Anti-foaming agent composition as well as preparation method and application thereof

By selecting suitable dispersing solvents, dispersing additives and antifoaming agent active ingredients in the transmission oil of new energy vehicles, and performing compounding and process design, the problems of poor performance and easy precipitation of antifoaming agents at high temperatures are solved, and the problem of antifoaming agents is achieved. Highly efficient anti-foaming performance and long-term stability improve the foam control and hardware life of oil products.

CN118931628AActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +2
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310523725.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The antifoaming agent in the transmission oil of new energy vehicles has poor performance at high temperatures, which is difficult to disperse in lubricating oil and is easy to precipitate, resulting in difficulty in foam control, affecting the integrity of the oil film and hardware wear, and insufficient long-term storage stability.

Method used

By selecting suitable dispersion solvents, dispersion additives and antifoam agent active ingredients, performing compounding and process design, the efficient dispersion and long-term stability of the antifoam agent composition in lubricating oil is achieved, and specific mixing methods and process steps are adopted. Such as dissolution, grinding, etc., ensure the dispersion stability of the antifoaming agent composition in the system.

Benefits of technology

It achieves efficient foam resistance, high-temperature foam resistance and long-term storage stability, solves the problems of foam control and precipitation, and improves the insulation performance and hardware life of oil products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of anti-foaming agent compositions, in particular to an anti-foaming agent composition as well as a preparation method and application thereof. The anti-foaming agent composition comprises a dispersing solvent, an anti-foaming agent effective component, a dispersing aid and base oil in a weight ratio of (1-50): (0.0001-5): (1-90): (1-20), the dispersing solvent is selected from one or more of acetone, kerosene, methyl-ethyl ketone, methyl isobutyl ketone, m-dibenzotrifluoride, methylbenzene and cyclohexanone. The anti-foaming agent composition provided by the invention has excellent anti-foaming performance, can quickly eliminate foams generated in lubricating oil due to factors such as mechanical stirring when being added into the lubricating oil, also can solve the problem that the anti-foaming agent is difficult to disperse and easy to precipitate in the oil, ensures the long-term stability of the anti-foaming agent in the lubricating oil, and further solves the problem of high-temperature stability. The anti-foaming agent composition disclosed by the invention is suitable for being applied to the field of lubricating oil, and is particularly applied to ultralow-viscosity lubricating oil for electric automobiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of antifoaming agent compositions, and in particular to an antifoaming agent composition and a preparation method and application thereof. Background Art

[0002] Compared with traditional cars, the transmission lubricant of new energy vehicles needs to adapt to the high-speed working environment of the motor, and at the same time requires low viscosity to reduce oil stirring loss and achieve energy saving. As a result, the ultra-low viscosity transmission oil foam is easy to generate and difficult to eliminate. The difficulty in controlling foam has become an industry pain point for the transmission oil of new energy vehicles. Poor foam control will cause oil to overflow from the application conditions. What is more serious is that poor foam performance will lead to poor oil film integrity and hardware wear problems. At the same time, poor anti-foaming performance will affect the insulation performance of the oil. The solution to the foam problem depends on anti-foaming agent technology. At present, the technical difficulties of anti-foaming agent technology are that high-performance anti-foaming agents and high-performance anti-foaming agents are difficult to disperse and easy to precipitate in lubricating oils, and have poor long-term storage stability, resulting in poor high-temperature anti-foaming performance.

[0003] Domestic and foreign researchers have completed some fruitful work in the field of antifoaming agents, but there are still some technical problems that are not fully solved. For example, CN 104232246 B discloses a lubricating oil composite antifoaming agent, which solves the shortcomings of high-temperature foaming performance, but fails to solve the long-term stability problem of the antifoaming agent. US13620190284501A1 discloses a dispersion method of an antifoaming agent to improve the antifoaming performance, but fails to solve the shortcomings of high-temperature antifoaming performance.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an antifoaming agent composition and a preparation method and application thereof. The antifoaming agent composition developed by the present invention has strong antifoaming performance, high temperature antifoaming performance and can be more stable in lubricating oil.

[0006] Specifically, the present invention explores the causes of the above-mentioned technical problems and finds that the optimization of the antifoaming agent composition and the use of appropriate components and proportions can well achieve the physical separation of the antifoaming agent and avoid the aggregation of antifoaming agent particles, so that the antifoaming agent composition has high-efficiency antifoaming performance and good high-temperature antifoaming performance in the lubricating oil, and is effectively dispersed in the lubricating oil to achieve reliable long-term storage stability.

[0007] In a first aspect, the present invention provides a new antifoaming agent composition, comprising: a dispersing solvent, an antifoaming agent active ingredient, a dispersing aid and a base oil in a weight ratio of 1-50:0.0001-5:1-90:1-20.

[0008] The present invention obtains an antifoaming agent composition with high-efficiency antifoaming performance and good high-temperature performance by selecting specific dispersing aids, dispersing solvents, base oils and effective ingredients of antifoaming agents for compounding, and fully disperses the antifoaming agent through process design, thereby effectively achieving the dispersibility of the antifoaming agent in the lubricating oil system and reliable long-term storage stability.

[0009] Preferably, the weight ratio of the dispersing solvent, the antifoaming agent effective ingredient, the dispersing aid and the base oil is 1-50: 0.0003-3: 2-70: 5-15.

[0010] Preferably, the dispersing solvent is selected from one or more of acetone, kerosene, methyl-ethyl ketone, methyl isobutyl ketone, m-ditrifluorotoluene, toluene and cyclohexanone.

[0011] Preferably, the anti-foaming agent active ingredient is selected from one or more of methacrylate-acrylate copolymer, polyethylene glycol ether-fatty alcohol-polytetramethylene glycol ether copolymer, polydimethylsiloxane, polyether and fluorinated ester co-modified silicone oil, and polysiloxane containing branched fluorocarbon structure.

[0012] Preferably, the polysiloxane containing a branched carbon fluoro structure has a structure shown in the following formula (I):

[0013]

[0014] Where R is C1-C 22 Straight-chain alkanes, x=1~90, y=1~30, z=10~22.

[0015] Preferably, the polyether and fluorinated ester co-modified silicone oil has a structure as shown in the following formula (II):

[0016]

[0017] Among them, m=1~90, n=1~20, p=1~20.

[0018] Preferably, the dispersing aid is selected from one or more of alkylamine friction modifiers, thiophosphate amine salt extreme pressure antiwear agents, polymethacrylate pour point depressants, polyacrylate viscosity index improvers, polyisobutylene bissuccinimide (T154) dispersants, and alkyl calcium salicylate (T106) detergents.

[0019] Preferably, the base oil is selected from one or more of mineral base oil, vegetable oil, poly-α-olefin synthetic base oil, polyol ester synthetic base oil, polyalkylene glycol, and diester synthetic base oil.

[0020] Preferably, the surface tension of the antifoaming agent active ingredient is 15 to 30 Nm / m, preferably 20 to 25 Nm / m.

[0021] Preferably, the kinematic viscosity of the dispersing agent at 100° C. is 20 to 300 cSt, preferably 50 to 200 cSt.

[0022] In a second aspect, the present invention also provides a method for preparing the above antifoaming agent composition. Specifically, the method for preparing the antifoaming agent composition provided by the present invention comprises the following steps:

[0023] 1) dissolving the antifoaming agent active ingredient in the dispersing solvent to obtain a clear and transparent component A;

[0024] 2) The clear and transparent component A, the dispersing aid and the base oil are mixed according to a proportion, ground, and cooled to room temperature to obtain an antifoaming agent composition.

[0025] The present invention finds that the above-mentioned specific mixing method can further ensure the dispersion stability of the antifoaming agent composition in the system, which is beneficial to improving the antifoaming performance, high temperature antifoaming performance and long-term storage stability of the antifoaming agent composition.

[0026] Preferably, in step (2), the grinding is performed at 30 to 100° C. for 0.1 to 1 hour;

[0027] Preferably, in step (2), the grinding is performed 1 to 6 times, preferably 2 times;

[0028] Preferably, in step (2), the mixing is carried out in one or more of a stirred tank, a colloid mill, and a high-speed homogenizer. The present invention selects the above-mentioned specific dispersing aid, dispersing solvent, base oil and antifoaming agent effective ingredients for compounding, and fully disperses them through designs such as a colloid mill and a high-speed homogenizer, which can more effectively achieve the dispersibility and reliable long-term storage stability of the antifoaming agent in the lubricating oil system.

[0029] In the present invention, steps (1) to (2) are mixed in the above-mentioned specific manner, which is more conducive to the dispersion of the antifoaming agent composition, thereby improving its dispersion degree in the system and achieving high-efficiency antifoaming performance, high-temperature antifoaming performance and reliable long-term storage stability.

[0030] In a third aspect, the present invention also provides the application of the antifoaming agent composition or the preparation method of the antifoaming agent composition in the field of lubricating oil, preferably in ultra-low viscosity lubricating oil for electric vehicles. The antifoaming agent composition of the present invention has a good application effect in the field of lubricating oil, especially in the application of ultra-low viscosity lubricating oil used in electric vehicles.

[0031] The present invention prepares a high-performance antifoaming agent composition by preparing an antifoaming agent composition and a preparation process, and realizes effective dispersion of the antifoaming agent by inventing a preparation method, solves the problem that the antifoaming agent is difficult to disperse and easy to precipitate, realizes long-term storage stability in lubricating oil, and solves the problem of poor high-temperature antifoaming performance. The beneficial effects of the present invention are at least:

[0032] 1) The antifoaming agent composition and preparation method provided by the present invention can be fully dispersed in lubricating oil, so that the lubricating oil has high-efficiency antifoaming performance, high-temperature antifoaming performance and reliable long-term storage stability, thereby solving the problem of difficult foam control of lubricating oil.

[0033] 2) The antifoaming agent composition provided by the present invention does not change its antifoaming agent particles after long-term storage, and its antifoaming performance and high-temperature antifoaming performance are not affected when used in lubricating oil, thereby solving the problem of precipitation and stratification of antifoaming agents during storage, which in turn renders the antifoaming agent ineffective. DETAILED DESCRIPTION

[0034] The following examples are used to illustrate the present invention but are not intended to limit the scope of the present invention.

[0035] Example 1

[0036] This embodiment provides an antifoaming agent composition, including: a dispersing solvent, an antifoaming agent effective ingredient, a dispersing aid and a base oil. The weight ratio of the dispersing solvent, the antifoaming agent effective ingredient, the dispersing aid and the base oil is 1:0.0001:1:1. The dispersing solvent is kerosene, the antifoaming agent effective ingredient is polydimethylsiloxane, and the surface tension is 15Nm / m; the dispersing aid is a thiophosphate amine salt extreme pressure antiwear agent, and the kinematic viscosity at 100°C is 300cSt; the base oil is mineral oil HVI III4.

[0037] This embodiment also provides a method for preparing the antifoaming agent composition, comprising the following steps:

[0038] (1) The antifoaming agent active ingredient is dissolved in a dispersing solvent to obtain a clear and transparent component A.

[0039] (2) After the clear and transparent component A, the dispersing aid and the base oil are mixed according to the proportion, they are ground once for 0.1 hour at 100° C. using a high-speed homogenizer (10000 rpm), and cooled to room temperature to obtain an antifoaming agent composition.

[0040] Example 2

[0041] This embodiment provides an antifoaming agent composition, including: a dispersing solvent, an antifoaming agent effective ingredient, a dispersing aid and a base oil. The weight ratio of the dispersing solvent, the antifoaming agent effective ingredient, the dispersing aid and the base oil is 50:5:90:20. The dispersing solvent is kerosene, the antifoaming agent effective ingredient is a polysiloxane containing a branched carbon fluorostructure, the surface tension is 30Nm / m, and the structure is as follows; the dispersing aid is a thiophosphate amine salt extreme pressure anti-wear agent, and the kinematic viscosity at 100°C is 20cSt; the base oil is a poly-alpha-olefin synthetic base oil PAO4.

[0042] The polysiloxane containing a branched fluorocarbon structure has the structure shown in the following formula:

[0043]

[0044] Where R is C 22 A straight-chain alkane with x=1, y=1, z=10.

[0045] This embodiment also provides a method for preparing the antifoaming agent composition, comprising the following steps:

[0046] (1) The antifoaming agent active ingredient is dissolved in a dispersing solvent to obtain a clear and transparent component A.

[0047] (2) After the clear and transparent component A, the dispersing aid and the base oil are mixed according to the proportion, they are ground six times at 30° C. for 1 hour using a high-speed homogenizer (10,000 rpm), and cooled to room temperature to obtain an antifoaming agent composition.

[0048] Example 3

[0049] This embodiment provides an antifoaming agent composition, including: a dispersing solvent, an antifoaming agent effective ingredient, a dispersing aid, and a base oil. The weight ratio of the dispersing solvent, the antifoaming agent effective ingredient, the dispersing aid, and the base oil is 20:0.0003:2:5. The dispersing solvent is methyl ethyl ketone, the antifoaming agent effective ingredient is a methacrylate-acrylate copolymer, and the surface tension is 25Nm / m; the dispersing aid is a polyisobutylene succinimide dispersant, and the kinematic viscosity at 100°C is 200cSt; the base oil is polyalkylene glycol.

[0050] This embodiment also provides a method for preparing the antifoaming agent composition, comprising the following steps:

[0051] (1) The antifoaming agent active ingredient is dissolved in a dispersing solvent to obtain a clear and transparent component A.

[0052] (2) After the clear and transparent component A, the dispersing aid and the base oil are mixed according to the proportion, they are ground twice at 80° C. for 0.5 hours using a colloid mill and cooled to room temperature to obtain an antifoaming agent composition.

[0053] Example 4

[0054] This embodiment provides an antifoaming agent composition, including: a dispersing solvent, an antifoaming agent effective ingredient, a dispersing aid and a base oil. The weight ratio of the dispersing solvent, the antifoaming agent effective ingredient, the dispersing aid and the base oil is 20:3:70:15. The dispersing solvent is methyl isobutyl ketone, the antifoaming agent effective ingredient is a polysiloxane containing a branched carbon fluorostructure, the surface tension is 20Nm / m, and the structure is as follows; the dispersing aid is a polymethacrylate pour point depressant, and the kinematic viscosity at 100°C is 50cSt; the base oil is a polyol ester synthetic base oil.

[0055] The polysiloxane containing a branched fluorocarbon structure has the structure shown in the following formula:

[0056]

[0057] Wherein, R is a C8 straight chain alkane, x=90, y=30, z=22

[0058] This embodiment also provides a method for preparing the antifoaming agent composition, comprising the following steps:

[0059] (1) The antifoaming agent active ingredient is dissolved in a dispersing solvent to obtain a clear and transparent component A.

[0060] (2) After the clear and transparent component A, the dispersing aid and the base oil are mixed according to the proportion, they are ground twice at 80° C. for 0.5 hours using a colloid mill and cooled to room temperature to obtain an antifoaming agent composition.

[0061] Example 5

[0062] This embodiment provides an antifoaming agent composition, including: a dispersing solvent, an antifoaming agent effective ingredient, a dispersing aid and a base oil. The weight ratio of the dispersing solvent, the antifoaming agent effective ingredient, the dispersing aid and the base oil is 20:0.002:70:9.998. The dispersing solvent is meta-trifluorotoluene, the antifoaming agent effective ingredient is a phenyl hydrogenated silicone oil co-modified by a polyether and a fluorinated ester, the surface tension is 15Nm / m, and the structure is as follows; the dispersing aid is a calcium alkyl salicylate T106 detergent, the kinematic viscosity at 100°C is 150cSt; the base oil is a diester synthetic base oil.

[0063] The polyether and fluorinated ester co-modified phenyl hydrogen silicone oil has the structure shown in the following formula:

[0064]

[0065] Among them, m=1, n=1, p=1.

[0066] This embodiment also provides a method for preparing the antifoaming agent composition, comprising the following steps:

[0067] (1) The antifoaming agent active ingredient is dissolved in a dispersing solvent to obtain a clear and transparent component A.

[0068] (2) After the clear and transparent component A, the dispersing aid and the base oil are mixed according to the proportion, they are ground twice for 0.5 hours using a colloid mill at 70° C. and cooled to room temperature to obtain an antifoaming agent composition.

[0069] Example 6

[0070] This embodiment provides an antifoaming agent composition, including: a dispersing solvent, an antifoaming agent effective ingredient, a dispersing aid and a base oil. The weight ratio of the dispersing solvent, the antifoaming agent effective ingredient, the dispersing aid and the base oil is 1:0.001:50:10. The dispersing solvent is acetone, the antifoaming agent effective ingredient is a phenyl hydrogenated silicone oil co-modified by polyether and fluorinated ester, and the surface tension is 15Nm / m; the dispersing aid is a molybdenum dithiophosphate friction modifier, and the kinematic viscosity at 100°C is 300cSt; the base oil is a vegetable oil.

[0071] The polyether and fluorinated ester co-modified phenyl hydrogen silicone oil has the structure shown in the following formula:

[0072]

[0073] Among them, m=90, n=20, p=20.

[0074] This embodiment also provides a method for preparing the antifoaming agent composition, comprising the following steps:

[0075] (1) The antifoaming agent active ingredient is dissolved in a dispersing solvent to obtain a clear and transparent component A.

[0076] (2) After the clear and transparent component A, the dispersing aid and the base oil are mixed according to the proportion, they are ground once for 0.1 hour at 100° C. using a high-speed homogenizer, and cooled to room temperature to obtain an antifoaming agent composition.

[0077] Comparative Example 1

[0078] This embodiment provides an antifoaming agent composition, including: a dispersing solvent, an antifoaming agent effective ingredient and a base oil. The weight ratio of the dispersing solvent, the antifoaming agent effective ingredient and the base oil is 20:0.002:79.998. The dispersing solvent is meta-trifluorotoluene, the antifoaming agent effective ingredient is a phenyl hydrogenated silicone oil co-modified by a polyether and a fluorinated ester, the surface tension is 15 Nm / m, and the structure is as follows; the base oil is a diester synthetic base oil.

[0079] The polyether and fluorinated ester co-modified silicone oil has the structure shown in the following formula:

[0080]

[0081] Among them, m=1, n=1, p=1.

[0082] This embodiment also provides a method for preparing the antifoaming agent composition, comprising the following steps:

[0083] (1) The antifoaming agent active ingredient is dissolved in a dispersing solvent to obtain a clear and transparent component A.

[0084] (2) After the clear and transparent component A and the base oil are mixed according to the proportion, they are ground twice at 70° C. for 0.5 hours using a colloid mill and cooled to room temperature to obtain an antifoaming agent composition.

[0085] Comparative Example 2

[0086] This embodiment provides an antifoaming agent composition, including: a dispersing solvent, an antifoaming agent effective ingredient, a dispersing aid and a base oil. The weight ratio of the dispersing solvent, the antifoaming agent effective ingredient, the dispersing aid and the base oil is 20:0.002:70:9.998. The dispersing solvent is meta-ditrifluorotoluene, the antifoaming agent effective ingredient is a phenyl hydrogenated silicone oil co-modified by a polyether and a fluorinated ester, the surface tension is 15Nm / m, and the structure is as follows; the dispersing aid is an alkyl calcium salicylate detergent, and the kinematic viscosity at 100°C is 150cSt; the base oil is a diester synthetic base oil.

[0087] The polyether and fluorinated ester co-modified phenyl hydrogen silicone oil has the structure shown in the following formula:

[0088]

[0089] Among them, m=1, n=1, p=1.

[0090] This embodiment also provides a method for preparing the antifoaming agent composition, comprising the following steps:

[0091] Add each component directly into the oil according to the proportion and perform simple mechanical stirring.

[0092] Test Example 1

[0093] This test example is for the antifoaming agent composition of Examples 1 to 6 and Comparative Examples 1 and 2. The antifoaming agent composition is applied to lubricating oil, and the oil is blended by the pulse blending method commonly used for lubricating oil. The foam performance of lubricating oil is evaluated by GB / T 12579 "Evaluation Method for Foam Characteristics of Lubricating Oil", and the high-temperature foam performance of lubricating oil is evaluated by SH / T 0722 "Determination Method for High-Temperature Foam Characteristics of Lubricating Oil"; after the oil is centrifuged at 1280rpm for 3 hours, the foam performance of the upper layer of the oil is evaluated by GB / T 12579 and SH / T 0722, which is used to evaluate the stability of the antifoaming agent in the oil after long-term storage of the oil, and the precipitation of the antifoaming agent is evaluated by observing the bottom of the centrifuge tube, and the silicon content in the oil is determined by GB / T 17476 inductively coupled plasma emission spectrometry.

[0094] Among them, the foam performance evaluation is carried out from four procedures, including 24℃, 93.5℃, post-24℃, and 150℃, among which procedure I (24℃) represents the foam volume on the oil surface at the end of the blowing cycle at 24℃; procedure II (93.5℃) represents the foam volume on the oil surface at the end of the blowing cycle at 93.5℃; procedure III (post-24℃) represents the foam volume on the oil surface at the end of the blowing cycle after the oil treated at 93.5℃ is placed in a 24℃ temperature environment; procedure IV (150℃) represents the foam volume on the oil surface at the end of the blowing cycle at 150℃. The lower the value, the better the foam performance.

[0095] As shown in Table 1. From Examples 1 to 6, different dispersing aids, antifoaming agent active ingredients, dispersing solvents and base oils were selected and processed according to the dispersion process. The antifoaming performance, especially the foaming performance of the oil at 150°C, was excellent, and the oil was centrifuged at high speed, and the Si content in the oil was also well maintained; compared with Comparative Examples 1 and 2, the antifoaming performance of the oil at 150°C in the comparative examples was poor, and precipitation problems caused by the precipitation of the antifoaming agent occurred. It shows that the solution proposed by the present invention has good high-temperature foam control ability and stability, and achieves excellent long-term stability.

[0096] Table 1 Test results of foam performance of oil products in Examples 1 to 6 and Comparative Examples 1 and 2

[0097]

[0098] Although the present invention has been described in detail above by means of general description, specific implementation methods and tests, it is obvious to those skilled in the art that some modifications or improvements may be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. An antifoaming agent composition comprising: The weight ratio of the dispersion solvent, the antifoaming agent active ingredient, the dispersion aid and the base oil is 1-50:0.0001-5:1-90:1-20.

2. The antifoaming agent composition according to claim 1, characterized in that The weight ratio of the dispersing solvent, the antifoaming agent effective component, the dispersing aid and the base oil is 1-50: 0.0003-3: 2-70: 5-15.

3. The antifoaming agent composition according to claim 2, characterized in that The anti-foaming agent active ingredient is selected from one or more of methacrylate-acrylate copolymer, polyethylene glycol ether-fatty alcohol-polytetramethylene glycol ether copolymer, polydimethylsiloxane, polyether and fluorinated ester co-modified phenyl hydrogen silicone oil, and polysiloxane containing branched fluorocarbon structure; and / or, The dispersing solvent is selected from one or more of acetone, kerosene, methyl-ethyl ketone, methyl isobutyl ketone, m-ditrifluorotoluene, toluene, and cyclohexanone; and / or, The dispersing aid is selected from one or more of a friction modifier, an extreme pressure antiwear agent, a pour point depressant, a viscosity index improver, a dispersant, and a detergent; and / or, The base oil is selected from one or more of mineral oil, vegetable oil, poly-α-olefin synthetic base oil, polyol ester synthetic base oil, polyalkylene glycol, and diester synthetic base oil.

4. The antifoaming agent active ingredient according to claim 3, characterized in that The polysiloxane containing a branched carbon fluorine structure has a structure shown in the following formula (I): In formula (I), R is C1 to C 22 A divalent straight-chain alkane group, x=1-90, y=1-30, z=10-22; And / or, the polyether and fluorinated ester co-modified silicone oil has a structure shown in the following formula (II): In formula (II), m=1-90, n=1-20, and p=1-20.

5. The antifoaming agent composition according to any one of claims 1 to 4, characterized in that The surface tension of the effective ingredient of the antifoaming agent is 15 to 30 Nm / m, preferably 20 to 25 Nm / m.

6. The antifoaming agent composition according to any one of claims 1 to 4, characterized in that The kinematic viscosity of the dispersing agent at 100° C. is 20 to 300 cSt, preferably 50 to 200 cSt.

7. The method for preparing the antifoaming agent composition according to any one of claims 1 to 6, characterized in that: The steps include: (1) dissolving the antifoaming agent active ingredient in the dispersing solvent to obtain a clear and transparent component A; (2) The clear and transparent component A, the dispersing aid and the base oil are mixed according to a proportion, ground and cooled to room temperature to obtain an antifoaming agent composition.

8. The method for preparing the antifoaming agent composition according to claim 7, characterized in that: In step (2), the grinding is performed at 30 to 100° C. for 0.1 to 1 hour / time; And / or, in step (2), the grinding is performed 1 to 6 times; And / or, in step (2), the mixing is carried out in a stirred tank, a colloid mill, a high-speed homogenizer or a combination of the two.

9. Use of the antifoaming agent composition according to any one of claims 1 to 6 or the antifoaming agent composition prepared by the preparation method of the antifoaming agent composition according to claim 7 or 8 in the field of lubricating oil.

10. The use of the antifoaming agent composition according to claim 9, characterized in that: Application of the antifoaming agent composition in ultra-low viscosity lubricating oil for electric vehicles.

Citation Information

Patent Citations

  • Method for improving stability of mineral oil defoaming agent

    CN101445760A

  • High-efficiency antifoaming agent

    CN102949867A

  • Lubricating oil composite type antifoaming agent and application thereof

    CN104232246A

  • Anti-foaming agent composition and application thereof

    CN105385484A

  • Method for synthesizing fluorine silicon antifoaming agent for engine oil

    CN105542170A