Red luminescent material activated by Eu < 3 + > ions as well as preparation method and application of red luminescent material

By using tungstate oxide as a matrix and Eu3+ to replace Gd3+ in Ba4GdMgNbWO12:xEu material, it is excited in the ultraviolet-blue light band, and the problem of low light absorption efficiency of Eu3+ activation phosphor is solved, achieving high efficiency of red luminescence efficiency and stability , suitable for white-glow LEDs.

CN118931537AActive Publication Date: 2024-11-12CHANGSHU INSTITUTE OF TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411001662.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

Eu3+ activated phosphor has low light absorption resonance efficiency in the UV-visible wavelength range, resulting in low luminous efficiency.

Method used

Using Ba4GdMgNbWO12:xEu red-luminescent material, using tungstate oxide as matrix, Eu3+ replaces Gd3+, excites in the ultraviolet-blue band, emits red light with sharp characteristic peaks at 613 nanometers, and improves the material's material through multiple sintering processes. Light absorption and emission characteristics.

Benefits of technology

It improves light absorption capacity and emission characteristics, enhances the luminous efficiency and stability of fluorescent materials, and is suitable for white-luminous LEDs excitated based on near-ultraviolet and blue-ray semiconductor chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931537A_ABST
    Figure CN118931537A_ABST
Patent Text Reader

Abstract

The invention provides a red luminescent material activated by Eu < 3 + > ions and a preparation method and application thereof, and belongs to the technical field of inorganic luminescent materials. The chemical formula of the red luminescent material is Ba4GdMgNbWO12: xEu, x is the mole number of Gd < 3 + > replaced by Eu < 3 + >, and x is more than or equal to 0.003 and less than or equal to 0.40. In the Eu < 3 + >-doped fluorescent powder, the tungstate oxide is used as the matrix, so that the light absorption capacity can be improved, the emission characteristic and stability of the fluorescent material can be enhanced, and the application performance and quality of the fluorescent powder can be improved; the red luminescent material can be excited by light (230-470 nanometers) with the wavelength ranging from ultraviolet to blue light and can emit a sharp spectrum with the wavelength peak value located at 613 nanometers, and the emitted light is pure in red degree, high in luminescent intensity and good in temperature stability. In addition, the red light-emitting material can be combined with ultraviolet, near ultraviolet or blue light semiconductor chips to prepare polychromatic light LED lighting devices with high light-emitting performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of inorganic luminescent materials and specifically relates to a Eu 3+ Ion-activated red luminescent material and preparation method and application thereof. Background Art

[0002] Rare earth elements have relatively stable f-electron orbitals in their atomic structures, and the energy levels of electrons in different orbitals interact with each other, resulting in complex and diverse spectral characteristics. Compared with general transition metal ions, rare earth ions are more likely to achieve electronic transitions and have more possibilities when absorbing and emitting photons. Therefore, phosphors activated by rare earth ions can emit spectra of different wavelengths, producing colorful luminescence effects, and play an important role in the fields of luminescence and display.

[0003] Among rare earth activating ions, europium ions (Eu 3+ ) is the most important red luminescent activator, and its ground state electronic configuration is [Xe]4f 6 In the excited state, it emits strong red light from the 4f-4f transition, and the light energy is concentrated and the red color is pure. 3+ It can be excited to an excited state by absorbing high-energy photons such as ultraviolet light or blue light, and then emit red fluorescence. This luminescence characteristic makes it widely used in fluorescent materials, optical display devices, biological fluorescent markers and other fields. However, in Eu 3+ In activated phosphors, the matrix absorbs the excitation energy of UV-visible wavelengths and then transfers the excitation energy to Eu 3+ To achieve its red emission, therefore, in the UV-visible wavelength range Eu 3+ The light absorption resonance efficiency is very low, which further leads to its low luminescence efficiency. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art and provide a Eu 3+ Ion-activated red luminescent material and preparation method and application thereof.

[0005] In one aspect of the present disclosure, there is provided a Eu 3+ Ion-activated red luminescent material, the chemical formula of the red luminescent material is Ba4GdMgNbWO 12 :xEu, where x is Eu 3+ Replace Gd 3+ The number of moles, and 0.003≤x≤0.40.

[0006] Optionally, the red luminescent material can emit red light with a sharp characteristic peak at 613 nanometers under the excitation of light in the ultraviolet-blue light band.

[0007] Another aspect of the present disclosure is to provide a method for preparing Eu as described above. 3+ A method for producing an ion-activated red luminescent material, the method comprising:

[0008] According to the chemical formula Ba4GdMgNbWO 12 :xEu, weighing a compound containing barium ions, a compound containing gadolinium ions, a compound containing magnesium ions, a compound containing niobium ions, a compound containing tungsten ions, and a compound containing europium ions, wherein 0.003≤x≤0.40, grinding and mixing the weighed compounds to obtain an initial raw material mixture;

[0009] The initial raw material mixture is pre-sintered for the first time in an air atmosphere at a sintering temperature of 300° C. to 600° C. for a sintering time of 1 to 5 hours, the sintered product is naturally cooled to room temperature, and fully ground to mix uniformly to obtain a first pre-sintered mixture;

[0010] The first pre-sintered mixture is subjected to a second sintering in an air atmosphere at a sintering temperature of 800° C. to 1000° C. for a sintering time of 1 to 10 hours, and the sintered product is naturally cooled to room temperature to obtain a second pre-sintered mixture;

[0011] The second pre-sintered mixture is sintered for the third time in an air atmosphere at a sintering temperature of 1000° C. to 1350° C. for 3 to 10 hours, and the sintered product is naturally cooled to room temperature to obtain a Eu 3+ Ion-activated red luminescent material.

[0012] Optionally, the compound containing barium ions is one of barium oxide, barium nitrate and barium carbonate.

[0013] Optionally, the compound containing gadolinium ions is one of gadolinium oxide, gadolinium nitrate and gadolinium carbonate.

[0014] Optionally, the compound containing magnesium ions is one of basic magnesium carbonate tetrahydrate, magnesium nitrate, magnesium oxide, and magnesium hydroxide.

[0015] Optionally, the compound containing niobium ions is one of niobium pentoxide, niobium pentachloride and niobium hydroxide.

[0016] Optionally, the compound containing tungsten ions is one of tungsten oxide and ammonium tungstate.

[0017] Optionally, the compound containing europium ions is europium oxide.

[0018] Another aspect of the present disclosure is to provide a Eu as described above. 3+Ion-activated red light-emitting materials are used in white light-emitting LEDs based on near-ultraviolet and blue light semiconductor chip excitation.

[0019] The present disclosure proposes a Eu 3+ Ion-activated red luminescent material and its preparation method and application. The chemical formula of the red luminescent material is Ba4GdMgNbWO 12 :xEu, where x is Eu 3+ Replace Gd 3+ The number of moles of Eu 3+ In doped phosphors, using tungstate oxide as a matrix can not only improve the light absorption capacity, but also enhance the emission characteristics and stability of the fluorescent material, which is beneficial to improving the application performance and quality of the phosphors. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a flowchart of the red light-emitting material activated by Eu3+ ions according to an embodiment of the present disclosure;

[0021] Figure 2 The XRD diffraction patterns of the samples prepared in Examples 1, 2, 3, and 4 of the present disclosure are compared with the X-ray diffraction standard card PDF#33-1069;

[0022] Figure 3 The excitation spectrum and luminescence spectrum of the sample prepared in Example 1 of the present disclosure;

[0023] Figure 4 is the luminescence decay curve of the sample prepared in Example 1 of the present disclosure;

[0024] Figure 5 The excitation spectrum and luminescence spectrum of the sample prepared in Example 2 of the present disclosure;

[0025] Figure 6 is the luminescence decay curve of the sample prepared in Example 2 of the present disclosure;

[0026] Figure 7 The excitation spectrum and luminescence spectrum of the sample prepared in Example 3 of the present disclosure;

[0027] Figure 8 is the luminescence decay curve of the sample prepared in Example 3 of the present disclosure;

[0028] Fig. 9 The excitation spectrum and luminescence spectrum of the sample prepared in Example 4 of the present disclosure;

[0029] Fig.10 This is the luminescence attenuation curve of the sample prepared in Example 4 of the present disclosure. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the disclosure. The described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure.

[0031] In one aspect of the present disclosure, there is provided a Eu 3+ Ion-activated red luminescent material, the chemical formula of which is Ba4GdMgNbWO 12 :xEu, where x is a europium ion (Eu 3+ ) replaces the gadolinium ion (Gd 3+ ), and 0.003≤x≤0.40.

[0032] It should be understood that the choice of matrix has a significant impact on the 3+ Activated phosphors are very important. Among common oxide matrices, tungstate is one of the most effective matrices. This is mainly because tungstate oxide has a wide range of light absorption and can effectively absorb ultraviolet light, visible light and light energy in different wavelength ranges, thereby improving the luminous efficiency of fluorescent materials. In addition, tungstate oxide has high thermal stability and chemical stability, which can ensure the stability and durability of phosphors under different environments and lighting conditions. Therefore, this embodiment proposes a method of using tungstate as a matrix and europium ions Eu as a matrix. 3+ Phosphor as activator.

[0033] In this embodiment, the matrix material has good light absorption in the ultraviolet-visible light wavelength range. 3+ The energy transfer efficiency between the substrate and the lattice is high; and the lattice of the matrix material has WO6 octahedron and NbO6 octahedron, which enhances the lattice strength, so that the gadolinium ions (Gd 3+ ), magnesium ion (Mg 2+ ) and niobium ions (Nb 5+ ) randomly and uniformly occupy the same octahedral lattice position, which greatly enhances the disturbance of the matrix crystal field and is beneficial to Eu 3+ of 5 D0→ 7 F2 luminescence transition has pure chromaticity and high luminescence efficiency.

[0034] The red light emitting material of this embodiment can emit red light with a sharp characteristic peak at 613 nanometers under the excitation of light in the ultraviolet-blue light band.

[0035] like Figure 1 As shown, in another aspect of the present disclosure, there is provided a Eu 3+ The preparation method S100 of the ion-activated red luminescent material specifically includes the following steps S110 to S140:

[0036] S110, according to the chemical formula Ba4GdMgNbWO 12 :xEu (0.003≤x≤0.40) contains barium ions (Ba 2+ ) compounds, gadolinium ions (Gd 3+ ) compounds, magnesium ions (Mg 2+ ) compounds, niobium ions (Nb 5+ ) compounds, tungsten ions (W 6+ ) compounds, europium ions (Eu 3+ ) compounds, grinding and mixing the weighed compounds to obtain an initial raw material mixture.

[0037] In some preferred embodiments, the barium ion (Ba 2+ ) is one of barium oxide, barium nitrate and barium carbonate. For example, barium carbonate is preferred.

[0038] In other preferred embodiments, the gadolinium ion (Gd 3+ ) is one of gadolinium oxide, gadolinium nitrate and gadolinium carbonate. For example, gadolinium oxide is preferred.

[0039] In other preferred embodiments, the magnesium ion (Mg 2+ ) is one of basic magnesium carbonate tetrahydrate, magnesium nitrate, magnesium oxide, and magnesium hydroxide. For example, basic magnesium carbonate tetrahydrate is preferred.

[0040] In some other preferred embodiments, the niobium ion (Nb 5+ ) is one of niobium pentoxide, niobium pentachloride and niobium hydroxide. For example, niobium pentoxide is preferred.

[0041] In other preferred embodiments, the tungsten ion (W 6+ ) is one of tungsten oxide and ammonium tungstate. For example, ammonium tungstate is preferred.

[0042] S120, pre-sintering the weighed initial raw material mixture for the first time in an air atmosphere at a sintering temperature of 300° C. to 600° C. for 1 to 5 hours, naturally cooling the sintered product to room temperature, and grinding it thoroughly to mix it evenly to obtain a first pre-sintered mixture.

[0043] In some preferred embodiments, the temperature of the first pre-sintering is preferably 300°C, 350°C, 400°C, 500°C, 600°C, etc., and the sintering time is preferably 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, etc.

[0044] S130, sintering the first pre-sintered mixture for a second time in an air atmosphere at a sintering temperature of 800° C. to 1000° C. for a sintering time of 1 to 10 hours, and naturally cooling the sintered product to room temperature to obtain a second pre-sintered mixture.

[0045] In some preferred embodiments, the temperature of the second pre-sintering is preferably 800°C, 900°C, 950°C, 1000°C, etc., and the sintering time is preferably 1 hour, 3 hours, 4 hours, 5 hours, 7 hours, 10 hours, etc.

[0046] S140, sintering the second pre-sintered mixture for a third time in an air atmosphere at a sintering temperature of 1000° C. to 1350° C. for 3 to 10 hours, and naturally cooling the sintered product to room temperature to obtain a Eu 3+ Ion-activated red luminescent material.

[0047] In some preferred embodiments, the temperature of the third pre-sintering is preferably 1000°C, 1100°C, 1200°C, 1250°C, 1300°C, 1350°C, etc., and the sintering time is preferably 3 hours, 5 hours, 7 hours, 10 hours, etc.

[0048] The preparation method of this embodiment is simple, low-cost, pollution-free, has no waste gas or waste liquid emissions, is environmentally friendly, has a low sintering temperature, saves energy, and is easy to produce.

[0049] Another aspect of the present disclosure is to provide a Eu as described above. 3+ Ion-activated red light-emitting materials are used in white light-emitting LEDs based on near-ultraviolet and blue light semiconductor chip excitation.

[0050] It should be understood that the red light-emitting material based on the present embodiment has pure red light chromaticity and high light-emitting efficiency, and can emit red light with a sharp characteristic peak at 613 nanometers under excitation in the ultraviolet to blue light band. Therefore, the red light-emitting material can be used in various types of lighting and display equipment, especially in white light-emitting LEDs based on near-ultraviolet and blue light semiconductor chips.

[0051] The following will further illustrate Eu 3+ Ion-activated red luminescent materials and their properties:

[0052] Example 1

[0053] In this example, Eu 3+The method for preparing an ion-activated red luminescent material comprises the following steps:

[0054] S1, according to the chemical formula Ba4GdMgNbWO 12 :0.003Eu, respectively weigh: 31.574 g of barium carbonate, 7.228 g of gadolinium oxide, 0.021 g of europium oxide, 3.885 g of basic magnesium carbonate tetrahydrate, 5.316 g of niobium pentoxide, and 10.141 g of ammonium tungstate, put the raw materials weighed above into a mortar, grind and mix them evenly, and obtain an initial raw material mixture.

[0055] S2. Then, the initial raw material mixture obtained in step S1 is pre-calcined for the first time in an air atmosphere at a calcination temperature of 300° C. for 5 hours. The calcination furnace is naturally cooled to room temperature. The sample is taken out and ground and mixed again to obtain a first pre-sintered mixture.

[0056] S3, calcining the first pre-sintered mixture for a second time in an air atmosphere at a calcination temperature of 800° C. for 10 hours, and cooling the calcining furnace naturally to room temperature; taking out the sample again, grinding and mixing it evenly, to obtain a second pre-sintered mixture.

[0057] S4, the second pre-sintered mixture is calcined for the third time in an air atmosphere at a calcination temperature of 1350°C for 3 hours. The calcination furnace is naturally cooled to room temperature, and the sintering preparation of the sample is completed to obtain a Eu 3+ Ion-activated red luminescent material.

[0058] See attached Figure 2 , is the X-ray powder diffraction pattern of the sample prepared according to this Example 1, and the result shows that the sample is a single-phase material.

[0059] See attached Figure 3 , is the photoluminescence spectrum of the sample prepared according to Example 1. It can be seen that the sample exhibits good excitation in the ultraviolet-blue light range, and its luminescence is a sharp red luminescence spectrum with a peak at 613 nanometers;

[0060] See attached Figure 4 , is the luminescence decay curve of the sample prepared according to Example 1, and its luminescence lifetime is 1.51 milliseconds, which is Eu 3+ The characteristic luminescence decay of ions can meet the needs of luminescence display without the afterglow phenomenon.

[0061] Example 2

[0062] In this example, Eu 3+ The method for preparing an ion-activated red luminescent material comprises the following steps:

[0063] S1, according to the chemical formula Ba4GdMgNbWO 12 :0.15Eu, respectively weigh: 7.893 g of barium carbonate, 1.541 g of gadolinium oxide, 1.264 g of europium oxide, 0.971 g of basic magnesium carbonate tetrahydrate, 1.329 g of niobium pentoxide, and 2.535 g of ammonium tungstate, put the raw materials weighed above into a mortar, grind and mix them evenly, and obtain an initial raw material mixture.

[0064] S2. Then, the initial raw material mixture obtained in step S1 is pre-calcined for the first time in an air atmosphere at a calcination temperature of 600° C. for 1 hour. The calcination furnace is naturally cooled to room temperature. The sample is taken out and ground and mixed again to obtain a first pre-sintered mixture.

[0065] S3, calcining the first pre-sintered mixture for a second time in an air atmosphere at a calcination temperature of 1000° C. for 1 hour, and cooling the calcination furnace naturally to room temperature; taking out the sample again, grinding and mixing it evenly, to obtain a second pre-sintered mixture.

[0066] S4, the second pre-sintered mixture is calcined for the third time in an air atmosphere at a calcination temperature of 1000°C for 10 hours. The calcination furnace is naturally cooled to room temperature, and the sintering preparation of the sample is completed to obtain a Eu 3+ Ion-activated red luminescent material.

[0067] See attached Figure 2 , is the X-ray powder diffraction pattern of the sample prepared according to Example 2, and the result shows that the sample is a single-phase material.

[0068] See attached Figure 5 , is the photoluminescence spectrum of the sample prepared according to Example 2. It can be seen that the sample exhibits good excitation in the ultraviolet-blue light range, and its luminescence is a sharp red luminescence spectrum with a peak at 613 nanometers;

[0069] See attached Figure 6 , is the luminescence decay curve of the sample prepared according to Example 2, and its luminescence lifetime is 1.33 milliseconds, which is Eu 3+ The characteristic luminescence decay of ions can meet the needs of luminescence display without the afterglow phenomenon.

[0070] Example 3

[0071] In this example, Eu 3+ The method for preparing an ion-activated red luminescent material comprises the following steps:

[0072] S1, according to the chemical formula Ba4GdMgNbWO 12:0.3Eu, respectively weigh: 6.315 g of barium carbonate, 1.015 g of gadolinium oxide, 0.422 g of europium oxide, 0.777 g of basic magnesium carbonate tetrahydrate, 1.063 g of niobium pentoxide, and 2.028 g of ammonium tungstate, put the raw materials weighed above into a mortar, grind and mix them evenly, and obtain an initial raw material mixture.

[0073] S2. Then, the initial raw material mixture obtained in step S1 is pre-calcined for the first time in an air atmosphere at a calcination temperature of 350° C. for 3 hours. The calcination furnace is naturally cooled to room temperature. The sample is taken out and ground and mixed again to obtain a first pre-sintered mixture.

[0074] S3, calcining the first pre-sintered mixture for a second time in an air atmosphere at a calcination temperature of 900° C. for 5 hours, and cooling the calcination furnace naturally to room temperature; taking out the sample again, grinding and mixing it evenly, to obtain a second pre-sintered mixture.

[0075] S4, the second pre-sintered mixture is calcined for the third time in an air atmosphere at a calcination temperature of 1250°C for 5 hours, and the calcination furnace is naturally cooled to room temperature, thus completing the sintering preparation of the sample and obtaining a Eu 3+ Ion-activated red luminescent material.

[0076] See attached Figure 2 , is the X-ray powder diffraction pattern of the sample prepared according to Example 3, and the result shows that the sample is a single-phase material.

[0077] See attached Figure 7 , is the photoluminescence spectrum of the sample prepared according to Example 3. It can be seen that the sample exhibits good excitation in the ultraviolet-blue light range, and its luminescence is a sharp red luminescence spectrum with a peak at 613 nanometers;

[0078] See attached Figure 8 , is the luminescence decay curve of the sample prepared according to Example 3, and its luminescence lifetime is 1.11 milliseconds, which is Eu 3+ The characteristic luminescence decay of ions can meet the needs of luminescence display without the afterglow phenomenon.

[0079] Example 4

[0080] In this example, Eu 3+ The method for preparing an ion-activated red luminescent material comprises the following steps:

[0081] S1, according to the chemical formula Ba4GdMgNbWO 12:0.4Eu, respectively weigh: 5.526 g of barium carbonate, 0.761 g of gadolinium oxide, 0.493 g of europium oxide, 0.679 g of basic magnesium carbonate tetrahydrate, 0.931 g of niobium pentoxide, and 1.775 g of ammonium tungstate, put the above weighed raw materials into a mortar, grind and mix them evenly, to obtain an initial raw material mixture.

[0082] S2. Then, the initial raw material mixture obtained in step S1 is pre-calcined for the first time in an air atmosphere at a calcination temperature of 350° C. for 5 hours. The calcination furnace is naturally cooled to room temperature. The sample is taken out and ground and mixed again to obtain a first pre-sintered mixture.

[0083] S3, calcining the first pre-sintered mixture for a second time in an air atmosphere at a calcination temperature of 900° C. for 5 hours, and cooling the calcination furnace naturally to room temperature; taking out the sample again, grinding and mixing it evenly, to obtain a second pre-sintered mixture.

[0084] S4, the second pre-sintered mixture is calcined for the third time in an air atmosphere at a calcination temperature of 1250°C for 5 hours, and the calcination furnace is naturally cooled to room temperature, thus completing the sintering preparation of the sample and obtaining a Eu 3+ Ion-activated red luminescent material.

[0085] See attached Figure 2 , is the X-ray powder diffraction pattern of the sample prepared according to Example 4, and the result shows that the sample is a single-phase material.

[0086] See attached Fig. 9 , is the photoluminescence spectrum of the sample prepared according to Example 4. It can be seen that the sample exhibits good excitation in the ultraviolet-blue light range, and its luminescence is a sharp red luminescence spectrum with a peak at 613 nanometers;

[0087] See attached Fig.10 , is the luminescence decay curve of the sample prepared according to Example 4, and its luminescence lifetime is 0.93 milliseconds, which is Eu 3+ The characteristic luminescence decay of ions can meet the needs of luminescence display without the afterglow phenomenon.

[0088] The present disclosure proposes a Eu 3+ The ion-activated red luminescent material and its preparation method and application have the following beneficial effects compared with the prior art:

[0089] First, the advantages of the red luminescent material provided by the present disclosure are: 3+ ), magnesium ion (Mg 2+ ) and niobium ions (Nb 5+ ) randomly and uniformly occupy the same crystallographic lattice, activating the ion Eu3+ The crystal field can achieve strong perturbations, which is beneficial to the full splitting of the 4f energy level and is particularly beneficial to Eu 3+ of 5 D0→ 7 The electric dipole transition of F2 makes its red luminescence pure in chromaticity and high in luminescence efficiency.

[0090] Second, compared with the prior art, the advantages of the red luminescent material disclosed in the present invention are: the matrix tungstate salt of the red luminescent material has strong light absorption in the near-ultraviolet and blue light ranges, and the matrix and the activation center europium ion (Eu 3+ ) has high energy transfer efficiency.

[0091] Third, compared with common tungstate matrices such as CaWO4, the matrix lattice of the phosphor disclosed in the present invention has not only WO6 octahedrons but also NbO6 octahedrons, which enhances the lattice strength so that the phosphor has very good luminous efficiency and temperature stability.

[0092] Fourth, compared with the traditional red luminescent powder Y2O3:Eu 3+ 、YVO4:Eu 3+ Compared with other methods, the phosphor preparation method provided by the present invention is simple, pollution-free, has no waste gas or waste liquid emissions, has a low sintering temperature, saves energy, and is easy to produce.

[0093] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. Eu 3+ An ion-activated red luminescent material, characterized in that The chemical formula of the red luminescent material is Ba4GdMgNbWO 12 :xEu, where x is Eu 3+ Replace Gd 3+ The number of moles, and 0.003≤x≤0.

40.

2. Eu according to claim 1 3+ An ion-activated red luminescent material, characterized in that The red luminescent material can emit red light with a sharp characteristic peak at 613 nanometers under the excitation of light in the ultraviolet-blue light band.

3. A method for preparing Eu as claimed in claim 1 or 2 3+ A method for ion-activated red luminescent material, characterized in that The method comprises: According to the chemical formula Ba4GdMgNbWO 12 :xEu, weighing a compound containing barium ions, a compound containing gadolinium ions, a compound containing magnesium ions, a compound containing niobium ions, a compound containing tungsten ions, and a compound containing europium ions, wherein 0.003≤x≤0.40, grinding and mixing the weighed compounds to obtain an initial raw material mixture; The initial raw material mixture is pre-sintered for the first time in an air atmosphere at a sintering temperature of 300° C. to 600° C. for a sintering time of 1 to 5 hours, the sintered product is naturally cooled to room temperature, and fully ground to mix uniformly to obtain a first pre-sintered mixture; The first pre-sintered mixture is subjected to a second sintering in an air atmosphere at a sintering temperature of 800° C. to 1000° C. for a sintering time of 1 to 10 hours, and the sintered product is naturally cooled to room temperature to obtain a second pre-sintered mixture; The second pre-sintered mixture is sintered for the third time in an air atmosphere at a sintering temperature of 1000° C. to 1350° C. for 3 to 10 hours, and the sintered product is naturally cooled to room temperature to obtain a Eu 3+ Ion-activated red luminescent material.

4. The method according to claim 3, characterized in that The compound containing barium ions is one of barium oxide, barium nitrate and barium carbonate.

5. The method according to claim 3, characterized in that: The compound containing gadolinium ions is one of gadolinium oxide, gadolinium nitrate and gadolinium carbonate.

6. The method according to claim 3, characterized in that The compound containing magnesium ions is one of basic magnesium carbonate tetrahydrate, magnesium nitrate, magnesium oxide and magnesium hydroxide.

7. The method according to claim 3, characterized in that The compound containing niobium ions is one of niobium pentoxide, niobium pentachloride and niobium hydroxide.

8. The method according to claim 3, characterized in that The compound containing tungsten ions is one of tungsten oxide and ammonium tungstate.

9. The method according to claim 3, characterized in that: The compound containing europium ions is europium oxide.

10. Eu as claimed in claim 1 or 2 3+ Ion-activated red light-emitting materials are used in white light-emitting LEDs based on near-ultraviolet and blue light semiconductor chip excitation.

Citation Information

Patent Citations

  • Tungstate fluorescent powder as well as preparation method and application thereof

    CN102925150A