Self-doped long afterglow crystal material with same-type structure as well as preparation method and application of self-doped long afterglow crystal material
Through the self-doped long afterglow crystal material of the same type of structure, the evaporation crystallization method of carbazole derivatives and N-methylcarbazole is solved, and the problem of difficulty in observing long afterglow in room temperature and atmospheric environment is achieved. The yellow afterglow luminescence improves the material's afterglow time and color performance, and is suitable for information encryption and anti-counterfeiting.
Patent Information
- Application Number
- CN202411001351.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult to observe the long afterglow luminescence phenomenon in existing organic long afterglow materials in room temperature and atmospheric environments, and most materials emit green afterglow, and there are very few afterglow materials in other colors, which limits their application in the fields of information encryption and anti-counterfeiting.
Using a long afterglow crystal material with a self-doped structure of the same type, the carbazole derivatives of a specific structure are evaporated and crystallized by evaporating and crystallization with N-methylcarbazole as the main material to construct a regular crystal structure, which promotes singlet state and three-wire The generation of state excitons delays fluorescence and phosphorescence, and achieves yellow afterglow emission.
The material with a afterglow time of more than 4 seconds and a yellow afterglow color is obtained under aerobic conditions in room temperature, has good yellow afterglow luminescence performance, and is suitable for applications in the fields of information encryption and anti-counterfeiting.
Smart Images

Figure CN118931529A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic afterglow crystal materials, and in particular to self-doped long afterglow crystal materials of the same type of structure and a preparation method and application thereof. Background Art
[0002] Due to the unique advantages of long lifetime and large Stokes shift, organic room temperature phosphorescent (RTP) materials have attracted extensive attention in many research fields such as anti-counterfeiting, bio-imaging, sensors and electronic devices. Compared with inorganic materials, organic molecules have better biocompatibility, easier structure modification, and are free from the constraints of rare earth elements, which is of great research significance.
[0003] However, due to the inherent spin-forbidden ISC and non-radiative transitions of triplet excitons, efficient and long-lasting RTP emission from metal-free pure organic materials is difficult to achieve. This is mainly because the lowest excited triplet exciton (T1) of organic molecules returns to the ground state (S0) through radiative transitions to produce phosphorescence, but the long afterglow luminescence of organic molecules can usually only be observed at low temperatures (77K) or inert atmospheres, and it is difficult to observe the long afterglow luminescence phenomenon under room temperature oxygen conditions because the triplet excitons of organic molecules are easily quenched by oxygen molecules in the air. At the same time, the vibration of organic molecules is strong under room temperature atmospheric conditions, resulting in a high non-radiative transition rate (Knr), and the energy is mainly consumed in the form of heat. Therefore, it is difficult to observe the long afterglow luminescence phenomenon of pure organic molecules under room temperature atmospheric conditions.
[0004] At present, how to obtain room temperature phosphorescence and obtain room temperature long afterglow phenomenon can be achieved mainly through two means: 1) Promote the spin-orbit coupling (SOC) of molecules to promote the intersystem crossing (ISC) process from the excited singlet state to the excited triplet state of molecules; 2) Inhibit the non-radiative transition of molecules so that more energy is released in the form of light energy. This has led researchers to develop crystal engineering, heavy atom effect, H-aggregation, host-guest doping, introduction of polymer matrix and some other methods to prepare pure organic long afterglow materials with excellent luminescence performance in atmospheric environment. Among these methods for preparing pure organic long afterglow materials, crystal engineering is the most commonly used one by researchers, because through crystallization, the rigidity of the molecular structure can be increased, the non-radiative transition of molecules can be effectively compressed, and it can also play a role in isolating oxygen, thereby obtaining pure organic long afterglow luminescent materials. However, since most of the organic long afterglow crystal materials currently constructed have large conjugated structures and aggregated luminescence, the afterglow emitted by most crystal materials is green, and there are very few crystal materials that can emit afterglow of other colors.
[0005] Therefore, developing more afterglow materials with other colors is the key to realizing the full-spectrum afterglow characteristics of organic long afterglow materials. It is also expected to achieve specific RTP performance on demand for better application in information encryption, afterglow anti-counterfeiting and other fields. Summary of the invention
[0006] Based on the above problems, one of the objects of the present invention is to provide a long afterglow crystal material with a self-doped structure of the same type, which uses the same type of carbazole derivatives as host and guest materials for co-doping. The obtained crystal material has good afterglow luminescence performance under room temperature and aerobic conditions, a long afterglow life and a yellow afterglow color, which is conducive to the full-spectrum afterglow characteristics of the long afterglow material.
[0007] The second object of the present invention is to provide a method for preparing the self-doped long afterglow crystal material of the same type of structure, which uses the same type of host material and guest material with simple structure, low cost and easy to obtain to prepare the crystal material, and the preparation method is simple, the conditions are mild and do not require harsh conditions such as high temperature and high pressure. At the same time, the prepared material has a regular crystal morphology and good afterglow luminescence performance, and is suitable for industrial application.
[0008] The third object of the present invention is to provide the application of the self-doped long afterglow crystal material of the same type of structure as above.
[0009] The purpose of the present invention is achieved by the following technical solutions:
[0010] A self-doped long afterglow crystal material with the same type of structure is prepared by evaporating and crystallizing a main material and a guest material; in the self-doped long afterglow crystal material with the same type of structure, the main material forms regular crystals, and the guest material is freely dispersed in the crystals of the main material;
[0011] The main material is The guest material is
[0012] When constructing the crystal structure, the present invention selects two carbazole derivatives of specific structures (tetramethyl-9H-carbazole-3,6-diamine or 5,9-dibromo-7H-dibenzo[c,g]carbazole) as guest materials, and uses N-methylcarbazole as the host material to construct a new type of self-doping system of the same type, which has obvious technical advantages in realizing pure organic long afterglow crystal structure. First, the guest material has a similar molecular structure to the host material, and the introduction of the guest will not significantly change the lattice structure of the host molecule, maintaining the high quantum efficiency characteristics of the carbazole molecular system; second, the charge separation between the host and the guest material can promote the generation of singlet and triplet excitons, which are then transmitted to the guest molecule and cause delayed fluorescence and phosphorescence through radiation transition. The present invention constructs a structurally regular crystalline material through the above-mentioned same type of self-doping strategy, and obtains a new long afterglow luminescent material with adjustable time. The afterglow time of this material exceeds 4s, and the afterglow color is yellow. It has good yellow afterglow luminescent performance, demonstrating its application potential in the fields of information encryption and anti-counterfeiting, and is also conducive to the full-spectrum afterglow characteristics of the long afterglow material.
[0013] More preferably, the mass ratio of the host material to the guest material is (80-120):1, more preferably 100:1.
[0014] Further preferably, the excitation wavelength of the self-doped long afterglow crystal material of the same type of structure is 360-380 nm, more preferably 365 nm.
[0015] A method for preparing a self-doped long afterglow crystal material of the same type of structure comprises the following steps:
[0016] (1) mixing the host material and the guest material uniformly to obtain a solid powder;
[0017] (2) The solid powder is stirred and dissolved in a solvent, and then allowed to stand for volatilization to precipitate crystals, thereby obtaining the self-doped long afterglow crystal material of the same type of structure.
[0018] When preparing the crystal material, the present invention uses a simple evaporation crystal mixing method to dope a small amount of specific carbazole derivatives as guest materials into the main material formed by N-methylcarbazole, thereby successfully constructing a new type of crystal afterglow material, which can be excited by ultraviolet light and can effectively enhance the afterglow time of the crystal material and adjust the afterglow color to yellow, which can effectively support the high-efficiency long afterglow luminescence application of organic crystalline long afterglow materials.
[0019] Further preferably, in step (2), the solvent is dichloromethane and ethanol; the volume ratio of dichloromethane to ethanol is 1:(80-120).
[0020] Further preferably, in step (2), after stirring and dissolving, the concentration of the solid powder in the solvent is 18 to 25 mg / mL.
[0021] Further preferably, in step (2), the stirring and dissolving is performed at a speed of 500 to 1000 rpm and for a time of 3 to 10 min.
[0022] More preferably, in step (2), the temperature for standing and volatilizing is 15 to 30°C.
[0023] More preferably, after the crystals are precipitated in step (2), the method further includes centrifuging the solution after the crystals are precipitated, and washing and drying the obtained crystals after centrifugation.
[0024] The application of the self-doped long afterglow crystal material of the same type of structure as mentioned above is specifically the application as a luminescent material in data encryption materials or afterglow anti-counterfeiting materials.
[0025] The self-doped long afterglow crystal material of the same type of structure provided by the present invention is successfully prepared by the simplest host-guest material with similar structure mixed crystallization to obtain an afterglow material capable of presenting yellow luminescence, which can be excited by ultraviolet light, has the characteristics of environmental stability under room temperature and oxygen environment, can form a regular crystal morphology, has an afterglow time of more than 4s, and has a yellow afterglow color, and has better performance than conventional crystal afterglow materials. Therefore, the long afterglow crystal material provided by the present invention can provide new ideas for designing and synthesizing new crystal materials with yellow long afterglow luminescence, and can also provide a theoretical basis and more crystal structure options for practical applications such as data encryption and afterglow anti-counterfeiting. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solution of the present invention, the following briefly introduces the drawings required for describing the embodiments and test examples;
[0027] Figure 1 The optical images of the afterglow display of the self-doped long afterglow crystal material of the same type of structure obtained in Example 1 of the present invention before (a) and after (bf) irradiation with 365nm ultraviolet light;
[0028] Figure 2 The optical images of the afterglow display of the self-doped long afterglow crystal material of the same type of structure obtained in Example 2 of the present invention before (a) and after (bf) irradiation with 365nm ultraviolet light;
[0029] Figure 3 This is an optical image of the afterglow display of the crystal material obtained in Comparative Example 1 after being illuminated by 365nm ultraviolet light (ad). DETAILED DESCRIPTION
[0030] The technical scheme and technical effects of the present invention will be clearly and completely described below in conjunction with specific embodiments and accompanying drawings. However, it should be understood by those skilled in the art that the embodiments are only used to illustrate the technical scheme of the present invention and should not be regarded as limiting the scope of protection of the present invention. Based on the following embodiments, all other implementation schemes obtained by ordinary technicians in the field without making creative work, such as modification, deformation or simple replacement, should belong to the scope of protection of the present invention.
[0031] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the raw materials used are all commonly used in the art, available to the public or commercially available, unless otherwise specified; the terms and abbreviations involved have the conventional meanings in the art.
[0032] Example 1
[0033] The self-doped long afterglow crystal material of the same type of structure provided in this embodiment is prepared by using a main material and a guest material through an evaporation crystallization method; in the long afterglow crystal material, the main material forms regular crystals, and the guest material is freely dispersed in the crystals of the main material; the structural formula of the main material is: (N-methylcarbazole); the structural formula of the guest material is: (5,9-dibromo-7H-dibenzo[c,g]carbazole).
[0034] The preparation method of the above-mentioned host-guest type organic long afterglow crystal material comprises the following steps:
[0035] According to the mass ratio of the host material to the guest material of 100:1; accurately weigh 0.0010 g of the guest material (5,9-dibromo-7H-dibenzo[c,g]carbazole) and 0.1000 g of the host material (N-methylcarbazole) and mix them to obtain a solid powder;
[0036] Add 0.05 mL of dichloromethane to the solid powder and dissolve it for 1 min, then add 5 mL of ethanol, stir at room temperature (20-25°C) and 600 rpm for 5 min until it is completely dissolved, then place it in an atmospheric environment at room temperature of 20-25°C to evaporate slowly until crystals precipitate. After the crystals precipitate, centrifuge the solution containing the crystals, wash the crystals with ethanol after centrifugation, and dry them at room temperature (20-25°C) for 3 h to obtain a self-doped long afterglow crystal material with the same structure as Example 1.
[0037] Example 2
[0038] The self-doped long afterglow crystal material of the same type of structure provided in this embodiment is prepared by using a main material and a guest material through an evaporation crystallization method; in the long afterglow crystal material, the main material forms regular crystals, and the guest material is freely dispersed in the crystals of the main material; the structural formula of the main material is: (N-methylcarbazole); the structural formula of the guest material is: (Tetramethyl-9H-carbazole-3,6-diamine).
[0039] The preparation method of the above-mentioned host-guest type organic long afterglow crystal material comprises the following steps:
[0040] According to the mass ratio of the host material to the guest material of 100:1, 0.0010 g of the guest material (tetramethyl-9H-carbazole-3,6-diamine) and 0.1000 g of the host material (N-methylcarbazole) were accurately weighed and mixed to obtain a solid powder;
[0041] Add 0.05 mL of dichloromethane to the solid powder and dissolve it for 1 min, then add 5 mL of ethanol, stir at room temperature (20-25°C) and 600 rpm for 5 min until it is completely dissolved, then place it in an atmospheric environment at room temperature of 20-25°C to slowly evaporate until crystals precipitate. After the crystals precipitate, centrifuge the solution containing the crystals, wash the crystals with ethanol after centrifugation, and dry them at room temperature (20-25°C) for 3 h to obtain a self-doped long afterglow crystal material with the same structure as Example 2.
[0042] Comparative Example 1
[0043] This comparative example provides a crystalline material, and its preparation process is carried out with reference to Example 1. The only difference from Example 1 is that the structure of the main material used is different, and the other conditions are the same as Example 1. The main material used in this comparative example is
[0044]
[0045] Test Example 1: Performance test of the material in Example 1
[0046] Under room temperature and atmospheric conditions, a 365nm ultraviolet lamp was used to excite the long afterglow crystal material of Example 1, and then the excitation light source was turned off, and the afterglow brightness change of the crystal material after the light source was removed was recorded. The results are as follows: Figure 1 shown.
[0047] Depend on Figure 1 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Example 1 ( Figure 1 a), turn off the excitation light source. After removing the light source, the crystal material emits a yellow afterglow ( Figure 1 b) In the first 3 seconds, Figure 1b~1d represent the 1s, 2s, and 3s after the light source is removed. During this time, the afterglow brightness of the crystal material is strong. From 3.5s (such as Figure 1 e) and then the afterglow gradually weakened. At 4.1s ( Figure 1 f) After that, the afterglow is still not obvious. It can be seen that the afterglow time of the crystal material of Example 1 is as high as 4.1s, and the afterglow performance is excellent.
[0048] Test Example 2: Performance Test of Material in Example 2
[0049] Under room temperature and atmospheric conditions, a 365nm ultraviolet lamp was used to excite the long afterglow crystal material of Example 2, and then the excitation light source was turned off, and the afterglow brightness change of the crystal material after the light source was removed was recorded. The results are as follows: Figure 2 shown.
[0050] Depend on Figure 2 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Example 2 ( Figure 2 a), turn off the excitation light source. After removing the light source, the crystal material emits a yellow afterglow ( Figure 2 b) In the first 3 seconds, Figure 2 b~2d represent the 1st, 2nd, and 3rd seconds after the light source is removed. During this time, the afterglow brightness of the crystal material is strong. From the 4th second (such as Figure 2 e) and then the afterglow gradually weakened, and at 4.5s ( Figure 2 f) The afterglow is not obvious. It can be seen that the afterglow time of the crystal material of Example 2 is as high as 4.5s, and the afterglow performance is excellent.
[0051] Test Example 3: Performance test of materials in Comparative Example 1
[0052] Under room temperature and atmospheric conditions, the crystal material of Comparative Example 1 was excited by a 365nm ultraviolet lamp, and then the excitation light source was turned off, and the change in the afterglow brightness of the crystal material after the light source was removed was recorded. The results are as follows Figure 3 shown.
[0053] Depend on Figure 3 It can be seen that the 365nm ultraviolet lamp excites the crystal material of Comparative Example 1, and the excitation light source is turned off. After the light source is removed, the crystal material emits a green afterglow ( Figure 3 a), in the first 1s, Figure 3 a~3b represent the 0th and 1st seconds after the light source is removed. During this time, the afterglow brightness of the compound is strong. From 1.5 seconds (such as Figure 3 c) and then the afterglow gradually weakens. Figure 3d) The afterglow is not obvious. It can be seen that the afterglow time of the crystal material of comparative example 1 is only 2s. Analysis shows that the afterglow time of the material of comparative example 1 is not only shorter than that of the long afterglow crystal material of the present invention, but also the afterglow color is the common green. It can be seen that the present invention uses a host-guest material with a similar structure to mix and crystallize, which can effectively improve the afterglow time of the material and adjust the afterglow color to yellow.
[0054] In summary, the self-doped long afterglow crystal material with the same type of structure provided by the present invention has excellent yellow afterglow luminescence performance, which can provide new ideas for the design and synthesis of new yellow luminescent crystal long afterglow materials, and can also provide theoretical basis and material foundation for practical applications such as data encryption and afterglow anti-counterfeiting.
[0055] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A self-doped long afterglow crystal material of the same type of structure, characterized in that: It is prepared by evaporation and crystallization of the main material and the guest material; in the self-doped long afterglow crystal material of the same type of structure, the main material forms regular crystals, and the guest material is freely dispersed in the crystals of the main material; The main material is The guest material is 2. The self-doped long afterglow crystal material of the same type of structure as claimed in claim 1, characterized in that: The mass ratio of the host material to the guest material is (80-120):
1.
3. The self-doped long afterglow crystal material of the same type of structure as claimed in claim 1, characterized in that: The excitation wavelength of the self-doped long afterglow crystal material of the same type of structure is 360-380nm.
4. A method for preparing a self-doped long afterglow crystal material of the same type of structure as claimed in claim 1, characterized in that: The following steps are involved: (1) mixing the host material and the guest material uniformly to obtain a solid powder; (2) The solid powder is stirred and dissolved in a solvent, and then allowed to stand for volatilization to precipitate crystals, thereby obtaining the self-doped long afterglow crystal material of the same type of structure.
5. The method for preparing the self-doped long afterglow crystal material of the same type of structure according to claim 4, characterized in that: In step (2), the solvent is dichloromethane and ethanol; the volume ratio of dichloromethane to ethanol is 1: (80-120).
6. The method for preparing the self-doped long afterglow crystal material of the same type of structure according to claim 4, characterized in that: In step (2), after stirring and dissolving, the concentration of the solid powder in the solvent is 18 to 25 mg / mL.
7. The method for preparing the self-doped long afterglow crystal material of the same type of structure according to claim 4, characterized in that: In step (2), the stirring and dissolving is performed at a speed of 500 to 1000 rpm and for a time of 3 to 10 minutes.
8. The method for preparing the self-doped long afterglow crystal material of the same type of structure according to claim 4, characterized in that: In step (2), the temperature for standing and volatilizing is 15 to 30°C.
9. The method for preparing a self-doped long afterglow crystal material of the same type of structure according to any one of claims 4 to 8, characterized in that: After the crystals are precipitated in step (2), the method further includes centrifuging the solution after the crystals are precipitated, and washing and drying the obtained crystals after centrifugation.
10. An application of the self-doped long afterglow crystal material of the same type of structure as claimed in claim 1, characterized in that: Application as luminescent material in data encryption material or afterglow anti-counterfeiting material.