the mass ratio of the high-viscosity terminal hydroxyl polydimethylsiloxane to the low-viscosity terminal hydroxyl polydimethylsiloxane is 1:(0.1-0.4).
[0013] In the preferred technical scheme of the above-mentioned sealant, the coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, and amino coupling agent oligomers; and / or the catalyst is dibutyltin dilaurate, stannous octoate or dibutyltin diceneodecanoate.
[0014] In the preferred technical solution of the above sealant, the initial tensile strength of the sealant is not less than 2.8 MPa, and the tensile strength after DH1000 is not less than 2.20 MPa.
[0015] In a second aspect, the present application provides a method for preparing a sealant, which is used to prepare the above-mentioned sealant, and the method for preparing the sealant comprises the following steps: mixing the base glue, the calcium carbonate, and the white carbon black to prepare a base material; mixing the base material with the cross-linking agent to prepare an intermediate; mixing the intermediate, the coupling agent, and the catalyst to prepare the sealant.
[0016] In the preferred technical scheme of the preparation method of the above-mentioned sealant, at least one of the conditions (1) to (3) is satisfied: (1) in the step of preparing the base material, the mixing temperature is 100 to 120°C, the vacuum degree is ≤-0.095 MPa, and the mixing is performed with stirring for 2 to 4 hours; (2) in the step of preparing the intermediate, the mixing is performed with stirring for 15 min to 30 min; (3) in the step of preparing the sealant, the mixing is performed with stirring for 15 min to 30 min, and the vacuum degree is ≤-0.095 MPa.
[0017] In a third aspect, the present application provides the use of the above-mentioned sealant in preparing a packaging structure.
[0018] In a fourth aspect, the present application provides a photovoltaic module, wherein the photovoltaic module includes a packaging structure made of the above-mentioned sealant.
[0019] Compared with the prior art, the sealant of the present application has the following technical effects:
[0020] 1. The sealant of the present application increases the reactive functional groups of the cross-linking agent by adding a second cross-linking agent of the oligomer, effectively improving the cross-linking density, thereby improving the initial mechanical properties; due to the increased cross-linking density, the mechanical attenuation caused by the hydrolysis reaction of the chemical bonds inside the colloid can be effectively alleviated, thereby improving the retention rate of the mechanical properties of the colloid. The sealant of the present application greatly improves its mechanical properties while ensuring the sizing process. Its initial tensile strength is not less than 2.8MPa, and its tensile strength after DH1000 is not less than 2.20MPa, thereby improving the bonding ability of the component laminate and the profile, ensuring the bearing capacity of the component, and extending the service life of the component, which is of great significance for the development and promotion of photovoltaic new energy products.
[0021] 2. The calcium carbonate used in this application has a specific surface area of 27 to 32 m 2 / g and pH value of 7.5 to 8.5, the modified nano calcium carbonate, by utilizing the larger specific surface area of the modified nano calcium carbonate, greatly enhances the binding force between the modified nano calcium carbonate and the base glue (hydroxyl-terminated polydimethylsiloxane), and improves the initial mechanical properties of the sealant. In addition, since the pH value of the modified nano calcium carbonate is neutral, during the aging process of the colloid, it can effectively avoid the residual hydroxyl groups in the reinforcing filler from participating in the hydrolysis reaction of the chemical bonds inside the colloid, thereby improving the retention rate of the mechanical properties of the colloid. And when used in conjunction with the second cross-linking agent of the oligomer, due to the increase in cross-linking density, it can effectively alleviate the mechanical attenuation caused by the hydrolysis reaction of the chemical bonds inside the colloid, thereby further improving the retention rate of the mechanical properties of the colloid, greatly improving the load-bearing capacity of the component, and ensuring the long-term reliability of the component.
[0022] 3. The base glue of the present application is a compound mixture of high-viscosity terminal hydroxyl polydimethylsiloxane and low-viscosity terminal hydroxyl polydimethylsiloxane. By adding a certain proportion of low-viscosity terminal hydroxyl polydimethylsiloxane, the sealant can be kept within a certain viscosity range, thereby reducing the difficulty of extrusion of the sealant during production and use, making it easier to use. DETAILED DESCRIPTION
[0023] The preferred embodiments of the present application are described below. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present application and are not intended to limit the protection scope of the present application.
[0024] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0025] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0026] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0027] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0028] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0029] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0030] The experimental methods in the following examples are conventional methods unless otherwise specified, and the materials, reagents, etc. used in the following examples are commercially available unless otherwise specified.
[0031] Although the initial tensile strength of the improved silicone sealant in the prior art mentioned in the background art can reach 2.5 MPa, it cannot continue to maintain excellent mechanical properties after aging; that is, the mechanical property retention rate of the existing silicone sealant is poor.
[0032] The sealant of the present application is improved on the basis of the existing photovoltaic sealant. By adding a second cross-linking agent of an oligomer, the reactive functional group of the cross-linking agent is increased, and the cross-linking density is effectively improved, thereby improving the initial mechanical properties of the sealant. Moreover, due to the increase in cross-linking density, the mechanical attenuation caused by the hydrolysis reaction of the chemical bonds inside the colloid can be effectively alleviated, thereby improving the retention rate of the mechanical properties of the colloid. In addition, the sealant of the present application greatly improves the initial mechanical properties under the premise of ensuring the sizing process. Its initial tensile strength is not less than 2.8MPa, and the tensile strength after DH1000 is not less than 2.20MPa. It has an excellent mechanical property retention rate, thereby improving the bonding ability of the component laminate and the profile, ensuring the bearing capacity of the component, and extending the service life of the component, which is of great significance for the development and promotion of photovoltaic new energy products.
[0033] Specifically, the present application provides a sealant in a first aspect, which includes a base glue, calcium carbonate, white carbon black, a cross-linking agent, a coupling agent and a catalyst, wherein the cross-linking agent is a mixture of a first cross-linking agent and a second cross-linking agent, the first cross-linking agent includes at least one of methyl tributylacetoximine silane, vinyl tributylacetoximine silane, and tetrabutyl tributylacetoximine silane, and the second cross-linking agent is a butanone tributylacetoximine silane oligomer.
[0034] It should be noted that the polymerization degree of the butanone oxime silane oligomer in the present application is 4 to 10 and the molecular weight is not higher than 2,000.
[0035] The sealant of the present application is improved on the basis of the existing photovoltaic sealant, so that the cross-linking agent is a mixture of a first cross-linking agent and a second cross-linking agent. By adding a second cross-linking agent of butanone oxime silane oligomer, the reactive functional groups of the cross-linking agent are increased, and the cross-linking density is effectively improved, thereby improving the initial mechanical properties of the sealant. Due to the increase in the cross-linking density, the mechanical attenuation caused by the hydrolysis reaction of the chemical bonds inside the colloid can be effectively alleviated, thereby improving the retention rate of the mechanical properties of the colloid.
[0036] The sealant of the present application greatly improves its initial mechanical properties while ensuring the gluing process. Its initial tensile strength is not less than 2.8MPa, and the tensile strength after DH1000 is not less than 2.20MPa, thereby improving the bonding ability between the component laminates and the profiles, ensuring the bearing capacity of the components, and extending the service life of the components, which is of great significance for the development and promotion of photovoltaic new energy products.
[0037] In some preferred embodiments, the sealant of the present application includes the following components by mass: 30-60 parts of base glue, 30-60 parts of calcium carbonate, 0.5-3 parts of white carbon black, 2-5 parts of cross-linking agent, 0.3-3 parts of coupling agent, and 0.05-0.2 parts of catalyst.
[0038] In specific use, the mass fraction of the base glue is controlled to be 30 to 60 parts, so as to obtain a sealant with better performance. Optionally, the mass fraction of the base glue is 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts or any value within the range composed of the above values.
[0039] In specific use, the mass fraction of calcium carbonate is controlled to be 30 to 60 parts, so as to obtain a sealant with better performance. Optionally, the mass fraction of calcium carbonate is 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts or any value within the range composed of the above values.
[0040] In specific use, the mass fraction of white carbon black is controlled to be 0.5 to 3 parts, so as to obtain a sealant with better performance. Optionally, the mass fraction of white carbon black is 0.5 parts, 0.8 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts or any value within the range composed of the above values.
[0041] In specific use, the mass fraction of the crosslinking agent is controlled to be 2 to 5 parts, so as to obtain a sealant with better performance. Optionally, the mass fraction of the crosslinking agent is 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts or any value within the range of the above values.
[0042] In specific use, the mass fraction of the coupling agent is controlled to be 0.3 to 3 parts, so as to obtain a sealant with better performance. Optionally, the mass fraction of the coupling agent is 0.3 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts or any value within the range of the above values.
[0043] In specific use, the mass fraction of the catalyst is controlled to be 0.05-0.2 parts, and a sealant with better performance can be obtained. Optionally, the mass fraction of the catalyst is 0.05 parts, 0.08 parts, 0.1 parts, 0.12 parts, 0.15 parts, 0.18 parts, 0.2 parts or any value within the range composed of the above values.
[0044] In some preferred embodiments, the mass ratio of the first cross-linking agent to the second cross-linking agent is 1:(0.3-1).
[0045] By controlling the mass ratio of the first cross-linking agent to the second cross-linking agent to be 1:(0.3-1), a sealant with good mechanical properties can be prepared.
[0046] In practical applications, the mass ratio of the first cross-linking agent to the second cross-linking agent can be 1:0.3, 1:0.4, 1:0.5, 1:0.8 or 1:1.
[0047] In some preferred embodiments, the calcium carbonate is modified nano calcium carbonate, wherein the specific surface area of the modified nano calcium carbonate is 27 to 32 m 2 / g, the pH value of modified nano calcium carbonate is 7.5-8.5.
[0048] The calcium carbonate used in this application has a specific surface area of 27 to 32 m 2 / g and pH value of 7.5 to 8.5, the modified nano calcium carbonate greatly enhances the binding force between the modified nano calcium carbonate and the base glue (hydroxyl-terminated polydimethylsiloxane) by utilizing the larger specific surface area of the modified nano calcium carbonate, and improves the initial mechanical properties of the sealant. In addition, since the pH value of the modified nano calcium carbonate is neutral, during the aging process of the colloid, it can effectively avoid the residual hydroxyl groups in the reinforcing filler from participating in the hydrolysis reaction of the chemical bonds inside the colloid, and improve the retention rate of the mechanical properties of the colloid. As a result, the sealant has a good mechanical property retention rate and improves the service life of the sealant.
[0049] It should be noted that the present application does not impose any restrictions on the specific modification method of modified nano-calcium carbonate. As long as the final modified nano-calcium carbonate meets the specific surface area of 27 to 32 m 2 / g and the pH value is 7.5-8.5. In practical applications, those skilled in the art can select the corresponding modification method to modify calcium carbonate according to actual needs to obtain the nano calcium carbonate, or directly purchase calcium carbonate with a specific surface area of 27-32 m 2 / g and a finished modified nano calcium carbonate with a pH value of 7.5 to 8.5.
[0050] In some preferred embodiments, the white carbon black includes fumed white carbon black, and the specific surface area of the fumed white carbon black is 150 to 250 m 2 / g.
[0051] The white carbon black used in this application has a specific surface area of 150 to 250 m 2 / g of fumed silica can ensure the excellent mechanical properties of the prepared sealant.
[0052] In some preferred embodiments, the base glue is a compound mixture of high-viscosity terminal hydroxyl polydimethylsiloxane and low-viscosity terminal hydroxyl polydimethylsiloxane, wherein the viscosity of the high-viscosity terminal hydroxyl polydimethylsiloxane is 10000-80000 mPa·s, and the viscosity of the low-viscosity terminal hydroxyl polydimethylsiloxane is 1000-5000 mPa·s.
[0053] The base glue of the present application is a compound mixture of high-viscosity terminal hydroxyl polydimethylsiloxane and low-viscosity terminal hydroxyl polydimethylsiloxane. By adding a certain proportion of low-viscosity terminal hydroxyl polydimethylsiloxane, the sealant can be kept within a certain viscosity range, has good extrusion performance, and is convenient for the sizing process of the subsequent production line.
[0054] In some preferred embodiments, the mass ratio of the high viscosity terminal hydroxyl polydimethylsiloxane to the low viscosity terminal hydroxyl polydimethylsiloxane is 1:(0.1-0.4).
[0055] By controlling the mass ratio of high-viscosity terminal hydroxyl polydimethylsiloxane to low-viscosity terminal hydroxyl polydimethylsiloxane to 1:(0.1-0.4), a sealant that is easier to extrude and use can be prepared.
[0056] In practical applications, the mass ratio of the high viscosity hydroxyl-terminated polydimethylsiloxane to the low viscosity hydroxyl-terminated polydimethylsiloxane may be 1:0.1, 1:0.2, 1:0.3, 1:0.35 or 1:0.4.
[0057] Optionally, the coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, and amino coupling agent oligomer.
[0058] Optionally, the catalyst is dibutyltin dilaurate, stannous octoate or dibutyltin diceneodecanoate.
[0059] Preferably, the initial tensile strength of the sealant is not less than 2.8 MPa, and the tensile strength after DH1000 is not less than 2.20 MPa.
[0060] The present application provides a method for preparing a sealant in a second aspect, which is used to prepare the sealant provided in the first aspect. The method comprises the following steps S110 to S130:
[0061] S110: Mixing base rubber, calcium carbonate and white carbon black to prepare a base material.
[0062] In some embodiments, in step S110, the mixing temperature is 100-120°C, the vacuum degree is ≤-0.095MPa, and stirring is performed during mixing for a stirring time of 2-4h.
[0063] S120: Mixing the base material and the cross-linking agent to prepare an intermediate.
[0064] In some embodiments, in step S120, stirring is performed during mixing and the stirring time is 15 min to 30 min.
[0065] S130: Mixing the intermediate, the coupling agent and the catalyst to prepare a sealant.
[0066] In some embodiments, in step S130, stirring is performed during mixing and the stirring time is 15 min to 30 min, and the vacuum degree is ≤-0.095 MPa.
[0067] The preparation method of the sealant is simple in process and low in cost, and the prepared sealant has both good mechanical properties and mechanical property retention rate, and is suitable for preparing packaging structures, especially for packaging of photovoltaic modules.
[0068] The present application provides, in a third aspect, the use of the sealant provided in the first aspect of the present application in preparing a packaging structure.
[0069] The present application provides a photovoltaic module in a fourth aspect, and the photovoltaic module includes a packaging structure made of the sealant provided in the first aspect.
[0070] The photovoltaic module includes a packaging structure made of the sealant, and the photovoltaic module has good sealing performance and better long-term reliability.
[0071] In some embodiments, the photovoltaic module also includes a solar module. Specifically, the solar module includes a perovskite solar module, a crystalline silicon solar module or an amorphous silicon solar module.
[0072] In order to make the purpose, technical solutions and advantages of the present application more concise and clear, the present application is described with the following specific embodiments, but the present application is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present application and can be used to describe the present application, and cannot be understood as limiting the scope of the present application. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
[0073] In order to better illustrate the present application, the present application content is further described below in conjunction with the embodiments. The following are specific embodiments. Unless otherwise specified, in the following embodiments, the parts refer to the parts by mass. Wherein, the butanone oxime-based silane oligomer in the embodiments of the present application is an existing product purchased on the market.
[0074] Example 1
[0075] In this embodiment, the components of the sealant include: 47 parts of base glue, 50 parts of calcium carbonate, 1.2 parts of white carbon black, 4 parts of cross-linking agent, 1.5 parts of coupling agent, and 0.08 parts of catalyst.
[0076] The base glue includes 37 parts of high-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 50000mPa·s and 10 parts of low-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 1000mPa·s; calcium carbonate has a specific surface area of 26m 2 / g, modified nano calcium carbonate with a pH value of 8.0, and white carbon black with a specific surface area of 250m 2 / g of fumed silica, the crosslinking agent is 0.5 parts of methyl tributylacetoximate silane, 1.5 parts of vinyl tributylacetoximate silane and 2.0 parts of butanone tributylacetoximate silane oligomer, the coupling agent is 1 part of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 0.5 parts of amino coupling agent oligomer, and the catalyst is dibutyltin dilaurate.
[0077] The preparation method of the sealant of this embodiment comprises the following steps:
[0078] (1) Add the base rubber and filler into a kneader in sequence, stir for 4 hours at a temperature of 110° C. and a vacuum degree of no higher than −0.095 MPa, and cool to obtain a base material.
[0079] (2) Add the base material and cross-linking agent into a planetary mixer and stir to react for 30 minutes.
[0080] (3) Add a coupling agent and a catalyst into the planetary mixer, evacuate and stir until the vacuum degree reaches -0.095 MPa, and continue stirring for 30 minutes to obtain the silicone sealant.
[0081] Example 2
[0082] The preparation method of the sealant of this embodiment is the same as that of Embodiment 1. The components of the sealant of this embodiment include: 30 parts of base glue, 30 parts of calcium carbonate, 0.5 parts of white carbon black, 2 parts of cross-linking agent, 0.3 parts of coupling agent, and 0.05 parts of catalyst.
[0083] The base glue includes 25 parts of high-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 50000mPa·s and 5 parts of low-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 1000mPa·s; calcium carbonate has a specific surface area of 26m 2 / g, modified nano calcium carbonate with a pH value of 8, and white carbon black with a specific surface area of 250m 2 / g of fumed silica, the crosslinking agent is 0.5 parts of methyl tributylacetoximate silane, 0.5 parts of vinyl tributylacetoximate silane and 1.0 parts of butanone tributylacetoximate silane oligomer, the coupling agent is 0.2 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 0.1 parts of amino coupling agent oligomer, and the catalyst is dibutyltin dilaurate.
[0084] Example 3
[0085] The preparation method of the sealant of this embodiment is the same as that of Embodiment 1. The components of the sealant of this embodiment include: 60 parts of base glue, 60 parts of calcium carbonate, 3 parts of white carbon black, 5 parts of cross-linking agent, 3 parts of coupling agent, and 0.2 parts of catalyst.
[0086] The base glue includes 50 parts of high-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 50000 mPa·s and 10 parts of low-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 1000 mPa·s; calcium carbonate has a specific surface area of 26 m 2 / g, modified nano calcium carbonate with a pH value of 8, and white carbon black with a specific surface area of 250m 2 / g of fumed silica, the crosslinking agent is 1.5 parts of methyl tributylacetoximate silane, 1 part of vinyl tributylacetoximate silane and 2.5 parts of butanone tributylacetoximate silane oligomer, the coupling agent is 2 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 1 part of amino coupling agent oligomer, and the catalyst is dibutyltin dilaurate.
[0087] Example 4
[0088] The preparation method of the sealant of this embodiment is the same as that of Example 1. The components of the sealant of this embodiment are different from those of Example 1 only in that the cross-linking agent is 4 parts, wherein the cross-linking agent is 1.5 parts of methyl tributylacetoximine silane, 1.3 parts of vinyl tributylacetoximine silane and 1.2 parts of butanone tributylacetoximine silane oligomer.
[0089] Example 5
[0090] The preparation method of the sealant of this embodiment is the same as that of Example 1. The components of the sealant of this embodiment are different from those of Example 1 only in that the cross-linking agent is 4 parts, wherein the cross-linking agent is 1.2 parts of methyl tributylacetoximine silane, 1 part of vinyl tributylacetoximine silane and 1.8 parts of butanone tributylacetoximine silane oligomer.
[0091] Example 6
[0092] The preparation method of the sealant of this embodiment is the same as that of embodiment 1. The components of the sealant of this embodiment are different from those of embodiment 1 in that: calcium carbonate has a specific surface area of 30 m 2 / g, modified nano calcium carbonate with a pH value of 7.5.
[0093] Example 7
[0094] The preparation method of the sealant of this embodiment is the same as that of embodiment 1. The components of the sealant of this embodiment are different from those of embodiment 1 in that: calcium carbonate has a specific surface area of 29 m 2 / g, modified nano calcium carbonate with a pH value of 8.5.
[0095] Example 8
[0096] The preparation method of the sealant of this embodiment is the same as that of Embodiment 1. The components of the sealant of this embodiment include: 45 parts of base glue, 54 parts of calcium carbonate, 0.8 parts of white carbon black, 3.5 parts of cross-linking agent, 1.2 parts of coupling agent, and 0.12 parts of catalyst.
[0097] The base glue includes 40 parts of high-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 30000mPa·s and 5 parts of low-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 3000mPa·s; calcium carbonate has a specific surface area of 30m 2 / g, modified nano calcium carbonate with a pH value of 7.8, and white carbon black with a specific surface area of 150m 2 / g of fumed silica, the crosslinking agent is 1 part of tetrabutyl ketone oxime silane, 1.5 parts of vinyl tributyketone oxime silane and 1 part of butanone oxime silane oligomer, the coupling agent is 0.7 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 0.5 parts of amino coupling agent oligomer, and the catalyst is dibutyltin dilaurate.
[0098] Example 9
[0099] The preparation method of the sealant of this embodiment is the same as that of Example 1. The components of the sealant of this embodiment include: 50 parts of base glue, 48 parts of calcium carbonate, 1 part of white carbon black, 3.7 parts of cross-linking agent, 1 part of coupling agent, and 0.1 part of catalyst.
[0100] The base glue includes 42 parts of high-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 20000 mPa·s and 8 parts of low-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 2000 mPa·s; calcium carbonate has a specific surface area of 32 m 2 / g, modified nano calcium carbonate with a pH value of 8.3, and white carbon black with a specific surface area of 250m 2 / g of fumed silica, the crosslinking agent is 1.7 parts of tetrabutyl ketone oxime silane, 1 part of vinyl tributyketone oxime silane and 2 parts of butanone oxime silane oligomer, the coupling agent is 0.5 parts of γ-aminopropyltriethoxysilane and 0.5 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, and the catalyst is dibutyltin dilaurate.
[0101] Example 10
[0102] The preparation method of the sealant of this embodiment is the same as that of Example 1. The only difference between this embodiment and Example 1 is that the ratio of low-viscosity terminal hydroxyl polydimethylsiloxane to high-viscosity terminal hydroxyl polydimethylsiloxane in the base glue is different. Specifically, the base glue includes 42.7 parts of high-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 50000mPa·s and 4.3 parts of low-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 1000mPa·s.
[0103] Embodiment 11
[0104] The preparation method of the sealant of this embodiment is the same as that of Example 1. The only difference between this embodiment and Example 1 is that the ratio of low-viscosity terminal hydroxyl polydimethylsiloxane to high-viscosity terminal hydroxyl polydimethylsiloxane in the base glue is different. Specifically, the base glue includes 33.6 parts of high-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 50000mPa·s and 13.4 parts of low-viscosity terminal hydroxyl polydimethylsiloxane with a viscosity of 1000mPa·s.
[0105] Comparative Example 1
[0106] The preparation method of the sealant in this comparative example is the same as that in Example 1. The difference between this comparative example and Example 1 is that: the calcium carbonate has a specific surface area of 20 m 2 / g, ordinary nano calcium carbonate with a pH value of 9.5.
[0107] Comparative Example 2
[0108] The preparation method of the sealant in this comparative example is the same as that in Example 1. The difference between this comparative example and Example 1 is that the crosslinking agent is 4 parts, wherein the crosslinking agent is 2.5 parts of methyltributylacetonato silane and 1.5 parts of vinyltributylacetonato silane.
[0109] Comparative Example 3
[0110] The preparation method of the sealant in this comparative example is the same as that in Example 1. The difference between this comparative example and Example 1 is that the crosslinking agent is 2 parts, wherein the crosslinking agent is 0.5 parts of methyltributylacetonato silane and 1.5 parts of vinyltributylacetonato silane.
[0111] Preparation of the packaging structure, the sealants of Examples 1 to 11 and Comparative Examples 1 to 3 were cured at 25°C and 50% RH for 7 days, and the packaging structures were prepared as test samples and the various properties of each test sample were tested, and the test results are shown in Table 1. Among them, the packaging structure uses a large-format component with a size of 2382mm*1303mm.
[0112] Specifically, the test items include initial load test pass rate, DH1000 post-load test pass rate, hardness, shear strength, initial tensile strength, and tensile strength after DH1000.
[0113] The load test method is as follows: first apply a front load of 5400Pa for 1h, then apply a back load of 2400Pa for 1h. This is one cycle. A total of 3 cycles are tested to observe the situation of the components falling out of the frame. At the same time, 5 components are arranged for each test to calculate the test pass rate.
[0114] Pass GB / T 531 to test the hardness of the packaging structure.
[0115] Passed GB / T 7124 test for shear strength of package structure (tested with anodized aluminum profile).
[0116] The initial tensile strength of the packaging structure and the tensile strength after DH1000 were tested according to GB / T 528, and the mechanical retention rate after DH1000 was calculated.
[0117] Table 1 Mechanical properties of the packaging structures obtained in the embodiments and comparative examples
[0118] Compare the data of the embodiment with the comparative example:
[0119] 1. It can be seen from the experimental data of Examples 1 to 11 that the sealant of the present application has good mechanical properties, its initial tensile strength can reach more than 2.8 MPa, the tensile strength after DH1000 is not less than 2.2 MPa, the mechanical retention rate after DH1000 is not less than 80%, and the component load pass rate before and after environmental aging is 100%, which greatly improves the bearing capacity of the component, thereby extending the service life of the component, and the gluing process is simple, it only needs to be used like ordinary photovoltaic sealants, and does not affect the production line process at all, which has important practical significance for the development and promotion of photovoltaic new energy products.
[0120] 2. It can be seen from Examples 1, 4 and 5 that when the mass ratio of the first cross-linking agent to the second cross-linking agent is 1:(0.3-1), the sealant obtained has better performance. Therefore, it is preferred that the mass ratio of the first cross-linking agent to the second cross-linking agent is 1:(0.3-1).
[0121] 3. Comparing Example 1 with Comparative Example 1, the data of hardness, shear strength, initial tensile strength, tensile strength after DH1000, mechanical retention rate after DH1000 and load test pass rate after DH1000 of Example 1 are all higher than those of Comparative Example 1. It can be seen that the specific surface area of 27 to 32 m 2 / g and a pH value of 7.5 to 8.5 can effectively improve the initial mechanical properties of the sealant and can improve the mechanical property retention rate of the sealant, thereby making the prepared sealant have a longer service life and be resistant to aging.
[0122] 4. Comparing Example 1 with Comparative Examples 2 and 3, the shear strength, initial tensile strength, tensile strength after DH1000, mechanical retention rate after DH1000 and pass rate of the load test after DH1000 of Example 1 are all higher than those of Comparative Examples 2 and 3. It can be seen that only using the first cross-linking agent to prepare the sealant (without adding the second cross-linking agent) cannot effectively improve the initial tensile strength, tensile strength after DH1000, mechanical retention rate after DH1000 and pass rate of the load test after DH1000 of the sealant. Therefore, only when the cross-linking agent is a mixture of the first cross-linking agent and the second cross-linking agent, can the initial mechanical properties of the sealant be effectively improved, and the mechanical attenuation can be slowed down to improve the retention rate of the mechanical properties.
[0123] In summary, the sealant of the present application has excellent initial mechanical properties, is resistant to aging, has excellent mechanical property retention rate, has a long service life, and has good sealing and reliability when applied to packaging structures.
[0124] So far, the technical solutions of the present application have been described in conjunction with the preferred embodiments, but it is easy for those skilled in the art to understand that the protection scope of the present application is obviously not limited to these specific embodiments. Without departing from the principles of the present application, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present application.
Claims
1. A sealant, characterized in that: The sealant comprises base glue, calcium carbonate, white carbon black, a cross-linking agent, a coupling agent and a catalyst. The crosslinking agent is a mixture of a first crosslinking agent and a second crosslinking agent, wherein the first crosslinking agent includes at least one of methyl tributylacetoximine silane, vinyl tributylacetoximine silane, and tetrabutyl tributylacetoximine silane, and the second crosslinking agent is a butanone oxime silane oligomer.
2. The sealant according to claim 1, characterized in that: The sealant comprises the following components by mass: 30-60 parts of base rubber, 30-60 parts of calcium carbonate, 0.5-3 parts of white carbon black, 2-5 parts of cross-linking agent, 0.3-3 parts of coupling agent, and 0.05-0.2 parts of catalyst.
3. The sealant according to claim 1 or 2, characterized in that: The mass ratio of the first cross-linking agent to the second cross-linking agent is 1:(0.3-1).
4. The sealant according to claim 1, characterized in that: The calcium carbonate is modified nano calcium carbonate, wherein the specific surface area of the modified nano calcium carbonate is 27 to 32 m 2 / g, the pH value of the modified nano calcium carbonate is 7.5-8.5; And / or, the white carbon black comprises fumed white carbon black, and the specific surface area of the fumed white carbon black is 150 to 250 m 2 / g.
5. The sealant according to claim 1, characterized in that: The base glue is a compound mixture of high-viscosity terminal hydroxyl polydimethylsiloxane and low-viscosity terminal hydroxyl polydimethylsiloxane. The high-viscosity terminal hydroxyl polydimethylsiloxane has a viscosity of 10,000 to 80,000 mPa·s, and the low-viscosity terminal hydroxyl polydimethylsiloxane has a viscosity of 1,000 to 5,000 mPa·s.
6. The sealant according to claim 5, characterized in that: The mass ratio of the high-viscosity terminal hydroxyl polydimethylsiloxane to the low-viscosity terminal hydroxyl polydimethylsiloxane is 1:(0.1-0.4).
7. The sealant according to claim 1, characterized in that: The coupling agent includes at least one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, and an amino coupling agent oligomer; And / or, the catalyst is dibutyltin dilaurate, stannous octoate or dibutyltin diceneodecanoate.
8. A method for preparing a sealant, for preparing the sealant according to any one of claims 1 to 7, characterized in that: The preparation method of the sealant comprises the following steps: The base rubber, the calcium carbonate and the white carbon black are mixed to prepare a base material; Mixing the base material with the cross-linking agent to prepare an intermediate; The intermediate, the coupling agent and the catalyst are mixed to prepare the sealant.
9. The method for preparing the sealant according to claim 8, characterized in that: Satisfy at least one of the following conditions: (1) In the step of preparing the base material, the mixing temperature is 100 to 120° C., the vacuum degree is ≤-0.095 MPa, and stirring is performed during mixing for a stirring time of 2 to 4 hours; (2) In the step of preparing the intermediate, stirring is performed during mixing and the stirring time is 15 min to 30 min; (3) In the step of preparing the sealant, stirring is performed during mixing and the stirring time is 15 min to 30 min, and the vacuum degree is ≤-0.095 MPa.
10. Use of the sealant according to any one of claims 1 to 7 in preparing a packaging structure.
11. A photovoltaic module, characterized in that: A packaging structure made of the sealant according to any one of claims 1 to 7.