Fluorescent material as well as preparation and application thereof

By preparing the combination of bridge organosilane with a specific structure and fluorescent indicator, the problems of poor light stability and long response time of fluorescent materials are solved, and fluorescent materials with high sensitivity and short response time are realized, suitable for real-time detection of dissolved oxygen in water. .

CN118931524APending Publication Date: 2024-11-12CHINA AGRI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310523173.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing fluorescent materials have poor light stability, low sensitivity and long response time, which cannot meet the real-time detection needs of dissolved oxygen in water.

Method used

By preparing the combination of bridge organosilanes of specific structures and fluorescent indicators, a fluorescent material with richer network structure and stronger adsorption power is formed, which improves the light stability and response speed of the material.

Benefits of technology

It realizes high sensitivity, short response time and better light stability of fluorescent materials, and is suitable for long-term detection of dissolved oxygen in water, improving detection efficiency and convenience of equipment maintenance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931524A_ABST
    Figure CN118931524A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of new materials, and particularly provides a fluorescent material and preparation and application thereof, the fluorescent material comprises bridge type organosilane and a fluorescent indicator adsorbed by the bridge type organosilane; the bridge type organosilane is obtained by enabling tetraethoxysilane, bridge type alkane and 3, 3, 3-trifluoropropyltrimethoxysilane to react under an acidic condition, and the bridge type organosilane is obtained by enabling the tetraethoxysilane, the bridge type alkane and the 3, 3, 3-trifluoropropyltrimethoxysilane to react under the acidic condition; the bridge alkane comprises more than one of bis (triethoxy phenyl) methane, bis (triethoxy phenyl) ethane, bis (triethoxy phenyl) propane, bis (triethoxy phenyl) hexane, bis (triethoxy phenyl) benzene and bis (triethoxy phenyl) octane. By preparing the bridge type organosilane with a specific structure, stable and efficient adsorption of the fluorescent indicator is realized, the fluorescent material with good light stability, high sensitivity and short response time is obtained, and the fluorescent material is particularly suitable for testing the content of dissolved oxygen.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new materials, and in particular to a fluorescent material and a preparation and application thereof. Background Art

[0002] Dissolved oxygen refers to oxygen in the water in a molecular state, and its main source is oxygen molecules in the air that diffuse into the water. Studies have shown that the dissolved oxygen content in aquaculture water is positively correlated with the growth rate of fish. Appropriate dissolved oxygen concentration can promote the growth of organisms, shorten the breeding cycle, and improve the economic benefits of production, so the monitoring of dissolved oxygen is very necessary.

[0003] At present, there are two main methods for detecting dissolved oxygen: iodine titration and chemical method. However, the iodine titration method is complicated to operate, and the detection results are lagging, which cannot achieve real-time detection of environmental water bodies. The electrochemical method detects the dissolved oxygen content by the current generated by the redox reaction of oxygen on the electrode. There are problems such as easy damage to the membrane, frequent replacement of electrolyte and complicated maintenance process. Compared with the above two methods, the dissolved oxygen sensor based on the principle of fluorescence quenching has a fast response speed and does not consume oxygen during the measurement process. It has a long service life and convenient equipment maintenance, which is very suitable for long-term detection of dissolved oxygen in water.

[0004] Fluorescent material is one of the core components of fluorescence quenching dissolved oxygen sensors, which has a key impact on the measurement effect of optical dissolved oxygen sensors prepared based on fluorescence method. However, fluorescent materials prepared by current technology generally have problems such as large individual differences, poor reproducibility, low sensitivity and long response time.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The present invention provides a fluorescent material and its preparation and application, which are used to solve the defects of the fluorescent materials in the prior art, such as poor photostability, low sensitivity and long response time. By preparing a bridge-type organosilane with a specific structure, stable and efficient adsorption of a fluorescent indicator is achieved, thereby obtaining a fluorescent material with good photostability, high sensitivity and short response time.

[0007] Specifically, the present invention provides a fluorescent material, including: a bridged organic silane and a fluorescent indicator adsorbed thereon;

[0008] The bridged organic silane is obtained by reacting ethyl orthosilicate, a bridged alkane and 3,3,3-trifluoropropyltrimethoxysilane under acidic conditions; the bridged alkane includes one or more of bis(triethoxyphenyl)methane, bis(triethoxyphenyl)ethane, bis(triethoxyphenyl)propane, bis(trimethoxyphenyl)hexane, bis(triethoxyphenyl)benzene and bis(triethoxyphenyl)octane.

[0009] The present invention prepares a bridged organosilane with a specific structure by adding the bridged alkane to a precursor composed of ethyl orthosilicate and 3,3,3-trifluoropropyltrimethoxysilane. Due to the introduction of the bridged alkane, the bridged organosilane has a silicon dioxide network with a richer network structure and a more controllable pore size gap, has better screening properties for dissolved oxygen molecules in water, and makes the adsorption force between the bridged organosilane and the fluorescent indicator stronger, and the intermolecular bonding is more stable. It is unexpectedly found that the bridged organosilane can also enhance the fluorescence performance of the fluorescent indicator, so that the obtained fluorescent material has higher sensitivity and shorter response time.

[0010] According to the fluorescent material provided by the present invention, the molar ratio of tetraethyl orthosilicate, bridged alkane and 3,3,3-trifluoropropyltrimethoxysilane is 5-1:5-1:1-6, such as the molar ratio is 5:5:2, 2:1:1, 1:1:1, 1:1:2, 1:1:4 or 1:1:6.

[0011] According to the fluorescent material provided by the present invention, the fluorescent indicator is one or more of tris(4,7-diphenyl-1,10-phenanthroline)ruthenium dichloride, octaethylporphyrin platinum and pentafluorophenylporphyrin platinum. Considering that the price of porphyrin platinum fluorescent indicators is relatively expensive, which is not conducive to the promotion and application in the fishery field, tris(4,7-diphenyl-1,10-phenanthroline)ruthenium dichloride is preferred.

[0012] According to the fluorescent material provided by the present invention, the bridge-type organic silane and the fluorescent indicator are located on a layer structure formed by sintering ethyl orthosilicate and tetrabutoxy zirconium sol.

[0013] It was found in the experiment that when the above-mentioned bridged organic silane and the said fluorescent indicator are located on the above-mentioned layer structure, the prepared fluorescent film has a better fluorescent indicator loading amount. Preferably, the thickness of the said layer structure is 2.0-3.5 μm.

[0014] According to the fluorescent material provided by the present invention, the layer structure is located on a substrate formed by sintering α-aluminum oxide particles.

[0015] It is found through experiments that the α-alumina particles in the present invention can make the precursor solution adsorbed on the surface of the glass slide better.

[0016] The present invention also provides a method for preparing the fluorescent material as described above, comprising:

[0017] reacting ethyl orthosilicate, a bridged alkane and 3,3,3-trifluoropropyltrimethoxysilane under acidic conditions to obtain the bridged organosilane;

[0018] A fluorescent indicator is added to the solution of the bridged organosilane.

[0019] The method for preparing the fluorescent material provided by the present invention further comprises: thoroughly mixing tetraethyl orthosilicate, bridged alkane, 3,3,3-trifluoropropyltrimethoxysilane and anhydrous ethanol at room temperature to obtain a first reaction liquid;

[0020] The first reaction solution is adjusted to be acidic, and reacted to obtain a second reaction solution. Preferably, the reaction temperature is 15-20° C., and the reaction time is 60-90 min.

[0021] For example, the second reaction liquid is obtained by adding an acidic solution to the first reaction liquid; preferably, the acidic solution is one or more of nitric acid, sulfuric acid, acetic acid, phosphoric acid, hydrofluoric acid and hydrochloric acid.

[0022] The method for preparing the fluorescent material provided by the present invention further comprises:

[0023] The second reaction liquid is mixed with a surfactant to obtain a third reaction liquid; preferably, the surfactant is Triton X-100. It is found in experiments that when Triton X-100 is used as the surfactant, the stability of the obtained fluorescent material is better;

[0024] The third reaction liquid is mixed with the fluorescent indicator to obtain a fourth reaction liquid; preferably, the third reaction liquid is mixed with the fluorescent indicator under ultrasonic conditions for more than 15 minutes, and more preferably, the ultrasonic time is 15 to 35 minutes, and the temperature of the system during the mixing is 10 to 35°C.

[0025] The fourth reaction liquid is gelled in a light-proof condition to obtain a hybrid derivative silica gel. For example, the fourth reaction liquid is placed in a light-proof condition and dried and aged at room temperature for a certain period of time (within 24 hours).

[0026] It was found in the experiment that when the sol-gel method was used and bridge-type organosilane was introduced, the stability of the fluorescent material obtained was better.

[0027] The method for preparing the fluorescent material provided by the present invention further comprises:

[0028] Coating a silicon-zirconia colloidal sol as a binder on a substrate to obtain a first carrier;

[0029] Coating α-alumina particles (e.g., particles with an average particle size of 0.2 μm and 3.0 μm in a mass ratio of 1:1) on the first carrier, and sintering to obtain a second carrier; preferably, the sintering temperature is 400 to 550° C., and the sintering time is 14 to 45 minutes;

[0030] Coating tetraethyl orthosilicate and tetrabutoxy zirconium sol on the second carrier, and firing to obtain a third carrier, which is used to obtain the layer structure with nanopore size; preferably, the firing temperature is 350-550° C., and the firing time is 5-25 min;

[0031] The hybrid derivative silica gel is coated on the third carrier and calcined in a light-proof environment to obtain the fluorescent material. In the experiment, this process can be repeated several times (such as 2 to 4 times) to obtain a fluorescent material with better performance and more stability. Preferably, the calcination temperature is 50 to 350°C.

[0032] The present invention also provides an application of the fluorescent material as described above, including the fluorescent material as described above. Preferably, the fluorescent material is applied in the form of a fluorescent film. Further preferably, the fluorescent film is placed in a sensor for testing the dissolved oxygen content.

[0033] The fluorescent material provided by the present invention achieves stable and efficient adsorption of the fluorescent indicator by preparing a bridge-type organosilane of a specific structure, thereby obtaining a fluorescent material with good light stability, high sensitivity and short response time. Moreover, when it is in the form of a fluorescent film, it is also found that the air permeability and film stability of the fluorescent film are significantly improved. Compared with traditional fluorescent materials, the film is less prone to cracks. The fluorescent material provided by the present invention has high sensitivity and fast response to dissolved oxygen testing, and is suitable for use as a fluorescent material for dissolved oxygen testing. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 It is a spectrum diagram of the fluorescent film prepared in Example 1 provided by the present invention when the dissolved oxygen content is 0% and 100%; wherein, the dissolved oxygen content in environment A is 0, and the dissolved oxygen content in environment B is 100%;

[0036] Figure 2 It is a spectrum diagram of the fluorescent film prepared in Comparative Example 1 provided by the present invention when the dissolved oxygen content is 0% and 100%; wherein, the dissolved oxygen content in environment A is 0%, and the dissolved oxygen content in environment B is 100%;

[0037] Figure 3 It is a spectrum diagram of the fluorescent film prepared in Comparative Example 2 provided by the present invention when the dissolved oxygen content is 0% and 100%; wherein, the dissolved oxygen content of environment A is 0%, and the dissolved oxygen content of environment B is 100%. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Combine the following Figure 1-Figure 3 The fluorescent material of the present invention and its preparation and application are described.

[0040] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.

[0041] Example 1

[0042] A method for preparing a fluorescent film, comprising the following steps:

[0043] (1) 0.792 ml of ethyl orthosilicate was added to a beaker, and mixed thoroughly with 0.732 ml of 3,3,3-trifluoropropyltrimethoxysilane, 1.241 ml of bis(triethoxyphenyl)methane and 1.50 ml of anhydrous ethanol, and allowed to stand for 30 minutes. Then, 1.0 ml of 1 mol / L hydrochloric acid was added as a catalyst. After being sealed with plastic wrap and magnetically stirred for 1 hour, 0.15 ml of a surfactant, Triton X-100, was added. After continuing to stir for 1 hour, 1.0 ml of tris(4,7-biphenyl-1,10-phenanthroline) dichlororuthenium ethanol solution (the concentration of tris(4,7-biphenyl-1,10-phenanthroline) dichlororuthenium was added (the concentration of tris(4,7-biphenyl-1,10-phenanthroline) dichlororuthenium was 0.0035 mol / ml), and ultrasonically stirred for 15 minutes. The mixture was placed in a dark environment and aged at room temperature for 2 hours to obtain a hybrid derivative silica gel.

[0044] (2) Using silica-zirconia colloidal sol as a binder, α-alumina particles (using an average particle size of 0.2 μm and 3.0 μm in a compounded manner in a mass ratio of 1:1) are coated on the surface of a glass slide, and sintered at 550°C for 30 minutes to form a smooth surface; further, ethyl orthosilicate and tetrabutoxy zirconium sol (0.5 wt%) in a volume ratio of 1:1 are coated on the smooth surface in an amount of 0.1 ml. After coating, the surface is sintered at 550°C for 15 minutes to form a nanopore intermediate layer.

[0045] (3) The hybrid derivative silica gel obtained in step (1) is spin-coated on the intermediate layer obtained in step (2) using a coating machine, with a coating amount of 0.25 ml, and the fluorescent film is calcined at 300° C. in a light-proof environment.

[0046] Repeat step (3) 4 times to obtain a dissolved oxygen fluorescent film.

[0047] Example 2

[0048] A method for preparing a fluorescent film, wherein the steps are substantially the same as those of Example 1, except that step (1) is:

[0049] (1) Add 0.792 ml of ethyl orthosilicate into a beaker, mix thoroughly with 0.732 ml of 3,3,3-trifluoropropyltrimethoxysilane, 1.543 ml of bis(triethoxyphenyl)methane and 1.50 ml of anhydrous ethanol, let stand for 30 minutes, then add 1.0 ml of 1 mol / L hydrochloric acid as a catalyst. Cover with plastic wrap and seal, stir magnetically for 1 hour, then add 0.15 ml of surfactant Triton X-100, continue stirring for 1 hour, then add 1.0 ml of tris(4,7-biphenyl-1,10-phenanthroline) dichlororuthenium ethanol solution, stir ultrasonically for 15 minutes, and age at room temperature in a dark environment for 8 hours.

[0050] Example 3

[0051] A method for preparing a fluorescent film, wherein the steps are substantially the same as those of Example 1, except that the aging time in step (1) is 20 hours.

[0052] Example 4

[0053] A method for preparing a fluorescent film, comprising the following steps:

[0054] (1) 1.584 ml of ethyl orthosilicate was added to a beaker, and mixed thoroughly with 0.732 ml of 3,3,3-trifluoropropyltrimethoxysilane, 2.482 ml of bis(triethoxyphenyl)methane and 1.50 ml of anhydrous ethanol. The mixture was allowed to stand for 30 minutes, and then 1.0 ml of 1 mol / L hydrochloric acid was added as a catalyst. After being sealed with plastic wrap and magnetically stirred for 1 hour, 0.15 ml of surfactant Triton X-100 was added. After continuing to stir for 1 hour, 1.0 ml of tris(4,7-biphenyl-1,10-phenanthroline) ruthenium dichloride ethanol solution (the concentration of tris(4,7-biphenyl-1,10-phenanthroline) ruthenium dichloride was added (the concentration of tris(4,7-biphenyl-1,10-phenanthroline) ruthenium dichloride was 0.0035 mol / ml), and ultrasonically stirred for 15 minutes. The mixture was placed in a dark environment and aged at room temperature for 5 hours.

[0055] (2) Using silica-zirconia colloidal sol as a binder, α-alumina particles (using a compounding method of average particle size of 0.2 μm and 3.0 μm in a mass ratio of 1:1) were coated on the surface of a glass slide, and sintered at 400°C for 30 minutes to form a smooth surface. Further, ethyl orthosilicate and tetrabutoxy zirconium sol (0.5wt%) in a volume ratio of 1:1 were coated on the smooth surface, and the coating amount was 0.1 ml. After coating, it was sintered at 400°C for 15 minutes to form a nanopore intermediate layer.

[0056] (3) The hybrid derivative silica gel obtained in step (1) is spin-coated on the intermediate layer obtained in step (2) using a coating machine, with a coating amount of 0.25 ml. The fluorescent film is calcined at 150° C. in a light-proof environment. The coating is repeated 4 times to obtain a dissolved oxygen fluorescent film.

[0057] Example 5

[0058] A method for preparing a fluorescent film, wherein the steps are substantially the same as those of Example 1, except that 2.482 ml of bis(triethoxyphenyl)methane in step (1) is replaced by 3.104 ml of bis(triethoxyphenyl)ethane.

[0059] Comparative Example 1

[0060] A method for preparing a fluorescent film, wherein the steps are substantially the same as those of Example 1, except that in step (1), 3,3,3-trifluoropropyltrimethoxysilane and bis(triethoxyphenyl)methane are replaced by ethyl orthosilicate in equal amounts.

[0061] Comparative Example 2

[0062] A method for preparing a fluorescent film, wherein the steps are substantially the same as those of Example 1, except that in step (1), an equal amount of 3,3,3-trifluoropropyltrimethoxysilane is replaced by ethyl orthosilicate.

[0063] The fluorescent films prepared in Examples 1 to 5 and Comparative Examples 1 to 2 were tested, and the test method was as follows:

[0064] Sensitivity: refers to the fluorescence intensity I0 of the fluorescent film when the oxygen content in the mixed gas is 0% and the fluorescence intensity I0 when the oxygen content in the mixed gas is 100%. 100 The larger the value, the better the sensitivity of the dissolved oxygen fluorescence membrane. The calculation formula is as follows:

[0065] Sensitivity = I0 / I 100 .

[0066] Attenuation: In order to analyze the attenuation of the fluorescent film, the prepared fluorescent film was placed in water for 1 hour, and its maximum fluorescence intensity I1 was measured by a fluorescence spectrophotometer. Then, it was placed in water for 1 hour under light-proof conditions, and then its maximum fluorescence intensity I2 was tested. That is, the change in the maximum fluorescence intensity of the fluorescent film before and after placement was observed by a fluorescence spectrophotometer to determine its stability. The lower the attenuation in the experiment, the better the photostability. The calculation formula is as follows:

[0067] Attenuation degree = (I1-I2) / I1×100%.

[0068] Maximum fluorescence intensity: In this experiment, a fluorescence spectrometer was used to detect the prepared fluorescent film and the maximum fluorescence intensity in the wavelength range of 415 to 430 nm was recorded.

[0069] The test results are as follows:

[0070]

[0071]

[0072] The spectra of the fluorescent films prepared in Example 1 and Comparative Examples 1 to 2 when the dissolved oxygen content is 0 and 100% are as follows: Figures 1 to 3 shown.

[0073] The experiment also found that the aging time will affect the performance of the fluorescent film. If the aging time is too long, the sensitivity of the fluorescent film will decrease, the attenuation will increase, and even cause defects such as cracking of the film. Moreover, compared with other bridged alkanes, the fluorescent film made of bis(triethoxyphenyl)methane has better effect.

[0074] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A fluorescent material, characterized in that: include: Bridged organosilane and fluorescent indicator adsorbed thereon; The bridged organic silane is obtained by reacting ethyl orthosilicate, a bridged alkane and 3,3,3-trifluoropropyltrimethoxysilane under acidic conditions; the bridged alkane includes one or more of bis(triethoxyphenyl)methane, bis(triethoxyphenyl)ethane, bis(triethoxyphenyl)propane, bis(trimethoxyphenyl)hexane, bis(triethoxyphenyl)benzene and bis(triethoxyphenyl)octane.

2. The fluorescent material according to claim 1, characterized in that The molar ratio of the tetraethyl orthosilicate, the bridged alkane and the 3,3,3-trifluoropropyltrimethoxysilane is 5-1:5-1:1-6.

3. The fluorescent material according to claim 1 or 2, characterized in that: The fluorescent indicator is one or more of tris(4,7-diphenyl-1,10-phenanthroline)ruthenium dichloride, octaethylporphyrin platinum and pentafluorophenylporphyrin platinum.

4. The fluorescent material according to any one of claims 1 to 3, characterized in that The bridge-type organic silane and the fluorescent indicator are located on a layer structure formed by sintering ethyl orthosilicate and tetrabutoxy zirconium sol.

5. The fluorescent material according to claim 4, characterized in that The layer structure is formed by sintering α-aluminum oxide particles.

6. The method for preparing the fluorescent material according to any one of claims 1 to 5, characterized in that: include: reacting ethyl orthosilicate, a bridged alkane and 3,3,3-trifluoropropyltrimethoxysilane under acidic conditions to obtain the bridged organosilane; A fluorescent indicator is added to the solution of the bridged organosilane.

7. The method for preparing the fluorescent material according to claim 6, characterized in that: Also includes: Thoroughly mixing tetraethyl orthosilicate, bridged alkane, 3,3,3-trifluoropropyltrimethoxysilane and anhydrous ethanol at room temperature to obtain a first reaction solution; The first reaction solution is adjusted to be acidic, and reacted to obtain a second reaction solution.

8. The method for preparing the fluorescent material according to claim 7, characterized in that: Also includes: Mixing the second reaction liquid with a surfactant to obtain a third reaction liquid; preferably, the surfactant is Triton X-100; Mixing the third reaction solution with the fluorescent indicator to obtain a fourth reaction solution; The fourth reaction solution is gelled under light-proof conditions to obtain hybrid derivative silica gel.

9. The method for preparing a fluorescent material according to claim 8, characterized in that: Also includes: Coating a silicon-zirconia colloidal sol as a binder on a substrate to obtain a first carrier; coating α-alumina particles on the first carrier, and sintering to obtain a second carrier; coating the second carrier with tetraethyl orthosilicate and tetrabutoxy zirconium sol, and firing the carrier to obtain a third carrier; The hybrid derivative silica gel is coated on the third carrier and calcined in a light-proof environment to obtain the fluorescent material.

10. An application of a fluorescent material, characterized in that: It comprises the fluorescent material according to any one of claims 1 to 5; preferably, the fluorescent material is applied in the form of a fluorescent film; further preferably, the fluorescent film is placed in a sensor for testing the content of dissolved oxygen.