Dual-curing LED packaging adhesive and preparation method thereof

Through the design of dual-curing LED packaging glue, the cross-linking of nonlinear thiol silicone resin and end-capped structure is used to solve the aging problem of LED packaging materials in high-temperature UV light environment, improve the mechanical properties and anti-aging properties, and extend the LED lifespan and improve packaging efficiency.

CN118931484APending Publication Date: 2024-11-12CHAMBROAD CHEM IND RES INST CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411164209.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing LED packaging materials age under high temperature and UV light environments, resulting in yellowing, discoloration, and decreased luminous efficiency, slow curing speed, low mechanical strength and short service life.

Method used

Using dual-curing LED packaging glue, its raw materials include components A and B. Through the click reaction of nonlinear thiol silicone resin and the crosslinking of the end capping structure, combined with photocuring and thermal curing, the mechanical properties and resistance of the glue are improved. Aging performance.

Benefits of technology

It significantly improves the tensile strength, tear resistance and light transmittance of LED packaging glue, extends the service life, solves the problems of easy yellowing and large packaging energy consumption, and achieves rapid curing and efficient packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005007360970000061
    Figure BDA0005007360970000061
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer material packaging adhesives, and provides a dual-curing LED packaging adhesive and a preparation method thereof.The dual-curing LED packaging adhesive is prepared from a component A and a component B. The weight ratio of the component A to the component B is (1-5): 1; the component A is prepared from the following components in parts by weight: 60 to 70 parts of phenyl vinyl silicone oil, 30 to 40 parts of silicon resin, 0.0007 to 0.0012 part of a KARTEDT catalyst and 0.0007 to 0.0012 part of a de-foaming agent; the component B is prepared from the following components in parts by weight: 60 to 70 parts of phenyl hydrogen-containing silicone oil, 25 to 45 parts of hydrogen-containing silicone resin and 0.001 to 0.0015 part of a photoinitiator; the packaging adhesive has the characteristics of high toughness, good anti-aging performance, low packaging energy consumption, easiness in industrialization and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer material packaging adhesives, and in particular relates to a dual-curable LED packaging adhesive and a preparation method thereof. Background Art

[0002] As a new type of environmentally friendly and energy-saving lighting equipment, LED equipment has strong vibration resistance and longer service life, better resistance to frequent switching of switches, and can also provide considerable brightness lighting in low voltage and low current environments. Due to these characteristics, the application of LED lamps is becoming more and more extensive.

[0003] For the practical application of LED lights, packaging technology is essential. The performance of packaging materials directly affects the brightness and service life of LED devices. The stronger the performance of LED, the higher the requirements for packaging materials. High-power LED lights need to withstand higher operating temperatures and high-intensity UV light when in use, which causes LED lights to age faster and reduce their service life. High-performance LED packaging materials should have high UV resistance, heat resistance and light transmittance.

[0004] However, the commonly used LED packaging materials show obvious yellowing or discoloration after light aging, heat aging, and long-term exposure to light and heat environments, and the luminous efficiency is significantly reduced. There are also problems such as slow curing speed, low mechanical strength, and serious time and energy consumption. The invention patent CN105176483B mentions a high refractive index and high toughness resistant sulfurized LED packaging silicone, which has excellent resistance to cold and heat shock, but its packaging energy consumption is large (150℃, 4h); the invention patent CN107841284B mentions a power LED packaging glue, which has a tensile strength of about 1.5MPa and poor toughness.

[0005] Therefore, there is an urgent need to develop LED packaging materials with high mechanical properties, long life, low packaging energy consumption, high toughness and anti-aging. Summary of the invention

[0006] In order to solve the problems of insufficient toughness and short service life of LED device packaging in the existing process, the present invention provides a dual-curable LED packaging adhesive and a preparation method thereof, which has the characteristics of high toughness, good anti-aging performance, low packaging energy consumption, and easy industrialization.

[0007] To solve the above problems, the specific technical solutions provided by the present invention are as follows:

[0008] A dual-curable LED encapsulation adhesive, the raw materials of which include component A and component B, in which, by weight, component A: component B = (1-5): 1; more preferably, component A: component B = (3-5): 1;

[0009] Within the above ratio range, it can meet both the faster curing speed and the larger cross-linking density and the viscosity required for construction.

[0010] The component A comprises, by weight, 60-70 parts of phenyl vinyl silicone oil, 30-40 parts of silicone resin, 0.0007-0.0012 parts of KARSTEDT catalyst and 0.0007-0.0012 parts of defoaming agent;

[0011] The B component comprises, by weight, 60-70 parts of phenyl hydrogen-containing silicone oil, 25-45 parts of hydrogen-containing silicone resin, and 0.001-0.0015 parts of photoinitiator.

[0012] Preferably, in the component A, the phenyl vinyl silicone oil is a non-end-capped structure.

[0013] Preferably, in the component A, the silicone resin is a mixture of phenyl vinyl MQ silicone resin, vinyl TQ silicone resin and mercapto silicone resin; more preferably, in the mixture, the molar ratio of the vinyl group of the phenyl vinyl MQ silicone resin: the vinyl group of the vinyl TQ silicone resin: the mercapto group of the mercapto silicone resin is (1-3):(0.4-3):(1-3).

[0014] The above-mentioned mixed silicone resin has different vinyl-containing structural units, which undergo addition reactions with the substances containing silicon-hydrogen bonds in component B, and undergo click reactions with the structural units having thiol groups under the action of the photoinitiator and light in component B. The degree of crosslinking is much higher than that of ordinary packaging glue, thereby making the glue have better toughness.

[0015] More preferably, the mercapto silicone resin has a viscosity of 20,000-30,000 mPa·s at 25° C. and a refractive index of 1.5600-1.5750.

[0016] The KARSTEDT catalyst in the above-mentioned component A is obtained by dispersing 3-8 parts by weight of a platinum-siloxane complex in 1000 parts by weight of phenyl vinyl silicone oil; the number of parts of the above-mentioned catalyst is the number of parts of the total KARSTEDT catalyst dispersion, that is, 0.0007-0.0012 parts of KARSTEDT catalyst in component A, which includes both the platinum-siloxane complex and the phenyl vinyl silicone oil used for dispersion.

[0017] More preferably, the viscosity of the phenyl vinyl silicone oil at 25° C. is 5000-8000 mPa·s.

[0018] Preferably, the phenyl mass content of the phenyl vinyl silicone oil and the phenyl vinyl silicone resin is greater than 45%; selecting the above standard can further improve the anti-aging performance of the product and extend its service life.

[0019] Preferably, in the component A, the defoaming agent is a combination of one or more of BYK-1796, BYK-1790, Sago-1685, DC-71, and Hongtai X-236.

[0020] In the B component, the phenyl hydrogen silicone oil is an end-capped structure; the phenyl hydrogen silicone oil adopts an end-capped structure, while the phenyl vinyl silicone oil in the A component adopts a non-end-capped structure, which helps to further improve the cross-linking performance and hardness of the product; if both the phenyl vinyl silicone oil and the phenyl hydrogen silicone oil adopt an end-capped structure, their structures after the reaction are linear, that is, the cross-linking density of the encapsulation glue is poor, and the direct phenomenon is that the product is gel-like or liquid, and its hardness cannot meet the requirements.

[0021] More preferably, the viscosity of the phenyl hydrogen silicone oil at 25° C. is 5000-8000 mPa·s.

[0022] Preferably, in the B component, the hydrogen-containing silicone resin is a phenyl hydrogen-containing silicone resin;

[0023] More preferably, the refractive index of the hydrogen-containing silicone resin is 1.5400-1.5500, and the hydrogen content is 0.4%-0.7%.

[0024] Preferably, in the component B, the photoinitiator is one or a combination of dihydroxy dimethyl propiophenone, dihydroxy tetramethoxybenzophenone, and dihydroxy tetra-n-octyloxybenzophenone;

[0025] More preferably, when the photoinitiator is added, first, 20-30 parts by weight of the photoinitiator needs to be dispersed in 100 parts by weight of phenyl hydrogenated silicone oil. After the photoinitiator dispersion is prepared, it is added to the B component system after conversion according to the amount of the pure photoinitiator substance. The phenyl hydrogenated silicone oil in the dispersion is included in 60-70 parts of the phenyl hydrogenated silicone oil in the above components. The 0.001-0.0015 parts of the photoinitiator in the B component refers only to the photoinitiator, and does not include the phenyl hydrogenated silicone oil in the photoinitiator dispersion.

[0026] In addition, the present invention also provides a method for preparing the dual-curable LED packaging adhesive, which specifically comprises the following steps:

[0027] 1) Preparation of component A: Add phenyl vinyl silicone oil, silicone resin, KARSTEDT catalyst and defoamer into a double planetary mixer in sequence, stir at 70-120 rpm for 60-100 min, and disperse at 1500-2500 rpm for 60-100 min. Wait until the stirring and dispersing process is completed, and evacuate until there is no bubble to obtain component A;

[0028] 2) Preparation of component B: Add phenyl hydrogen silicone oil, hydrogen silicone resin and photoinitiator into a double planetary mixer in sequence, stir at 70-120 rpm for 50-100 min, and disperse at 1500-2500 rpm for 50-100 min, wait for the stirring and dispersing process to end, and evacuate until there is no bubble, thereby obtaining component B;

[0029] 3) The above-mentioned component A and component B are mixed evenly according to a certain proportion, vacuum degassed, and cured to obtain the LED encapsulation adhesive.

[0030] Compared with the prior art, the dual-curable LED encapsulation adhesive provided by the present invention has achieved the following technical effects:

[0031] 1) The nonlinear mercapto silicone resin of the present invention introduces mercapto groups through a click reaction. Based on the ratio of the above-mentioned components A and B, the light curing and heat curing reaction systems can produce more than 2 times the effect, and the mechanical properties of the adhesive, such as tensile strength, tear strength, elongation at break, etc., are greatly improved after curing. The mercapto silicone resin prepared and used in the present invention has mercapto groups concentrated in the side chains and has multiple side chains. When reacting with the vinyl groups on the side chains of phenyl vinyl silicone oil, the crosslinking density can be greatly increased, thereby enhancing the mechanical properties of the adhesive;

[0032] 2) The present invention uses end-capped phenyl hydrogen silicone oil and non-end-capped phenyl vinyl silicone oil, and the prepared encapsulation glue has an ideal cross-linking density and improved hardness, which overcomes the problem that when both phenyl hydrogen silicone oil and phenyl vinyl silicone oil are end-capped, the cross-linking density and hardness are poor, and the product may be gel-like or liquid;

[0033] 3) The silicone resin used in the present invention, by limiting the ratio of the vinyl group to the mercapto group of the phenyl vinyl silicone resin and the mercapto silicone resin in its components, under the other component ratios in the present invention, the mechanical properties of the product are significantly improved, the light transmittance is good and yellowing is not easy to occur;

[0034] 4) The present invention adopts a dual curing method (light curing + heat curing), a photoinitiator is added to component B to absorb light of some wavelengths, and the phenyl mass content in phenyl vinyl silicone oil and phenyl vinyl silicone resin is greater than 45%, which improves the anti-aging performance of the glue and solves the problem that the high-power LED packaging glue is easy to yellow and thus shortens the service life of the LED device;

[0035] 5) The present invention applies light-thermal dual-curing organic silicone to high-power LED packaging, which shortens the molding time and greatly improves the packaging efficiency. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below in conjunction with specific embodiments. These embodiments are only used to illustrate the technical solution of the present invention in more detail and should not be construed as limiting the protection scope of the present invention.

[0037] Unless otherwise specified, the chemical substances, drugs, etc. used in the examples are all commercially available products.

[0038] Example 1

[0039] A dual-curable LED encapsulation adhesive, the raw materials of which include component A and component B, wherein the preparation of the mercapto silicone resin in component A is as follows: weigh 58.9g of trimercaptopropyl trimethoxysilane and 28.42g of isopropyl titanate in a three-necked round-bottom flask, stir magnetically for 20min at room temperature, and mix evenly; then weigh 129.79g of diphenylsilanediol and slowly add it to the three-necked flask, stir to make it evenly mixed; dropwise add 8.6g of concentrated hydrochloric acid as a catalyst, heat at 100°C for 4h, and continuously blow nitrogen into the solution during the reaction to take away the reaction byproduct methanol until the reaction is completed; after the reaction is completed, the following post-treatment is performed, namely, suction filtration, deacidification, suction filtration, rotary evaporation (70°C), and reduced pressure distillation (70°C) to obtain the mercapto silicone resin; the deacidification preferably uses a saturated sodium carbonate solution for deacidification, specifically, adding a saturated sodium carbonate solution to neutralize to pH 7. The obtained mercapto silicone resin has a viscosity of 27618mPa·s and a refractive index of 1.5670.

[0040] Example 2

[0041] A dual-curable LED packaging adhesive, the packaging adhesive comprising component A and component B, wherein the weight ratio of component A to component B is 4:1;

[0042] Component A, calculated by weight, includes: 60 parts of phenyl vinyl silicone oil (viscosity at 25°C is 5000mPa·s), 39.998 parts of silicone resin (viscosity at 25°C is 11000mPa·s), 0.001 parts of KARSTEDT catalyst (viscosity at 25°C is 5000mPa·s), and 0.001 parts of BYK-1790 defoamer;

[0043] The silicone resin is selected from a mixture of phenyl vinyl MQ silicone resin, vinyl TQ silicone resin, and mercapto silicone resin; wherein the molar ratio of phenyl vinyl MQ silicone resin vinyl / vinyl TQ silicone resin vinyl / mercapto silicone resin mercapto is 1:0.8:1.5, and the ratio of each functional group is calculated based on the known components of the raw materials;

[0044] The KARSTEDT catalyst in the A component is prepared by dispersing 4 parts by weight of a platinum-siloxane complex in 1000 parts by weight of phenyl vinyl silicone oil;

[0045] The number of parts of the KARSTEDT catalyst is the weight of the entire platinum-siloxane complex dispersion;

[0046] In the component A, the phenyl vinyl silicone oil is a non-terminated structure.

[0047] Component B includes, by weight: 65 parts of phenyl hydrogen-containing silicone oil, 34.9987 parts of hydrogen-containing silicone resin, and 0.0013 parts of photoinitiator;

[0048] The hydrogen-containing silicone resin is selected from phenyl hydrogen-containing silicone resin, has a refractive index of 1.5441, and a hydrogen content of 0.61%.

[0049] The phenyl hydrogen-containing silicone oil is a terminal-capped structure and has a viscosity of 5400 mPa·s.

[0050] The photoinitiator used is dihydroxydimethylpropiophenone. When the photoinitiator is added, 22 parts by weight of the photoinitiator need to be dispersed in 100 parts by weight of phenyl hydrogenated silicone oil. After the photoinitiator dispersion is prepared, it is added to the B component system after conversion according to the amount of pure photoinitiator substance. The phenyl hydrogenated silicone oil in the dispersion is counted into 65 parts of phenyl hydrogenated silicone oil in the above components.

[0051] The number of parts of the photoinitiator is the weight part of dihydroxydimethylpropiophenone alone.

[0052] The preparation method of the dual-curable LED packaging adhesive comprises the following specific steps:

[0053] 1) Preparation of component A: Add phenyl vinyl silicone oil, silicone resin, KARSTEDT catalyst and defoamer into a double planetary mixer in sequence, stir at 100 rpm for 90 min, and disperse at 2000 rpm for 85 min. Wait until the stirring and dispersing process is completed, and evacuate until there is no bubble, thereby obtaining component A;

[0054] 2) Preparation of component B: Add phenyl hydrogen silicone oil, hydrogen silicone resin and photoinitiator into a double planetary mixer in sequence, stir at 100 rpm for 60 min, and disperse at 2000 rpm for 55 min. Wait until the stirring and dispersing process is completed, and evacuate until there is no bubble, thereby obtaining component B;

[0055] 3) Mix component A and component B evenly, perform vacuum degassing, and obtain LED encapsulation adhesive after curing;

[0056] The dual curing process is to quickly cure under a UV lamp with a wavelength of 365nm for 10s, and then cure at 120℃ for 10min to fully cure.

[0057] Example 3

[0058] This embodiment is basically the same as Embodiment 2, except that component B includes, by weight, 60 parts of phenyl hydrogenated silicone oil, 39.9987 parts of hydrogenated silicone resin, and 0.0013 parts of photoinitiator.

[0059] Example 4

[0060] This embodiment is basically the same as Embodiment 2, except that component A contains, by weight, 62 parts of phenyl vinyl silicone oil (viscosity at 25°C is 5000 mPa·s), 37.998 parts of silicone resin (viscosity at 25°C is 10080 mPa·s), 0.0009 parts of KARSTEDT catalyst (viscosity at 25°C is 5000 mPa·s), and 0.0011 parts of BYK-1790 defoamer, wherein the ratio of phenyl vinyl MQ silicone resin vinyl / vinyl TQ silicone resin vinyl / thiol silicone resin thiol=1:1.25:1.875.

[0061] Comparative Example 1

[0062] This comparative example is basically the same as Example 2, except that in component A, by weight, there are 54 parts of phenyl vinyl silicone oil (viscosity at 25°C is 5000mPa·s), 45.998 parts of silicone resin (viscosity at 25°C is 11580mPa·s), 0.001 parts of KARSTEDT catalyst (viscosity at 25°C is 5000mPa·s), and 0.001 parts of BYK-1790 defoaming agent, wherein the ratio of vinyl MQ silicone resin vinyl / vinyl TQ silicone resin vinyl / thiol silicone resin thiol=2.5:1:0.

[0063] Comparative Example 2

[0064] This comparative example is basically the same as Example 2, except that the silicone resin is selected from a mixture of phenyl vinyl MQ silicone resin, vinyl TQ silicone resin, and mercapto silicone resin; wherein the molar ratio of phenyl vinyl MQ silicone resin vinyl / vinyl TQ silicone resin vinyl / mercapto silicone resin mercapto is 1:4:0.5.

[0065] Comparative Example 3

[0066] This comparative example is basically the same as Example 2, except that component B comprises, by weight, 50 parts of phenyl hydrogen-containing silicone oil, 49.9987 parts of hydrogen-containing silicone resin, and 0.0013 parts of photoinitiator.

[0067] Comparative Example 4

[0068] This comparative example is basically the same as Example 2, except that the packaging glue includes component A and component B, and the weight ratio of component A to component B is 3.4:1;

[0069] Component A includes, by weight: 46 parts of phenyl vinyl silicone oil (viscosity at 25°C is 5000 mPa·s), 53.998 parts of silicone resin (viscosity at 25°C is 13770 mPa·s), 0.001 parts of Karstedt catalyst (viscosity at 25°C is 5000 mPa·s), and 0.001 parts of BYK-1790 defoamer, wherein the ratio of phenyl vinyl MQ silicone resin vinyl / vinyl TQ silicone resin vinyl / thiol silicone resin thiol is 1:0.8:1.5;

[0070] Component B includes, by weight: 84 parts of phenyl hydrogen-containing silicone oil, 15.9992 parts of hydrogen-containing silicone resin, and 0.0008 parts of photoinitiator.

[0071] Comparative Example 5

[0072] This comparative example is basically the same as Example 2, except that the phenyl vinyl silicone oil has a capped structure and is in a gel state after curing, and is not suitable for packaging glue.

[0073] Experimental example

[0074] Refractive index: Use Abbe refractometer to test by dropping the uncured sample directly on the prism of Abbe refractometer. The test temperature is (25±2)℃.

[0075] Light transmittance: A sample with a length and width of 2 cm and a thickness of 3 mm was prepared using the encapsulation adhesive, and tested using an ultraviolet-visible spectrophotometer with a test scanning range of 300 to 800 nm.

[0076] Tensile strength and elongation at break test: A dumbbell-shaped specimen with a length of 80 mm and a thickness of 3 mm was made from the encapsulation adhesive and tested using a universal material testing machine.

[0077] Yellowing index test: A sample with a length and height of 2 cm and a thickness of 3 mm was prepared using the encapsulating glue, and its chromaticity was measured using a colorimeter.

[0078] High temperature and high humidity experiment: A sample with a thickness of 3 mm was prepared using the encapsulation adhesive and placed in a heat aging test chamber for 48 hours. The conditions of the heat aging test chamber were 120° C. and 100% RH.

[0079] Red ink experiment: Use the encapsulation glue to encapsulate the SMD lamp beads, quickly cure them under a UV lamp with a wavelength of 365nm for 10s, and then cure them at 120℃ for 10min. After the glue is cured, soak them in 50% red ink and boil them for 8 hours. Then wash the lamp beads and observe the red ink penetration under a microscope.

[0080] The test results are shown in Table 1.

[0081] Table 1 Performance test results of the cured adhesives of the embodiments and comparative examples

[0082]

[0083] It can be seen from Examples 2-4 in the above table that, through the formula of this invention, components AB cooperate with each other, component A contains different vinyl-containing structural units, which react with the silicon-hydrogen bond-containing substance in component B, and react with the structural units having thiol groups under the action of the initiator of component B and light, and the degree of crosslinking is much higher than that of ordinary packaging glue, so that the elongation at break and tensile strength data of the glue perform well, indicating that it has good toughness; and the data of high temperature and high humidity experiments and red ink experiments show that the glue has good anti-aging properties.

[0084] Compared with Example 2, Comparative Example 1 does not contain mercapto silicone resin, and cannot make use of the side chain structure of mercapto silicone resin itself and UV curing reaction for double addition, so the toughness and anti-aging performance of the prepared glue are affected. Compared with Example 2, Comparative Examples 2-4 do not meet the formula ratio, the various materials cannot cooperate with each other, and the prepared glue has poor performance.

[0085] It can be seen from the above that the encapsulation adhesive prepared by the present invention has certain toughness and good anti-aging performance and a high refractive index, and is very suitable for encapsulating high-power LEDs.

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any equivalent substitutions, modifications, etc. made by technicians in this field without any creative work within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A dual-curable LED encapsulation adhesive, characterized in that: The invention comprises component A and component B, wherein component A: component B = (1-5): 1, in parts by weight; the component A comprises, in parts by weight, 60-70 parts of phenyl vinyl silicone oil, 30-40 parts of silicone resin, 0.0007-0.0012 parts of KARSTEDT catalyst and 0.0007-0.0012 parts of defoaming agent; the component B comprises, in parts by weight, 60-70 parts of phenyl hydrogen-containing silicone oil, 25-45 parts of hydrogen-containing silicone resin and 0.001-0.0015 parts of photoinitiator.

2. The dual-curable LED packaging adhesive according to claim 1, characterized in that: By weight, component A: component B = (3-5):

1.

3. The dual-curable LED packaging adhesive according to claim 1 or 2, characterized in that: In the component A, the phenyl vinyl silicone oil is a non-terminated structure; the silicone resin is a mixture of phenyl vinyl MQ silicone resin, vinyl TQ silicone resin, and mercapto silicone resin; and the defoamer is a combination of one or more of BYK-1796, BYK-1790, Sago-1685, DC-71, and Hongtai X-236.

4. The dual-curable LED packaging adhesive according to claim 1 or 2, characterized in that: The KARSTEDT catalyst in component A is obtained by dispersing 3-8 parts by weight of a platinum-siloxane complex in 1000 parts by weight of phenyl vinyl silicone oil.

5. The dual-curable LED packaging adhesive according to claim 1 or 2, characterized in that: The molar ratio of vinyl group of phenyl vinyl MQ silicone resin: vinyl group of vinyl TQ silicone resin: mercapto group of mercapto silicone resin in the silicone resin is (1-3):(0.4-3):(1-3); the viscosity of the mercapto silicone resin at 25°C is 20000-30000 mPa·s, and the refractive index is 1.5600-1.5750.

6. The dual-curable LED packaging adhesive according to claim 3, characterized in that: The viscosity of the phenyl vinyl silicone oil at 25° C. is 5000-8000 mPa·s; the mass content of phenyl in the phenyl vinyl silicone oil and the phenyl vinyl silicone resin is greater than 45%.

7. The dual-curable LED packaging adhesive according to claim 1 or 2, characterized in that: The phenyl hydrogen-containing silicone oil in the B component is a capped structure; the viscosity of the phenyl hydrogen-containing silicone oil at 25° C. is 5000-8000 mPa·s.

8. The dual-curable LED packaging adhesive according to claim 1 or 2, characterized in that: In the B component, the hydrogen-containing silicone resin is a phenyl hydrogen-containing silicone resin; the refractive index of the hydrogen-containing silicone resin is 1.5400-1.5500, and the hydrogen content is 0.4%-0.7%.

9. The dual-curable LED packaging adhesive according to claim 1 or 2, characterized in that: In the component B, the photoinitiator is one or a combination of dihydroxy dimethyl propiophenone, dihydroxy tetramethoxy benzophenone, and dihydroxy tetra-n-octyloxy benzophenone.

10. The method for preparing the dual-curable LED encapsulation adhesive according to claim 1, characterized in that: The specific steps include: 1) Preparation of component A: Add phenyl vinyl silicone oil, silicone resin, KARSTEDT catalyst and defoamer into a double planetary mixer in sequence, stir at 70-120 rpm for 60-100 min, and disperse at 1500-2500 rpm for 60-100 min. Wait until the stirring and dispersing process is completed, and evacuate until there is no bubble to obtain component A; 2) Preparation of component B: Add phenyl hydrogen silicone oil, hydrogen silicone resin and photoinitiator into a double planetary mixer in sequence, stir at 70-120 rpm for 50-100 min, and disperse at 1500-2500 rpm for 50-100 min, wait for the stirring and dispersing process to end, and evacuate until there is no bubble, thereby obtaining component B; 3) The above-mentioned component A and component B are mixed evenly according to a certain proportion, vacuum degassed, and cured to obtain the LED encapsulation adhesive.

Citation Information

Patent Citations

  • A high-refractive-index, high-toughness, sulfur-resistant LED encapsulation silicone

    CN105176483B

  • A type of high-power LED encapsulating adhesive

    CN107841284B