High-performance matte silicone sealant and preparation method thereof
Through the synergistic effect of silane-modified polyurethane prepolymer with α,ω-dihydroxypolysiloxane and organic matting agent, the problem of insufficient mechanical properties and adhesive properties of existing matte silicone sealants is solved, and the problem of insufficient mechanical properties and adhesive properties of existing matte silicone sealants is achieved. High performance, low gloss matte effect.
Patent Information
- Application Number
- CN202411353240.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
AI Technical Summary
The existing matte silicone sealants have shortcomings in mechanical properties and adhesive properties, and the added large-particle inorganic matting agent has poor compatibility with polysiloxane, resulting in poor stability and wear resistance.
Use silane-modified polyurethane prepolymers in conjunction with α,ω-dihydroxypolysiloxane, organic matting agents such as cyclopentene, butadiene, pentadiene, etc., through isophorone diisocyanate and polypropylene glycol The reaction forms a polyurethane prepolymer with isocyanate group-terminated and reacts with nanoactive calcium carbonate, crosslinking agent and composite coupling agent in a vacuum environment to form a synergistic effect to improve matte effect and mechanical properties.
It realizes a high-performance, low-gloss matte silicone sealant, which has good mechanical properties and adhesive properties, avoiding the performance degradation caused by large-particle matting agents.
Smart Images

Figure BDA0005062886830000021 
Figure BDA0005062886830000031 
Figure BDA0005062886830000051
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sealants, and in particular relates to a high-performance matte silicone sealant and a preparation method thereof. Background Art
[0002] Dealcoholized one-component condensation type room temperature vulcanized liquid (RTV-1) silicone rubber is a paste made of α,ω-polydimethylsiloxane as the base polymer, supplemented with crosslinking agent, filler, plasticizer, coupling agent, and catalyst in a container isolated from moisture. It reacts with water in the air at room temperature and solidifies to form elastic silicone rubber. It has many excellent properties such as wide operating temperature range, excellent weather resistance, excellent electrical insulation performance, excellent biocompatibility, and adhesion to materials. In recent years, with the diversification of market demand and changes in people's aesthetic concepts, low-gloss silicone sealants with natural appearance and soft feel are becoming more and more popular.
[0003] At present, the common method for preparing matte silicone sealants on the market is to add a large-particle matting agent by simple physical blending to achieve a matte effect. Patent CN106634802A provides a method for preparing fluorescent matte silicone, in which tung oil is added as a matting agent in the formula of silicone sealant to achieve a matte effect. Due to the volatility and instability of tung oil, it is difficult for this formula to achieve a long-lasting matte effect and a good bonding effect, and the patent does not mention the specific gloss value. Patent CN115785890A achieves a matte effect by selecting a specific type and a specific particle size of matting powder. It includes silicon dioxide with a particle size of 3μm to 30μm and at least one of silicon micropowder, mica powder, and talcum powder with a particle size of 10μm to 50μm. The matting effect of adding matting agent to silicone sealant is excellent, but due to the poor compatibility of the added large-particle inorganic matting agent with polysiloxane, the matting agent is easy to agglomerate in the system, resulting in poor stability, poor wear resistance, reduced mechanical properties and poor adhesion of the sealant. Summary of the invention
[0004] The purpose of the present invention is to provide a matte silicone sealant with good mechanical properties and bonding properties.
[0005] The above-mentioned purpose is achieved by the following technical solutions.
[0006] The first aspect of the present invention provides a high-performance matte silicone sealant, which is prepared from raw materials including the following components in parts by weight:
[0007]
[0008] Wherein, the silane-modified polyurethane prepolymer is obtained by reacting a polyurethane prepolymer with 3-aminopropyltrimethoxysilane; the polyurethane prepolymer is obtained by reacting isophorone diisocyanate with polypropylene glycol;
[0009] The organic matting agent is at least one of cyclopentadiene, butadiene, pentadiene, heptadiene and cyclohexene.
[0010] In some of the embodiments, the molar ratio of the polypropylene glycol, isophorone diisocyanate and 3-aminopropyltrimethoxysilane is 1:2-4:2-4; preferably, the molar ratio of the polypropylene glycol, isophorone diisocyanate and 3-aminopropyltrimethoxysilane is 1:2-2.5:2-2.5.
[0011] In some embodiments, the method for preparing the silane-modified polyurethane prepolymer comprises the following steps:
[0012] Step 1. Under the protection of inert gas, isophorone diisocyanate and polypropylene glycol are reacted in the presence of a catalyst to form a polyurethane prepolymer;
[0013] Step 2: reacting the obtained polyurethane prepolymer with 3-aminopropyltrimethoxysilane to obtain the silane-modified polyurethane prepolymer.
[0014] In some embodiments, the catalyst is at least one of dibutyltin dilaurate, dimethyltin dineodecanoate, stannous octoate, and dibutyltin diacetate; and / or,
[0015] The amount of the catalyst used is 0.05 wt.% of the total weight of isophorone diisocyanate and polypropylene glycol; and / or,
[0016] In step 1, the reaction temperature is 65°C to 75°C, and the reaction time is 5h to 8h; and / or,
[0017] In step 2, the reaction temperature is 65°C to 75°C, and the reaction time is 1h to 3h; and / or,
[0018] The inert gas is nitrogen.
[0019] In some embodiments, the molecular weight of the polypropylene glycol is 1000-1500; preferably, the molecular weight of the polypropylene glycol is 1000-1200.
[0020] In some embodiments, the matte silicone sealant is prepared from the following components in parts by weight:
[0021]
[0022] In some embodiments, the organic matting agent is preferably pentadiene, and the usage ratio of the silane-modified polyurethane prepolymer to the pentadiene is 25-27:1.5.
[0023] In some embodiments, the viscosity of the α,ω-dihydroxy polysiloxane at 25° C. is 10000 mPa·s to 500000 mPa·s; and / or,
[0024] The viscosity of the dimethyl silicone oil at 25° C. is 100 mPa.s to 10000 mPa.s; and / or,
[0025] The particle size of the nano active calcium carbonate is between 100nm and 140nm.
[0026] In some embodiments, the crosslinking agent is at least one of methyltrimethoxysilane, methyltriethoxysilane, propyltrimethoxysilane, and propyltriethoxysilane; and / or,
[0027] The composite coupling agent is at least two of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, N-βaminoethylγ-aminopropyltriethoxysilane, glycidyltriethoxysilane, and glycidyltrimethoxysilane; and / or,
[0028] The titanate vulcanizing agent is diisopropoxytitanium bis(ethyl acetoacetate) chelate.
[0029] A second aspect of the present invention provides a method for preparing the matte silicone sealant as described above, the method comprising the following steps:
[0030] Step a, dehydrating and blending α,ω-dihydroxy polysiloxane, silane-modified polyurethane prepolymer, dimethyl silicone oil and nano-active calcium carbonate in a kneader to obtain a base material;
[0031] Step b, reacting the obtained base material with a crosslinking agent and an organic matting agent in a mixer in a vacuum environment at room temperature;
[0032] Step c: adding a complex coupling agent and a titanate vulcanizing agent to the reacted base material and reacting them in a mixer in a vacuum environment to obtain a matte silicone sealant.
[0033] In some embodiments, in step a, the reaction temperature is 80°C to 150°C, the vacuum degree is -0.09MPa to 0.099MPa, and the dehydration and blending are performed for 30 minutes to 300 minutes; and / or,
[0034] In the step b, the vacuum degree is -0.04 MPa to 0.04 MPa, the rotation speed is 10 rpm to 800 rpm, and the reaction time is 5 minutes to 30 minutes; and / or,
[0035] In the step c, the vacuum degree is -0.09 MPa to 0.099 MPa, the rotation speed is 10 rpm to 800 rpm, and the reaction time is 30 minutes to 120 minutes.
[0036] In the present invention, an isocyanate group-terminated polyurethane prepolymer is first generated by reacting isophorone diisocyanate and polypropylene glycol, and then 3-aminopropyltrimethoxysilane is added to the polyurethane prepolymer for reaction to obtain a silane-modified polyurethane prepolymer. It is found that when the silane-modified polyurethane prepolymer and α,ω-dihydroxy polysiloxane are used as a base polymer and an organic matting agent is used in combination to prepare a dealcoholized silicone sealant, the silane-modified polyurethane prepolymer and the organic matting agent can form a synergistic effect, which can make the obtained dealcoholized silicone sealant have a good matte effect on the one hand, and can have good mechanical properties and bonding properties on the other hand, and will not cause obvious negative effects on the mechanical properties and bonding properties of the silicone sealant, such as the dry time, tensile strength, and elongation at break. DETAILED DESCRIPTION
[0037] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0038] The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or conditions recommended by the manufacturers. The various commonly used chemical reagents used in the examples are all commercially available products.
[0039] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.
[0040] In the present invention, isophorone diisocyanate and polypropylene glycol are reacted to first generate an isocyanate group-terminated polyurethane prepolymer, and then 3-aminopropyltrimethoxysilane is added for reaction to obtain a silane-modified polyurethane prepolymer. The silane-modified polyurethane prepolymer and α,ω-dihydroxy polysiloxane are used as a base polymer. Due to the difference in cohesive energy between the two polymers and the effect of microphase separation, a non-uniform phase interface is formed during the curing process, and finally a complex microscopic rough surface is formed, thereby achieving a good matting effect. In addition, the polar groups such as urethane and urea groups in the silane-modified polyurethane prepolymer can also effectively improve the silicone sealing. The mechanical properties and adhesion of the sealant are improved; at the same time, conjugated olefins such as heptadiene, cyclohexene, cyclopentadiene, butadiene, and pentadiene are used as organic matting agents, which have a synergistic effect with the silane-modified polyurethane prepolymer and can further improve the matte effect of the sealant. It is found through testing that the matte effect is best when pentadiene and the silane-modified polyurethane prepolymer are used in a certain proportion, and the use of the above-mentioned various organic matting agents in combination with the silane-modified polyurethane prepolymer will not cause obvious negative effects on the mechanical properties and adhesion properties of the silicone sealant such as the surface drying time, tensile strength, and elongation at break, and finally a high-performance, high-adhesion matte silicone sealant is obtained.
[0041] Through the above, the embodiment of the present invention provides a high-performance matte silicone sealant, which is prepared by the following components in parts by weight:
[0042]
[0043] Wherein, the silane-modified polyurethane prepolymer is obtained by reacting a polyurethane prepolymer with 3-aminopropyltrimethoxysilane; the polyurethane prepolymer is obtained by reacting isophorone diisocyanate with polypropylene glycol;
[0044] The organic matting agent is at least one of cyclopentadiene, butadiene, pentadiene, heptadiene and cyclohexene.
[0045] The following are specific embodiments of the present invention.
[0046] Embodiment 1:
[0047] This embodiment provides a high-performance matte silicone sealant, and the preparation method thereof comprises the following steps:
[0048] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 25 parts of silane-modified polyurethane prepolymer, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120° C., the vacuum degree was -0.09 MPa, and dehydration and blending were performed for 180 minutes to obtain a base material, and then cooled for use;
[0049] At room temperature, the base material obtained above was added into a planetary mixer, and then 5 parts of methyltrimethoxysilane and 1.5 parts of heptadiene were added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0050] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a matte silicone sealant with long-term storage stability.
[0051] The preparation method of the silane-modified polyurethane prepolymer comprises the following steps:
[0052] Under nitrogen protection, isophorone diisocyanate, polypropylene glycol with a molecular weight of 1000 and dibutyltin dilaurate are reacted at a reaction temperature of 70°C and a reaction time of 6 hours to generate a polyurethane prepolymer terminated with an isocyanate group;
[0053] Then, 3-aminopropyltrimethoxysilane was added to the polyurethane prepolymer for reaction at a temperature of 70° C. for a reaction time of 1 h to obtain a silane-modified polyurethane prepolymer;
[0054] The molar ratio of isophorone diisocyanate, polypropylene glycol and 3-aminopropyltrimethoxysilane in the reaction is 2:1:2, and the amount of dibutyltin dilaurate used is 0.05wt.% of the total weight of isophorone diisocyanate and polypropylene glycol.
[0055] Embodiment 2:
[0056] This embodiment provides a high-performance matte silicone sealant, and the preparation method thereof comprises the following steps:
[0057] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 25 parts of silane-modified polyurethane prepolymer, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120° C., the vacuum degree was -0.09 MPa, and dehydration and blending were performed for 180 minutes to obtain a base material, and then cooled for use;
[0058] At room temperature, the base material obtained above was added into a planetary mixer, and then 5 parts of methyltrimethoxysilane and 1.5 parts of pentadiene were added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0059] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a matte silicone sealant with long-term storage stability.
[0060] The preparation method of the silane-modified polyurethane prepolymer is the same as that in Example 1.
[0061] Embodiment 3:
[0062] This embodiment provides a high-performance matte silicone sealant, and the preparation method thereof comprises the following steps:
[0063] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 30 parts of silane-modified polyurethane prepolymer, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120° C., the vacuum degree was -0.09 MPa, and dehydration and blending were performed for 180 minutes to obtain a base material, and then cooled for standby use;
[0064] At room temperature, the base material obtained above is added into a planetary mixer or a high-speed disperser, and then 5 parts of methyltrimethoxysilane and 1.8 parts of heptadiene are added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0065] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a matte silicone sealant with long-term storage stability.
[0066] The preparation method of the silane-modified polyurethane prepolymer is the same as that in Example 1.
[0067] Embodiment 4:
[0068] This embodiment provides a high-performance matte silicone sealant, and the preparation method thereof comprises the following steps:
[0069] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 30 parts of silane-modified polyurethane prepolymer, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120° C., the vacuum degree was -0.09 MPa, and dehydration and blending were performed for 180 minutes to obtain a base material, and then cooled for standby use;
[0070] At room temperature, the base material obtained above is added into a planetary mixer or a high-speed disperser, and then 5 parts of methyltrimethoxysilane and 2.0 parts of cyclohexene are added into the planetary mixer together with the base material to carry out chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0071] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium di(ethyl acetoacetate) chelate were added to the reacted base material and further reacted for 40 minutes at a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a matte silicone sealant with long-term storage stability.
[0072] The preparation method of the silane-modified polyurethane prepolymer is the same as that in Example 1.
[0073] Embodiment 5:
[0074] This embodiment provides a high-performance matte silicone sealant, and the preparation method thereof comprises the following steps:
[0075] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 35 parts of silane-modified polyurethane prepolymer, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120° C., the vacuum degree was -0.09 MPa, and dehydration and blending were performed for 180 minutes to obtain a base material, which was then cooled for standby use;
[0076] At room temperature, the base material obtained above was added into a planetary mixer, and then 5 parts of methyltrimethoxysilane and 1.5 parts of cyclohexene were added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0077] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a matte silicone sealant with long-term storage stability.
[0078] The preparation method of the silane-modified polyurethane prepolymer is the same as that in Example 1.
[0079] Embodiment 6:
[0080] This embodiment provides a high-performance matte silicone sealant, and the preparation method thereof comprises the following steps:
[0081] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 35 parts of silane-modified polyurethane prepolymer, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120° C., the vacuum degree was -0.09 MPa, and dehydration and blending were performed for 180 minutes to obtain a base material, which was then cooled for standby use;
[0082] At room temperature, the base material obtained above was added into a planetary mixer, and then 5 parts of methyltrimethoxysilane and 1.5 parts of pentadiene were added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0083] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a matte silicone sealant with long-term storage stability.
[0084] The preparation method of the silane-modified polyurethane prepolymer is the same as that in Example 1.
[0085] Comparative Example 1:
[0086] This comparative example provides a silicone sealant, which is different from Example 1 in that no silane-modified polyurethane prepolymer is added, and only an organic matting agent is added, and specifically comprises the following steps:
[0087] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120°C, the vacuum degree was -0.09 MPa, and the mixture was dehydrated and blended for 180 minutes to obtain a base material, which was then cooled for use;
[0088] At room temperature, the base material obtained above was added into a planetary mixer, and then 5 parts of methyltrimethoxysilane and 1.5 parts of heptadiene were added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0089] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a silicone sealant that is stable for long-term storage.
[0090] Comparative Example 2:
[0091] This comparative example provides a silicone sealant, which is different from Example 1 in that no organic matting agent is added, and only silane-modified polyurethane prepolymer is added, and specifically comprises the following steps:
[0092] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 25 parts of silane-modified polyurethane prepolymer, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120° C., the vacuum degree was -0.09 MPa, and dehydration and blending were performed for 180 minutes to obtain a base material, and then cooled for use;
[0093] At room temperature, the base material obtained above was added into a planetary mixer, and then 5 parts of methyltrimethoxysilane was added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0094] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a silicone sealant that is stable for long-term storage.
[0095] The preparation method of the silane-modified polyurethane prepolymer is the same as that in Example 1.
[0096] Comparative Example 3:
[0097] This comparative example provides a silicone sealant, which is different from Example 1 in that no organic matting agent is added, and no silane-modified polyurethane prepolymer is added. The specific steps include:
[0098] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120°C, the vacuum degree was -0.09 MPa, and the mixture was dehydrated and blended for 180 minutes to obtain a base material, which was then cooled for use;
[0099] At room temperature, the base material obtained above was added into a planetary mixer, and then 5 parts of methyltrimethoxysilane was added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0100] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a silicone sealant that is stable for long-term storage.
[0101] Comparative Example 4:
[0102] This comparative example provides a silicone sealant, which is different from Example 1 in that mica powder is used to replace silane-modified polyurethane prepolymer and heptadiene, and specifically comprises the following steps:
[0103] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 26.5 parts of mica powder with a particle size of 20-30 μm, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm are added into a kneader, the temperature is 120° C., the vacuum degree is -0.09 MPa, and the mixture is dehydrated and blended for 180 minutes to obtain a base material, which is then cooled for standby use;
[0104] At room temperature, the base material obtained above is added into a planetary mixer, and then 5 parts of methyltrimethoxysilane is added into a planetary mixer or a high-speed disperser mixer to carry out chemical reaction with the base material at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0105] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a silicone sealant that is stable for long-term storage.
[0106] Comparative Example 5:
[0107] This comparative example provides a silicone sealant, which is different from Example 1 in that heavy calcium carbonate is used to replace the silane-modified polyurethane prepolymer and heptadiene, and specifically comprises the following steps:
[0108] First, 100 parts of α,ω-dihydroxypolydimethylsiloxane with a viscosity of 50000 mPa·s, 26.5 parts of heavy calcium carbonate with a particle size of 1 μm, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-activated carbonic acid with a particle size of 120 nm were added into a kneader at a temperature of 120° C. and a vacuum degree of -0.09 MPa. The mixture was dehydrated and blended for 180 minutes to obtain a base material, which was then cooled for standby use.
[0109] At room temperature, the base material obtained above was added into a planetary mixer, and then 5 parts of methyltrimethoxysilane was added into the planetary mixer together with the base material for chemical reaction at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0110] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a silicone sealant that is stable for long-term storage.
[0111] Comparative Example 6
[0112] This comparative example provides a silicone sealant, which is different from Example 1 in that heptadiene is replaced by heavy calcium carbonate, and specifically comprises the following steps:
[0113] First, 100 parts of α,ω-dihydroxy polydimethylsiloxane with a viscosity of 50000 mPa·s, 25 parts of silane-modified polyurethane prepolymer, 5 parts of dimethyl silicone oil with a viscosity of 500 mPa·s, and 110 parts of nano-active calcium carbonate with a particle size of 120 nm were added into a kneader, the temperature was 120° C., the vacuum degree was -0.09 MPa, and dehydration and blending were performed for 180 minutes to obtain a base material, and then cooled for use;
[0114] At room temperature, the base material obtained above is added into a planetary mixer, and then 5 parts of methyltrimethoxysilane and 1.5 parts of heavy calcium carbonate are added into a planetary mixer or a high-speed disperser to carry out chemical reaction with the base material at a vacuum degree of -0.04 MPa and a rotation speed of 720 rpm for 10 minutes;
[0115] Finally, 2 parts of γ-aminopropyltrimethoxysilane, 0.5 parts of γ-glycidyloxypropyltrimethoxysilane, and 4 parts of diisopropoxytitanium bis(ethyl acetate) chelate were added to the reacted base material, and a chemical reaction was further carried out for 40 minutes under the conditions of a vacuum degree of -0.09 MPa and a rotation speed of 300 rpm to produce a silicone sealant that is stable for long-term storage.
[0116] The surface drying time of the silicone sealant in the above embodiments and comparative examples is tested according to the requirements of GB / T 13477.5, and the tensile bonding strength at 23°C, the bonding failure area, and the elongation at the maximum tensile strength at 23°C are tested according to the tensile adhesion determination index requirements in GB 16776-2005. The sealants prepared in the above embodiments and comparative examples are prepared into samples with a length, width and height of 50mm*50mm*2mm respectively, ensuring that the surface is flat, without bubbles, scratches, wrinkles, etc., and tested after curing for 48 hours under the conditions of 23±2°C and 50±10%RH. The surface gloss of the object is tested according to GB / T 4893.6-2013, and the gloss at six different positions is tested and the average value is taken as the result (the experimental results all use the value of the test angle of 60°). The specific test results are shown in Table 1.
[0117] Table 1 Performance test results of matte silicone sealant
[0118]
[0119]
[0120] As can be seen from Examples 1-6, isophorone diisocyanate and polypropylene glycol are reacted to first generate an isocyanate group-terminated polyurethane prepolymer, and then 3-aminopropyltrimethoxysilane is added to react to obtain a silane-modified polyurethane prepolymer. The silane-modified polyurethane prepolymer and α,ω-dihydroxy polysiloxane are combined as a base polymer. Due to the difference in cohesive energy between the two polymers and the effect of microphase separation, a non-uniform phase interface is formed during the curing process, and finally a complex microscopic rough surface is formed, thereby achieving a good matting effect. The polar groups such as carbamate and urea groups in the silane-modified polyurethane prepolymer can also effectively improve the mechanical properties and adhesion of the silicone sealant. At the same time, conjugated olefins such as cyclopentadiene, butadiene, and pentadiene are used as organic matting agents to further improve the matte effect of the sealant, and will not cause obvious negative effects on the mechanical properties and adhesion properties of the silicone sealant such as the surface drying time, tensile strength, and elongation at break, and finally a high-performance, high-adhesion matte silicone sealant is obtained. The test found that the best matting effect is achieved when pentadiene and silane-modified polyurethane prepolymer are used in a certain proportion.
[0121] By comparing Example 1 with Comparative Examples 1-3, it can be seen that the introduced silane-modified polyurethane prepolymer and the organic matting agent can effectively reduce the glossiness of the silicone sealant surface when used in combination, and the performance of the sealant does not decrease significantly, while it is difficult to achieve a matte effect when used alone.
[0122] By comparing Example 1 with Comparative Example 4, it can be seen that although the use of inorganic matting agents with large particle sizes can also achieve a matte effect, the tensile strength and elongation at break of the sealant are greatly reduced.
[0123] By comparing Example 1 with Comparative Example 5, it can be seen that the use of heavy calcium carbonate can reduce the glossiness, but it is difficult to achieve a matte finish, and the mechanical properties and bonding properties of the silicone sealant will also decrease.
[0124] By comparing Example 1 and Comparative Example 6, it can be seen that the silane-modified polyurethane prepolymer and heavy calcium carbonate can effectively reduce the glossiness of the silicone sealant surface when used in combination, but it is difficult to achieve a matte finish, and the performance of the sealant is slightly reduced due to the addition of heavy calcium carbonate.
[0125] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0126] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A high-performance matte silicone sealant, characterized in that: The matte silicone sealant is prepared from the following raw materials by weight: Wherein, the silane-modified polyurethane prepolymer is obtained by reacting a polyurethane prepolymer with 3-aminopropyltrimethoxysilane; the polyurethane prepolymer is obtained by reacting isophorone diisocyanate with polypropylene glycol; The organic matting agent is at least one of cyclopentadiene, butadiene, pentadiene, heptadiene and cyclohexene.
2. The high-performance matte silicone sealant according to claim 1, characterized in that: The molar ratio of the polypropylene glycol, isophorone diisocyanate and 3-aminopropyltrimethoxysilane is 1:2-4:2-4; preferably, the molar ratio of the polypropylene glycol, isophorone diisocyanate and 3-aminopropyltrimethoxysilane is 1:2-2.5:2-2.
5.
3. The high-performance matte silicone sealant according to claim 1, characterized in that: The preparation method of the silane-modified polyurethane prepolymer comprises the following steps: Step 1. Under the protection of inert gas, isophorone diisocyanate and polypropylene glycol are reacted in the presence of a catalyst to form a polyurethane prepolymer; Step 2: reacting the obtained polyurethane prepolymer with 3-aminopropyltrimethoxysilane to obtain the silane-modified polyurethane prepolymer.
4. The high-performance matte silicone sealant according to claim 3, characterized in that: The catalyst is at least one of dibutyltin dilaurate, dimethyltin diceneodecanoate, stannous octoate and dibutyltin diacetate; and / or, The amount of the catalyst used is 0.05 wt.% of the total weight of isophorone diisocyanate and polypropylene glycol; and / or, In step 1, the reaction temperature is 65°C to 75°C, and the reaction time is 5h to 8h; and / or, In step 2, the reaction temperature is 65°C to 75°C, and the reaction time is 1h to 3h; and / or, The inert gas is nitrogen.
5. The high-performance matte silicone sealant according to any one of claims 1 to 4, characterized in that: The molecular weight of the polypropylene glycol is 1000-1500; preferably, the molecular weight of the polypropylene glycol is 1000-1200.
6. The high-performance matte silicone sealant according to any one of claims 1 to 4, characterized in that: The matte silicone sealant is prepared from the following components in parts by weight:
7. The high-performance matte silicone sealant according to any one of claims 1 to 4, characterized in that: The viscosity of the α,ω-dihydroxy polysiloxane at 25° C. is 10000 mPa·s to 500000 mPa·s; and / or, The viscosity of the dimethyl silicone oil at 25° C. is 100 mPa.s to 10000 mPa.s; and / or, The particle size of the nano active calcium carbonate is between 100nm and 140nm.
8. The high-performance matte silicone sealant according to any one of claims 1 to 4, characterized in that: The crosslinking agent is at least one of methyltrimethoxysilane, methyltriethoxysilane, propyltrimethoxysilane and propyltriethoxysilane; and / or, The composite coupling agent is at least two of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, N-βaminoethylγ-aminopropyltriethoxysilane, glycidyltriethoxysilane, and glycidyltrimethoxysilane; and / or, The titanate vulcanizing agent is diisopropoxytitanium bis(ethyl acetoacetate) chelate.
9. A method for preparing the matte silicone sealant according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: Step a, dehydrating and blending α,ω-dihydroxy polysiloxane, silane-modified polyurethane prepolymer, dimethyl silicone oil and nano-active calcium carbonate in a kneader to obtain a base material; Step b, reacting the obtained base material with a crosslinking agent and an organic matting agent in a mixer in a vacuum environment at room temperature; Step c: adding a complex coupling agent and a titanate vulcanizing agent to the reacted base material and reacting them in a mixer in a vacuum environment to obtain a matte silicone sealant.
10. The preparation method according to claim 9, characterized in that: In the step a, the reaction temperature is 80°C to 150°C, the vacuum degree is -0.09MPa to 0.099MPa, and the dehydration and blending are performed for 30 minutes to 300 minutes; and / or, In the step b, the vacuum degree is -0.04 MPa to 0.04 MPa, the rotation speed is 10 rpm to 800 rpm, and the reaction time is 5 minutes to 30 minutes; and / or, In the step c, the vacuum degree is -0.09 MPa to 0.099 MPa, the rotation speed is 10 rpm to 800 rpm, and the reaction time is 30 minutes to 120 minutes.
Citation Information
Cited By
Ketoxime-removing type matte organic silicon sealant and preparation method thereof
CN122012015A
A ketoxime-based matte silicone sealant and its preparation method
CN122012015B