Terbium-europium double-doped hydroxyapatite luminescent material for fibers as well as preparation method and application of terbium-europium double-doped hydroxyapatite luminescent material
By adjusting the pH in disodium hydrogen phosphate solution and heating reaction in an autoclave, terbium europium double-doped hydroxyapatite was prepared, which solved the problems of complex operation and uneven product morphology in the prior art, and achieved the application of Efficient preparation in the fiber field has expanded the scope of application.
Patent Information
- Application Number
- CN202411108155.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is complex in the preparation of one-dimensional hydroxyapatite luminescent materials, the products are prone to agglomeration, uneven morphology, poor toughness, and cannot be applied to the fiber field. The use of microwave heating limits the application of efficient and convenient reaction devices.
Add sodium hydroxide to the disodium hydrogen phosphate solution to adjust the pH to form a strong alkaline solution, add a mixed solution of calcium chloride, terbium nitrate and europium nitrate dropwise, and carry out a heating reaction in the autoclave to control the reaction temperature and time. Prepare terbium europium double-doped hydroxyapatite, avoiding microwave heating and surfactants, and simplifying operation.
A double-doped hydroxyapatite luminescent material for fibers with uniform morphology and good toughness was obtained. It is suitable for LED and fluorescent anti-counterfeiting/detection fiber fields. It is simple to operate, low cost and high yield, and it expands hydroxyapatite. Application in the fields of fluorescence anti-counterfeiting and semiconductor devices.
Smart Images

Figure CN118931533A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanomaterials, and in particular to a terbium-europium double-doped hydroxyapatite luminescent material for fiber, and a preparation method and application thereof. Background Art
[0002] Hydroxyapatite Ca 10 (PO4)6(OH)2 is not only the most stable crystalline phase in the calcium phosphate structure, but also the main component of human bones and teeth. Due to its excellent biocompatibility, it is often used in biological fields such as bone regeneration, tumor treatment and dental treatment. Synthetic hydroxyapatite has a variety of morphologies due to the diversity of preparation methods, such as nanorods, nanowires, spheres, plates, etc.
[0003] Rare earth elements have the advantages of low toxicity, long fluorescence lifetime, good photostability, etc. Secondly, the radius of rare earth ions is similar to that of calcium ions. By utilizing the anion-cation exchange property of hydroxyapatite, rare earth ions can replace the calcium sites in hydroxyapatite, giving hydroxyapatite new properties.
[0004] Patent CN110423614A discloses a method for preparing a rare earth-doped one-dimensional nano-hydroxyapatite phosphor, wherein a mixed solution containing calcium salt, at least two rare earth metal salts, polyethylene glycol, phosphate (ammonium dihydrogen phosphate) and a surfactant is subjected to a hydrothermal reaction under microwave conditions, and the reaction solution is subjected to solid-liquid separation after the reaction, and dried to obtain a rare earth-doped one-dimensional nano-hydroxyapatite phosphor. However, in the process of preparing one-dimensional hydroxyapatite, the patent uses surfactants, polyethylene glycol and microwave heating assistance, and the operation process is relatively complicated, the experimental process is relatively cumbersome, and it also shows that the reaction products are easy to agglomerate, which is not conducive to the rapid preparation of the corresponding hydroxyapatite luminescent material. During the experiment, under the condition of microwave heating, efficient and convenient reaction devices such as metal reactors cannot be used. At the same time, the one-dimensional hydroxyapatite finally prepared by the patent is mostly long, reaching the micron level, and the morphology is not very uniform, the toughness is poor and it is easy to break, and it cannot be applied to fiber and other fields. The ammonium ions in the ammonium dihydrogen phosphate used in the preparation process are not completely hydrolyzed, and the pH value of the solution cannot be efficiently adjusted. Moreover, it is not easy to remove after the reaction, which objectively leads to the uneven morphology of the prepared one-dimensional hydroxyapatite. Summary of the invention
[0005] In view of the above problems, the present invention provides a terbium-europium dual-doped hydroxyapatite luminescent material for fiber and a preparation method and application thereof.
[0006] The technical solution of the present invention to solve the above technical problems is as follows: A method for preparing a terbium-europium double-doped hydroxyapatite luminescent material for fiber, comprising the following steps: Step 1, adding sodium hydroxide to the disodium hydrogen phosphate solution to adjust the pH of the solution to make the solution strongly alkaline; Step 2: Add a mixed solution of calcium chloride, europium nitrate and tris(III) nitrate dropwise to the strongly alkaline solution obtained in step 1, and stir at 40° C. until the mixture is completely dissolved to obtain a hydroxyapatite precursor solution; Step 3: placing the hydroxyapatite precursor solution obtained in step 2 in an autoclave and heating it to 150-200° C. for reaction; cooling at room temperature after the reaction is completed, centrifugation purification, and drying to obtain terbium-europium dual-doped hydroxyapatite luminescent material for fiber.
[0007] Furthermore, before performing step 1, the preparation method further comprises: Step 1', adding sodium hydroxide to the disodium hydrogen phosphate solution to adjust the pH of the solution to make the solution strongly alkaline; Step 2', adding a mixed solution of calcium chloride and terbium nitrate dropwise to the strongly alkaline solution obtained in step 1', stirring at 40° C. until completely dissolved, to obtain a hydroxyapatite precursor solution; Step 3', placing the hydroxyapatite precursor solution obtained in step 2' in an autoclave and heating it to 150-200°C for reaction, cooling at room temperature after the reaction is completed, centrifugation purification, and drying to obtain terbium mono-doped hydroxyapatite; Step 4', changing the doping concentration of terbium ions within a preset range according to a preset rule, and repeating steps 2' and 3' to determine the optimal doping concentration of terbium ions corresponding to the best luminescence performance of terbium-doped hydroxyapatite; Step 5': determine the relative doping ratio of terbium ions and europium ions according to the luminescence requirement, thereby preparing a terbium nitrate and europium nitrate solution with a required ratio.
[0008] Furthermore, in step 1, the amount of disodium hydrogen phosphate used is 5.372 g.
[0009] Furthermore, in step 2, the amounts of calcium chloride, terbium nitrate and europium nitrate are 0.277 g, 0.075 mmol and 0.020-0.075 mmol, respectively.
[0010] Furthermore, the stirring time in step 2 is 1 h.
[0011] Furthermore, the content of the hydroxyapatite precursor solution obtained in step 2 is 27.5 mL.
[0012] Furthermore, the reaction time in step 3 is 6-12 hours, the solvent required for the centrifugal purification process is deionized water, the centrifugal speed is 5000 rpm, the centrifugal time is 5 minutes, and the number of centrifugation is 3 times.
[0013] A terbium-europium double-doped hydroxyapatite luminescent material for fiber is prepared by any of the methods described above.
[0014] The above-mentioned fiber-used terbium-europium dual-doped hydroxyapatite luminescent material is used in the fields of LED and fluorescent anti-counterfeiting / detection fibers.
[0015] The beneficial effects of the present invention are: 1. The preparation method of the terbium-europium dual-doped hydroxyapatite luminescent material for fiber provided by the present invention is to firstly dope a rare earth terbium ion alone to find the terbium ion single-doped hydroxyapatite luminescent material with the best luminescent performance at the optimal doping concentration; by this method, the doping concentration of the terbium ion is first determined, and then the relative doping ratio of the two rare earths is determined based on this, so as to obtain a hydroxyapatite precursor solution; then the hydroxyapatite precursor solution is placed in an autoclave, and the hydroxyapatite with the best fluorescence performance is prepared by controlling the reaction time and the reaction temperature. Compared with the conventional hydroxyapatite synthesis process, the reaction temperature and reaction time required for the terbium-europium dual-doped hydroxyapatite are significantly changed. In addition, in previous studies, calcium nitrate is often used as a raw material for preparing hydroxyapatite, but calcium nitrate is easy to explode when in contact with organic matter, sulfur, etc. In the present invention, terbium-europium dual-doped hydroxyapatite is prepared using safer calcium chloride. At the same time, the present invention does not require microwave-assisted conditions or surfactants, is simple to operate and has low cost, and the produced products can be fully utilized with high yield.
[0016] 2. The present invention provides a new synthesis route for the study of rare earth doped hydroxyapatite, which is helpful for further exploration of the application of hydroxyapatite. The experimental preparation process is controlled in a closed space, with almost no or only a small amount of solvent volatilization, which reduces atmospheric environmental pollution and is an environmentally friendly synthesis method. In addition, the synthesized hydroxyapatite presents a regular nanorod shape, which is convenient for later compounding with high-performance fibers, light-emitting diodes, etc., and expands the application of hydroxyapatite in the fields of fluorescent anti-counterfeiting and semiconductor devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 A scanning electron microscope (SEM) morphology image of the terbium-europium dual-doped hydroxyapatite provided in Example 1 of the present invention; Figure 2 Related drawings provided for Example 2 of the present invention, wherein (a) and (b) are SEM images of terbium-europium dual-doped hydroxyapatite at different magnifications; (c) is an X-ray diffraction (XRD) spectrum of terbium-europium dual-doped hydroxyapatite; (d)-(h) are element distribution energy spectra of different elements on the surface of terbium-europium dual-doped hydroxyapatite nanorod luminescent materials; Figure 3(a) and (b) are respectively a luminous effect diagram and an emission spectrum diagram of the flexible luminous fiber provided in Example 7 of the present invention. DETAILED DESCRIPTION
[0018] The principles and features of the present invention are described below in conjunction with specific embodiments. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0019] Example 1 A method for preparing a terbium-europium double-doped hydroxyapatite luminescent material for fiber, comprising the following steps: Step 1: Dissolve 5.372 g of disodium hydrogen phosphate in 15 mL of deionized water to prepare a disodium hydrogen phosphate solution, adjust the pH of the disodium hydrogen phosphate solution to 11.5 with 1 mol / L of sodium hydroxide, dissolve 0.277 g of calcium chloride in 15 mL of deionized water, dissolve 0.075 mmol of terbium nitrate and 0.02 mmol of europium nitrate in 2.5 mL of deionized water, add the calcium chloride solution dropwise to the mixed solution of europium nitrate and terbium nitrate, and adjust the pH to 10 with 1 mol / L of sodium hydroxide.
[0020] Step 2: Add a mixed solution of calcium chloride, terbium nitrate and europium nitrate dropwise into a disodium hydrogen phosphate alkaline solution while stirring, and stir at 40° C. for 1 hour to obtain a hydroxyapatite precursor solution.
[0021] Step 3: The hydroxyapatite precursor solution obtained in step 2 is placed in a reactor, and the temperature is raised to 150°C and the reaction is carried out for 6 hours. No special auxiliary conditions such as microwaves, surfactants and polyethylene glycol are required during the experimental reaction. After the reaction, it is cooled to 30°C-40°C and centrifuged at a centrifugal speed of 5000rpm for 5 minutes. Then the supernatant is poured out, deionized water is added to the precipitate, and the precipitate is centrifuged at a centrifugal speed of 5000rpm for 5 minutes. Repeat 3 times to obtain a terbium-europium dual-doped hydroxyapatite product.
[0022] Test Characterization: Take the terbium-europium dual-doped hydroxyapatite product obtained in step 3, test XRD, SEM, and determine its structure and morphology, such as Figure 1 As shown, it is shown that the hydroxyapatite nanorod luminescent material prepared in this example has uniform morphology, narrow width and moderate length, which is conducive to compounding with fibers.
[0023] It should be further explained that before executing step 1, the present invention also provides a method for determining the relative doping ratio of terbium ions and europium ions to determine the amounts of calcium chloride, terbium nitrate and europium nitrate in the above step 2, and the specific steps are: Step 1', adding sodium hydroxide to the disodium hydrogen phosphate solution to adjust the pH of the solution to make the solution strongly alkaline.
[0024] Step 2', add a mixed solution of calcium chloride and terbium nitrate dropwise to the strong alkaline solution obtained in step 1', and stir at 40° C. until completely dissolved to obtain a hydroxyapatite precursor solution.
[0025] Step 3', placing the hydroxyapatite precursor solution obtained in step 2' in an autoclave and heating it to 150-200° C. for reaction, cooling at room temperature after the reaction is completed, centrifugation purification, and drying to obtain terbium mono-doped hydroxyapatite.
[0026] Step 4', changing the doping concentration of terbium ions within a preset range according to a preset rule, and repeating steps 2' and 3' to determine the optimal doping concentration of terbium ions corresponding to the best luminescence performance of terbium-doped hydroxyapatite.
[0027] Step 5': determine the relative doping ratio of terbium ions and europium ions according to the luminescence requirement, thereby preparing a terbium nitrate and europium nitrate solution with a required ratio.
[0028] Among them, in step 4', the preset range can be 0.01-10, and the preset rule can be increased or decreased in steps of 0.01mmol. In step 5', determining the relative doping ratio of terbium ions and europium ions according to the luminescence requirements specifically means that if the luminescent material is required to emit more green light, the terbium ion doping ratio is increased, and if the luminescent material is required to emit more red light, the europium ion doping ratio is increased. The relative ratio of the two can be adjusted according to actual needs.
[0029] Example 2 A method for preparing a terbium-europium double-doped hydroxyapatite luminescent material for fiber, comprising the following steps: Step 1: Dissolve 5.372 g of disodium hydrogen phosphate in 15 mL of deionized water to prepare a disodium hydrogen phosphate solution, adjust the pH of the disodium hydrogen phosphate solution to 11.5 with 1 mol / L of sodium hydroxide, dissolve 0.277 g of calcium chloride in 15 mL of deionized water, dissolve 0.075 mmol of terbium nitrate and 0.05 mmol of europium nitrate in 2.5 mL of deionized water, add the calcium chloride solution dropwise to the mixed solution of europium nitrate and terbium nitrate, and adjust the pH to 10 with 1 mol / L of sodium hydroxide.
[0030] Step 2: Add a mixed solution of calcium chloride, terbium nitrate and europium nitrate dropwise into a disodium hydrogen phosphate alkaline solution while stirring, and stir at 40° C. for 1 hour to obtain a hydroxyapatite precursor solution.
[0031] Step 3: Place the hydroxyapatite precursor solution obtained in step 2 into a metal reactor, heat it to 180°C, and react for 9 hours. No microwave-assisted conditions are required during the experimental reaction. After the reaction, cool it to 30°C-40°C, centrifuge it at a centrifugal speed of 5000rpm for 5 minutes, then pour out the supernatant, add deionized water to the precipitate, centrifuge it at a centrifugal speed of 5000rpm for 5 minutes, repeat 3 times, and obtain terbium-europium dual-doped hydroxyapatite product.
[0032] Test Characterization: Take the terbium-europium dual-doped hydroxyapatite product obtained in step 3, test XRD, SEM, and determine its structure and morphology, such as Figure 2 As shown, it is shown that the hydroxyapatite luminescent nanocrystals synthesized in this example have uniform morphology and size, various elements are evenly distributed, and rare earth elements are successfully doped into hydroxyapatite.
[0033] Example 3 A method for preparing a terbium-europium double-doped hydroxyapatite luminescent material for fiber, comprising the following steps: Step 1: Dissolve 5.372 g of disodium hydrogen phosphate in 15 mL of deionized water to prepare a disodium hydrogen phosphate solution, adjust the pH of the disodium hydrogen phosphate solution to 11.5 with 1 mol / L of sodium hydroxide, dissolve 0.277 g of calcium chloride in 15 mL of deionized water, dissolve 0.075 mmol of terbium nitrate and 0.075 mmol of europium nitrate in 2.5 mL of deionized water, add the calcium chloride solution dropwise to the mixed solution of europium nitrate and terbium nitrate, and adjust the pH to 10 with 1 mol / L of sodium hydroxide.
[0034] Step 2: Add a mixed solution of calcium chloride, terbium nitrate and europium nitrate dropwise into a disodium hydrogen phosphate alkaline solution while stirring, and stir at 40° C. for 1 hour to obtain a hydroxyapatite precursor solution.
[0035] Step 3: The hydroxyapatite precursor solution obtained in step 2 is placed in a reactor, and the temperature is raised to 200°C, and the reaction is carried out for 12 hours. Microwave-assisted conditions are not required during the experimental reaction. After the reaction, it is cooled to 30°C-40°C, centrifuged at a centrifugal speed of 5000 rpm for 5 minutes, and then the supernatant is poured out, deionized water is added to the precipitate, and centrifuged at a centrifugal speed of 5000 rpm for 5 minutes. Repeat 3 times to obtain a terbium-europium dual-doped hydroxyapatite product.
[0036] Test Characterization: The terbium-europium dual-doped hydroxyapatite product obtained in step 3 was tested by XRD and SEM to determine its structure and morphology.
[0037] Example 4 A method for preparing a terbium-europium double-doped hydroxyapatite luminescent material for fiber, comprising the following steps: Step 1: Dissolve 5.372 g of disodium hydrogen phosphate in 15 mL of deionized water to prepare a disodium hydrogen phosphate solution, adjust the pH of the disodium hydrogen phosphate solution to 11.5 with 1 mol / L of sodium hydroxide, dissolve 0.277 g of calcium chloride in 15 mL of deionized water, dissolve 0.075 mmol of terbium nitrate and 0.02 mmol of europium nitrate in 2.5 mL of deionized water, add the calcium chloride solution dropwise to the mixed solution of europium nitrate and terbium nitrate, and adjust the pH to 10 with 1 mol / L of sodium hydroxide.
[0038] Step 2: Add a mixed solution of calcium chloride, terbium nitrate and europium nitrate dropwise into a disodium hydrogen phosphate alkaline solution while stirring, and stir at 40° C. for 1 hour to obtain a hydroxyapatite precursor solution.
[0039] Step 3: The hydroxyapatite precursor solution obtained in step 2 is placed in a reactor and heated to 150°C for reaction for 8 hours. Microwave-assisted conditions are not required during the experimental reaction. After the reaction, it is cooled to 30°C-40°C and centrifuged at a centrifugal speed of 5000 rpm for 5 minutes. The supernatant is then poured out, deionized water is added to the precipitate, and the precipitate is centrifuged at a centrifugal speed of 5000 rpm for 5 minutes. Repeat 3 times to obtain a terbium-europium dual-doped hydroxyapatite product.
[0040] Test Characterization: The terbium-europium dual-doped hydroxyapatite product obtained in step 3 was tested by XRD and SEM to determine its structure and morphology.
[0041] Example 5 A method for preparing a terbium-europium double-doped hydroxyapatite luminescent material for fiber, comprising the following steps: Step 1: Dissolve 5.372 g of disodium hydrogen phosphate in 15 mL of deionized water to prepare a disodium hydrogen phosphate solution, adjust the pH of the disodium hydrogen phosphate solution to 11.5 with 1 mol / L of sodium hydroxide, dissolve 0.277 g of calcium chloride in 15 mL of deionized water, dissolve 0.075 mmol of terbium nitrate and 0.05 mmol of europium nitrate in 2.5 mL of deionized water, add the calcium chloride solution dropwise to the mixed solution of europium nitrate and terbium nitrate, and adjust the pH to 10 with 1 mol / L of sodium hydroxide.
[0042] Step 2: Add a mixed solution of calcium chloride, terbium nitrate and europium nitrate dropwise into a disodium hydrogen phosphate alkaline solution while stirring, and stir at 40° C. for 1 hour to obtain a hydroxyapatite precursor solution.
[0043] Step 3: The hydroxyapatite precursor solution obtained in step 2 is placed in a reactor and heated to 180°C for reaction for 10 hours. Microwave-assisted conditions are not required during the experimental reaction. After the reaction, it is cooled to 30°C-40°C and centrifuged at a centrifugal speed of 5000 rpm for 5 minutes. The supernatant is then poured out, deionized water is added to the precipitate, and the solution is centrifuged at a centrifugal speed of 5000 rpm for 5 minutes. This is repeated three times to obtain a terbium-europium dual-doped hydroxyapatite product.
[0044] Test Characterization: The terbium-europium dual-doped hydroxyapatite product obtained in step 3 was tested by XRD and SEM to determine its structure and morphology.
[0045] Example 6 A method for preparing a terbium-europium double-doped hydroxyapatite luminescent material for fiber, comprising the following steps: Step 1: Dissolve 5.372 g of disodium hydrogen phosphate in 15 mL of deionized water to prepare a disodium hydrogen phosphate solution, adjust the pH of the disodium hydrogen phosphate solution to 11.5 with 1 mol / L of sodium hydroxide, dissolve 0.277 g of calcium chloride in 15 mL of deionized water, dissolve 0.075 mmol of terbium nitrate and 0.075 mmol of europium nitrate in 2.5 mL of deionized water, add the calcium chloride solution dropwise to the mixed solution of europium nitrate and terbium nitrate, and adjust the pH to 10 with 1 mol / L of sodium hydroxide.
[0046] Step 2: Add a mixed solution of calcium chloride, terbium nitrate and europium nitrate dropwise into a disodium hydrogen phosphate alkaline solution while stirring, and stir at 40° C. for 1 hour to obtain a hydroxyapatite precursor solution.
[0047] Step 3: The hydroxyapatite precursor solution obtained in step 2 is placed in a reactor, and the temperature is raised to 200°C, and the reaction is carried out for 12 hours. Microwave-assisted conditions are not required during the experimental reaction. After the reaction, it is cooled to 30°C-40°C, centrifuged at a centrifugal speed of 5000 rpm for 5 minutes, and then the supernatant is poured out, deionized water is added to the precipitate, and centrifuged at a centrifugal speed of 5000 rpm for 5 minutes. Repeat 3 times to obtain a terbium-europium dual-doped hydroxyapatite product.
[0048] Test Characterization: The terbium-europium dual-doped hydroxyapatite product obtained in step 3 was tested by XRD and SEM to determine its structure and morphology.
[0049] Example 7 A method for preparing rare earth-doped hydroxyapatite for bio-based anti-counterfeiting detection fibers.
[0050] Example 1 was repeated, except that the prepared fiber was compounded with terbium-europium dual-doped hydroxyapatite luminescent material and aramid short-cut / polyphenylene sulfide fibers (ACFs / PPS) to prepare a flexible luminescent fiber with fluorescent properties.
[0051] Test Characterization: Take the flexible light-emitting fiber prepared in Example 7, test PL, and determine its emission spectrum. Figure 3 As shown, Figure 3 (a) is the luminescence effect diagram of the hydroxyapatite nanorod luminescent material / fiber composite film obtained by ultraviolet irradiation luminescence color stability test at room temperature and minus 50 degrees environment, (b) is the emission spectrum diagram obtained by fluorescence test of the luminescent fiber film, and the characteristic emission peaks of terbium ions and europium ions appear at 547nm, 591nm and 620nm respectively, indicating that the luminescent nanorods and fibers are successfully composited.
[0052] In addition, the experimental results show that when the reaction temperature is lower than 150°C or higher than 200°C, the TbEu doped hydroxyapatite product cannot be obtained, or the product contains a large amount of impurities such as byproducts or impurities. When the reaction temperature is 150-200°C and the reaction time is 6-12h, the average length of the TbEu doped hydroxyapatite nanorods is distributed in the range of 100-400nm, the average diameter is distributed in the range of 15-30nm, and the morphology is regular.
[0053] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing terbium-europium double-doped hydroxyapatite luminescent material for fiber, It is characterized in that The following steps are involved: Step 1, adding sodium hydroxide to the disodium hydrogen phosphate solution to adjust the pH of the solution to make the solution strongly alkaline; Step 2: Add a mixed solution of calcium chloride, terbium nitrate and europium nitrate dropwise to the strongly alkaline solution obtained in step 1, and stir at 40° C. until completely dissolved to obtain a hydroxyapatite precursor solution; Step 3: placing the hydroxyapatite precursor solution obtained in step 2 in an autoclave and heating it to 150-200° C. for reaction; cooling at room temperature after the reaction is completed, centrifugation purification, and drying to obtain terbium-europium dual-doped hydroxyapatite luminescent material for fiber.
2. The method for preparing the terbium-europium dual-doped hydroxyapatite luminescent material for fiber according to claim 1, It is characterized in that Before performing step 1, the preparation method further comprises: Step 1', adding sodium hydroxide to the disodium hydrogen phosphate solution to adjust the pH of the solution to make the solution strongly alkaline; Step 2', adding a mixed solution of calcium chloride and terbium nitrate dropwise to the strongly alkaline solution obtained in step 1', stirring at 40° C. until completely dissolved, to obtain a hydroxyapatite precursor solution; Step 3', placing the hydroxyapatite precursor solution obtained in step 2' in an autoclave and heating it to 150-200°C for reaction, cooling at room temperature after the reaction is completed, centrifugation purification, and drying to obtain terbium mono-doped hydroxyapatite; Step 4', changing the doping concentration of terbium ions within a preset range according to a preset rule, and repeating steps 2' and 3' to determine the optimal doping concentration of terbium ions corresponding to the best luminescence performance of terbium-doped hydroxyapatite; Step 5': determine the relative doping ratio of terbium ions and europium ions according to the luminescence requirement, thereby preparing a terbium nitrate and europium nitrate solution with a required ratio.
3. The method for preparing the terbium-europium dual-doped hydroxyapatite luminescent material for fiber according to claim 1, It is characterized in that The amount of disodium hydrogen phosphate used in step 1 is 5.372 g.
4. The method for preparing the terbium-europium dual-doped hydroxyapatite luminescent material for fiber according to claim 1, It is characterized in that The amounts of calcium chloride, terbium nitrate and europium nitrate used in step 2 are 0.277 g, 0.075 mmol and 0.020-0.075 mmol respectively.
5. The method for preparing the terbium-europium dual-doped hydroxyapatite luminescent material for fiber according to claim 1, It is characterized in that The stirring time in step 2 was 1 h.
6. The method for preparing the terbium-europium dual-doped hydroxyapatite luminescent material for fiber according to claim 1, It is characterized in that The content of the hydroxyapatite precursor solution obtained in step 2 is 27.5 mL.
7. The method for preparing the terbium-europium dual-doped hydroxyapatite luminescent material for fiber according to claim 1, It is characterized in that The reaction time in step 3 is 6-12 hours, the solvent required for the centrifugal purification process is deionized water, the centrifugal speed is 5000 rpm, the centrifugal time is 5 minutes, and the number of centrifugation is 3 times.
8. A terbium-europium double-doped hydroxyapatite luminescent material for fiber, It is characterized in that The fiber-based terbium-europium dual-doped hydroxyapatite luminescent material is prepared by the method described in any one of claims 1-7.
9. Application of the terbium-europium dual-doped hydroxyapatite luminescent material for fiber according to claim 8 in the field of LED and fluorescent anti-counterfeiting / detection fiber.